Method for smelting and desulfurizing titanium-reinforced automobile structural steel
By combining converter, LF refining and RH vacuum refining processes during steel smelting, and using CaO-CaF2-based desulfurization agent to perform desulfurization treatment in RH vacuum refining, the problem of difficult to reduce sulfur content in steel is solved, and the yield rate is improved. Reduced waste.
Patent Information
- Application Number
- CN202411041304.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art is difficult to effectively reduce the sulfur content in the steel during steel smelting, especially in the converter process, which leads to sulfur recovery due to the high sulfur load in the furnace, resulting in the finished material becoming a waste product or being degraded.
Using processes including converter steelmaking, LF refining and RH vacuum refining, the temperature and airflow conditions of the steel liquid are controlled to ensure that the sulfur content is lower than that of the RH vacuum refining process. 0.006%, and deoxygenation and desulfurization operations were carried out in the LF refining process.
It effectively reduces the sulfur content in the steel, reduces the downgrade of finished materials caused by sulfur edges, and improves the yield rate.
Smart Images

Figure BDA0004972455080000031 
Figure BDA0004972455080000041 
Figure BDA0004972455080000042
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steel smelting, and in particular relates to a method for smelting and desulfurizing titanium-reinforced automobile structural steel. Background Art
[0002] Sulfur exists in steel mainly in the form of non-metallic inclusions (such as Mns, FeS, etc.). It has a strong segregation effect, which can cause hot brittleness of steel and reduce the mechanical properties of steel, especially the fatigue limit, plasticity and wear resistance of steel. The low melting point caused by sulfide makes steel easy to produce hot cracks during welding, which significantly reduces weldability.
[0003] With the progress of society, modern industry has higher and higher requirements on the performance of steel. In order to meet this requirement, the research on clean steel technology has become an increasingly important research topic in the field of steel metallurgy technology.
[0004] Hot metal desulfurization is an economical and effective desulfurization method, which has been widely used in industrial production. As we all know, the desulfurization capacity of the converter is quite limited. Especially when the original sulfur content of the hot metal is very low, due to the high sulfur content of the lime, scrap steel and other furnace materials entering the furnace, the converter process often resulfurizes, causing the sulfur edge to make the finished product scrap or downgraded. Generally speaking, it is difficult to stably produce steel with a sulfur content of less than 80ppm by hot metal pretreatment alone. Therefore, it is imperative to desulfurize the hot metal outside the converter after the converter is tapped. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for smelting and desulfurizing titanium-reinforced automobile structural steel.
[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is:
[0007] A method for smelting and desulfurizing titanium-reinforced automobile structural steel, comprising converter steelmaking, LF refining, RH vacuum refining, and continuous casting steps;
[0008] In the RH vacuum refining process, the inner wall temperature of the vacuum tank before continuous vacuum refining treatment is greater than 1400°C. After the molten steel circulates in the vacuum tank, 30-100 kg of Taiwan aluminum is added, and the RH circulating argon flow rate is adjusted to 90-120 Nm 3 / h, after the molten steel circulates for 2 minutes, 300-500 kg / furnace of CaO-CaF2 desulfurizer is added, and the molten steel circulates for 3-6 minutes for desulfurization.
[0009] Furthermore, in the converter steelmaking process, the converter final temperature is 1640-1690°C, and the continuous pulling temperature is 1620-1670°C; the element weight content in the converter final molten steel is optimally controlled to be C: 0.03-0.04%, P≤0.012%, and S≤0.015%.
[0010] Furthermore, in the converter steelmaking process, the oxygen lance position during the smelting process is controlled at 1.4-1.7m, the oxygen pressure is 0.7-0.9Mpa, and the oxygen flow rate is 32000-38000Nm 3 / h, the oxygen flow rate of the top gun oxygen supply within 2 to 3 minutes is 26000Nm 3 / h, oxygen supply time is 13 to 16 minutes.
[0011] Furthermore, in the LF refining process, the LF enters the station for refining treatment, the argon flow rate is set to ≤1500NL / min, the feeding time is controlled at 2-3min, the total amount of small-grain lime added before the first heating is ≤800kg, and after the first heating is completed, the argon flow rate is adjusted to 800-1500NL / min for deoxidation and desulfurization operations.
[0012] Furthermore, in the LF refining process, FeO+MnO in the white slag is ≤1.0%, and the slag thickness is 2-4 mm.
[0013] Furthermore, in the RH vacuum refining process, after desulfurization is completed, the alloy composition is adjusted once to compensate for the process target, C: 0.05-0.08%, Si: 0.10-0.20%, Mn: 1.75-1.90%, P≤0.015%, S≤0.006%, Nb: 0.055-0.070%, Ti: 0.090-0.110%, Mo: 0.10-0.20%, Als: 0.020-0.050%, [N]≤35ppm.
[0014] Furthermore, in the RH vacuum refining process, the vacuum degree is maintained at ≤100Pa for 18-22min of cyclic degassing, the pure degassing time is ≥8min, the calcium iron wire feeding is 100-300m, the RH first furnace tapping temperature is 1590-1600°C, and the continuous drawing temperature is 1565-1575°C.
[0015] Furthermore, the main chemical components and mass percentages of the molten steel obtained by the method are: C: 0.05-0.08%, Si: 0.10-0.20%, Mn: 1.75-1.90%, P≤0.015%, S≤0.006%, Nb: 0.055-0.070%, Ti: 0.090-0.110%, Mo: 0.10-0.20%, Als: 0.020-0.050%, [N]≤35ppm, and the remainder is Fe and unavoidable impurities.
[0016] The beneficial effect produced by adopting the above technical scheme is that after the acid-soluble aluminum content in the molten steel is controlled to reach the middle and upper limit content required by the process in the RH vacuum furnace, a quantitative CaO-CaF2 series desulfurizer is added to effectively reduce the content, thereby solving the problem that when the original sulfur content of the molten iron is very low, the sulfur back occurs in the converter and LF furnace smelting process due to the high sulfur content of the furnace charge entering the furnace, thereby reducing the occurrence of finished products becoming waste or being downgraded due to sulfur edges, and ensuring the yield rate. DETAILED DESCRIPTION
[0017] The present invention is further described in detail below in conjunction with specific implementation modes.
[0018] Example 1-8: A method for smelting and desulfurizing titanium-reinforced automotive structural steel, wherein the composition content of the structural steel is (wt): C: 0.05-0.08%, Si: 0.10-0.20%, Mn: 1.75-1.90%, P≤0.015%, S≤0.006%, Nb: 0.055-0.070%, Ti: 0.09-0.110, Mo: 0.10-0.20%, Als: 0.020-0.050%, [N]≤35ppm, and the rest is Fe and unavoidable impurities. The method includes converter steelmaking, LF refining, RH vacuum refining, and continuous casting processes, and the steps of each process are as follows:
[0019] (1) Converter steelmaking process
[0020] The nominal capacity of the converter used is 150 tons. 2-3 tons of magnetic separation slag surface under the furnace are quantitatively proportioned to improve the activity of lime. The initial slag formation time can be advanced by 1-2 minutes, and the process slag drying phenomenon can be improved. A diversified slag making process is adopted to increase the self-produced slag surface and slag making materials with components such as MnO, Al2O3 and SiO2. The MgO and MnO in the slag are used to expand the liquid phase and promote the melting of lime. The slag retention operation is adopted. After steel is tapped, a part of the slag is left or the remaining slag is left in the furnace after N2 splashing slag. After adding 1-2 tons of lime and MgO materials, the high-temperature, oxidizing slag of the previous furnace is used to promote the rapid melting of lime during the smelting of the next furnace. In the early stage of blowing, the slag retention operation is used to increase the MgO ratio, and the MgO content is basically saturated, which can not only accelerate the rapid formation of the initial slag, but also slow down the erosion of the initial slag on the furnace lining, and also promote the early formation of the initial slag of steelmaking. The slag making process of adding lime in batches to reduce the alkalinity can effectively control the f-CaO content of the final slag of high-alkalinity steel slag.
[0021] The final temperature of the converter is 1640-1690℃, the continuous pulling temperature is 1620-1670℃, the oxygen lance position during the smelting process is controlled at 1.4-1.7m, the oxygen pressure is 0.7-0.9Mpa, and the oxygen flow rate is 32000-38000Nm 3 / h, the oxygen flow rate of the top gun oxygen supply within 2 to 3 minutes is 26000Nm 3 / h. According to the flame state and the sound in the furnace, the slagging situation and blowing state are determined, and the gun position and cold material addition are adjusted in time to stably control the oxygen supply time to 13-16min. When the oxygen supply reaches 85%, the auxiliary gun TSC is started to measure the temperature, sample and test the element composition content in the molten steel, and adjust the end point operation in time according to the measurement results. After the blowing is completed, TSO is used to measure the molten pool temperature and carbon content, and the steel is tapped after meeting the steel grade requirements. The optimal element weight content in the converter end point molten steel is controlled to be C: 0.03-0.04%, P≤0.012%, S≤0.015%.
[0022] The control parameters of the converter steelmaking process in each embodiment are shown in Table 1.
[0023] Table 1 Control parameters of converter steelmaking process in various embodiments
[0024]
[0025] (2) LF refining process
[0026] LF enters the station for refining treatment, the argon flow rate is set to ≤1500NL / min, and the feeding time is controlled at 2-3min. According to the sulfur content in the chemical sample steel of the previous process (argon station), deoxidizer and slag material are added, and then lime is added. The total amount of small-grain lime added before the first heating is ≤800kg, which can be added in batches. After the feeding is completed, it is fully stirred and melted, and then heated. In the early stage of electrode heating, long arc heating is used for 2-3min to melt the slag, and short arc + foam slag operation is used for rapid heating in the later stage. After the first heating is completed, the argon flow rate is adjusted to 800-1500NL / min for deoxidation and desulfurization operations. Observe the color and state of the sticky slag and add deoxidizer and slag agent in time. During the strong stirring process of argon, deep deoxidation forms white slag, and FeO+MnO in the white slag is ≤1.0%, and the slag thickness is 2-4mm. Adjust the argon flow rate to 200-300NL / min to stir the steel liquid with uniform temperature and uniform composition. Temperature measurement and sampling, the chemical composition of the samples all met the quality requirements, C: 0.05 ~ 0.08%, Si: 0.10 ~ 0.20%, Mn: 1.75 ~ 1.90%, P ≤ 0.015%, S ≤ 0.006%, Nb: 0.055 ~ 0.070%, Mo: 0.10 ~ 0.20%, Als: 0.020 ~ 0.035%.
[0027] The control parameters of the LF refining process in each embodiment are shown in Table 2, and the composition of the molten steel at the end of the LF refining process is shown in Table 3.
[0028] Table 2 LF refining process control parameters of each embodiment
[0029]
[0030] In Table 2, the argon gas flow rate corresponds to the argon gas flow rate control in the above-mentioned LF refining process in chronological order.
[0031] Table 3 Molten steel composition (wt%) at the end of LF refining process in each embodiment
[0032]
[0033]
[0034] (3) RH vacuum refining process
[0035] The top gun baking operation is carried out before the continuous vacuum refining treatment, and the coal-oxygen ratio is 1:1. The gun position is 4.5-5.5m, and the oxygen flow rate is 180-220Nm 3 / h, make the tank temperature (tank wall temperature)>1400℃, eliminate the cold steel nodules in the vacuum tank, after the molten steel circulates in the vacuum tank, add 30-100kg of Taiwan aluminum according to the acid-soluble aluminum content in the molten steel in the previous process (LF refining process) and the cold steel nodules in the vacuum tank, so that the acid-soluble aluminum content in the steel reaches the upper limit of the process requirements, avoid RH station molten steel circulation cold steel oxidation alloy burning and add CaO-CaF2 series desulfurization agent overflow. Adjust the RH circulation argon flow rate to 90-120Nm 3 / h, after the molten steel circulates for 2 minutes, 300-500 kg / furnace of CaO-CaF2 desulfurizer is added according to the sulfur content in the chemical sample, and the molten steel circulates for 3-6 minutes for desulfurization. In terms of weight percentage, the composition of the desulfurizer is Cao: 60-70%, CaF2: 15-22%, Al2O3: 10-15%, SiO2 <2.0%, and Mgo <1.0%.
[0036] After desulfurization, temperature measurement, sampling, aluminum determination, and alloying of molten steel components are carried out according to the alloy content of RH chemical samples. The alloy composition compensation is adjusted once to achieve the process target, C: 0.05-0.08%, Si: 0.10-0.20%, Mn: 1.75-1.90%, P≤0.015%, S≤0.006%, Nb: 0.055-0.070%, Ti: 0.09-0.110%, Mo: 0.10-0.20%, Als: 0.020-0.050%, [N]≤35ppm. Maintain vacuum degree ≤100Pa, cyclic degassing for 18-22min, pure degassing time ≥8min, calcium iron wire feeding wire 100-300m, RH first furnace tapping temperature 1590-1600℃, continuous drawing temperature 1565-1575℃.
[0037] The control parameters of the RH vacuum refining process of each embodiment are shown in Tables 4 and 5; the composition of the desulfurizing agent is shown in Table 6.
[0038] Table 4 RH vacuum refining process control parameters of each embodiment -1
[0039]
[0040]
[0041] Table 5 RH vacuum refining process control parameters of each embodiment-2
[0042]
[0043] In Table 5, the balance of the chemical composition of molten steel is Fe and unavoidable impurities.
[0044] Table 6 Composition and content of desulfurizer in RH vacuum refining process of each embodiment (wt%)
[0045] Example Cao <![CDATA[CaF2]]> <![CDATA[Al2O3]]> <![CDATA[SiO2]]> Mgo 1 70 15 10 1.8 0.9 2 68 18 12 1.2 0.8 3 65 20 13 1.5 0.5 4 63 21 13 1.9 0.9 5 69 18 11 1.3 0.7 6 66 20 12 1.0 0.8 7 62 21 14 1.6 0.6 8 60 22 15 1.8 0.9
[0046] From the comparison between Table 3 and Table 5, it can be seen that the present invention can effectively reduce the sulfur content by adding a CaO-CaF2 series desulfurizing agent in the RH vacuum refining process.
[0047] The above embodiments are only used to illustrate rather than limit the technical solutions of the present invention. Although the present invention is described in detail with reference to the above embodiments, those skilled in the art should understand that the present invention can still be modified or replaced by equivalents. Any modification or partial replacement that does not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.
Claims
1. A method for smelting and desulfurizing titanium-reinforced automotive structural steel, characterized in that: It includes converter steelmaking, LF refining, RH vacuum refining, and continuous casting processes; In the RH vacuum refining process, the inner wall temperature of the vacuum tank before continuous vacuum refining treatment is greater than 1400°C. After the molten steel circulates in the vacuum tank, 30-100 kg of Taiwan aluminum is added, and the RH circulating argon flow rate is adjusted to 90-120 Nm 3 / h, after the molten steel circulates for 2 minutes, 300-500 kg / furnace of CaO-CaF2 desulfurizer is added, and the molten steel circulates for 3-6 minutes for desulfurization.
2. The method for smelting and desulfurizing titanium-reinforced automobile structural steel according to claim 1, characterized in that: In the converter steelmaking process, the converter terminal temperature is 1640-1690° C. and the continuous pulling temperature is 1620-1670° C.; the element weight content in the converter terminal molten steel is optimally controlled to be C: 0.03-0.04%, P≤0.012%, and S≤0.015%.
3. The method for smelting and desulfurizing titanium-reinforced automobile structural steel according to claim 2, characterized in that: In the converter steelmaking process, the oxygen lance position is controlled at 1.4-1.7m, the oxygen pressure is 0.7-0.9Mpa, and the oxygen flow rate is 32000-38000Nm 3 / h, the oxygen flow rate of the top gun oxygen supply within 2 to 3 minutes is 26000Nm 3 / h, oxygen supply time is 13 to 16 minutes.
4. The method for smelting and desulfurizing titanium-reinforced automobile structural steel according to claim 3, characterized in that: In the LF refining process, LF enters the station for refining treatment, the argon flow rate is set to ≤1500NL / min, the feeding time is controlled at 2-3min, the total amount of small-grain lime added before the first heating is ≤800kg, and after the first heating is completed, the argon flow rate is adjusted to 800-1500NL / min for deoxidation and desulfurization operations.
5. The method for smelting and desulfurizing titanium-reinforced automobile structural steel according to claim 4, characterized in that: In the LF refining process, FeO+MnO in the white slag is ≤1.0%, and the slag thickness is 2-4 mm.
6. The method for smelting and desulfurizing titanium-reinforced automobile structural steel according to claim 5, characterized in that: In the RH vacuum refining process, after desulfurization is completed, the alloy composition is adjusted once to compensate for the process target, C: 0.05-0.08%, Si: 0.10-0.20%, Mn: 1.75-1.90%, P≤0.015%, S≤0.006%, Nb: 0.055-0.070%, Ti: 0.090-0.110%, Mo: 0.10-0.20%, Als: 0.020-0.050%, [N] ≤35ppm.
7. The method for smelting and desulfurizing titanium-reinforced automobile structural steel according to claim 6, characterized in that: In the RH vacuum refining process, the vacuum degree is maintained at ≤100Pa, the cyclic degassing is performed for 18 to 22 minutes, the pure degassing time is ≥8 minutes, the calcium iron wire feeding is 100 to 300 meters, the RH first furnace tapping temperature is 1590 to 1600°C, and the continuous drawing temperature is 1565 to 1575°C.
8. The method for smelting and desulfurizing titanium-reinforced automobile structural steel according to any one of claims 1 to 7, characterized in that: The main chemical components and mass percentages of the molten steel obtained by the method are: C: 0.05-0.08%, Si: 0.10-0.20%, Mn: 1.75-1.90%, P≤0.015%, S≤0.006%, Nb: 0.055-0.070%, Ti: 0.090-0.110%, Mo: 0.10-0.20%, Als: 0.020-0.050%, [N] ≤35ppm, and the remainder is Fe and unavoidable impurities.