Method for recovering gold and copper from waste printed circuit board step by step

Through the step-by-step method of synchronous electrodistribution of copper and gold recovery through flotation and electrooxidation leaching, the problem of low metal extraction rate in traditional electrolysis methods is solved, efficient and green gold and copper recovery is achieved, and resource utilization efficiency is improved.

CN118957268AActive Publication Date: 2024-11-15CENT SOUTH UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411032721.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The traditional electrolysis method has a low extraction rate for recovering metal from used printed circuit boards, and there are problems of high energy consumption and insufficient environmental friendliness.

Method used

The step-by-step method of synchronous electrocalization recovery of copper and gold is adopted for flotation and electrooxidation leaching. By adjusting the timing and conditions of synchronous electrocalization recovery of gold by electrooxidation leaching, two process flows are formed: flotation-electrooxidation leaching synchronous electrocalization recovery Copper-electrooxidation leaching synchronous electrodistribution recovery gold and electrooxidation leaching synchronous electrodistribution recovery gold-flotation-electrooxidation leaching synchronous electrodistribution recovery copper, using copper-amino alkaline electrolyte and potassium iodide electrolyte for electrolysis to accurately control electrolytic parameters To improve recycling efficiency.

Benefits of technology

It realizes efficient recycling of gold and copper from waste printed circuit boards in step by step, improves metal extraction rate, reduces the amount of materials and energy consumption of subsequent processing, obtains cathode products with high purity, and recycles metals in a green and efficient manner.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957268A_ABST
    Figure CN118957268A_ABST
Patent Text Reader

Abstract

The invention provides a method for recycling gold and copper from a waste printed circuit board step by step. The method comprises the steps of flotation, copper recycling through electrooxidation leaching and synchronous electrodeposition and gold recycling through electrooxidation leaching and synchronous electrodeposition. According to the method, plastic and metal are separated through the flotation technology, copper and gold are leached and electrodeposited through the electrooxidation leaching and synchronous electrodeposition technology, metal copper and metal gold are obtained through step-by-step extraction, efficient separation and recovery of the gold and the copper can be achieved, the follow-up separation procedures and cost are reduced, recycling of the waste printed circuit board is achieved, and the method is suitable for industrial production. Wide industrial application prospects are realized. The technology of electrooxidation leaching and electrodeposition copper recovery is adopted, the electrolyte contains CuSO4, NH3.H2O, (NH4) 2SO4 and ethidene diamine, the ethidene diamine is added into the electrolyte, the usage amount of ammonia water can be reduced, the copper recovery rate can be increased, the cathode copper-clad plate with the smooth and compact surface can be obtained under the low current density, the copper recovery rate reaches 90% or above, and the copper purity reaches 90% or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal recovery, in particular to a method for recovering gold and copper from waste printed circuit boards in steps. Background Art

[0002] In the past 20 years, electronic products such as computers, mobile phones, household appliances, and instruments have developed rapidly. While facilitating people's production and life, they have also brought a large amount of electronic waste. Printed circuit boards (PCBs) are composed of substrates made of resin and glass fiber materials, copper rivets and metal foil on the substrate, and electronic components. Waste printed circuit boards mainly contain precious metals such as gold, silver, and palladium, and heavy and light metals such as copper, aluminum, zinc, iron, and nickel. The copper content is as high as more than 13%, and the gold content is more than 40g / t, which is much higher than the grade of ore.

[0003] The technologies for recovering metals, especially copper and gold, from waste printed circuit boards can be divided into mechanical and physical methods, pyrometallurgy, biotechnology, hydrometallurgy and electrolysis. However, the products recovered from waste printed circuit boards by mechanical methods are mostly mixtures of metals and non-metals; the energy consumption of pyrometallurgical processes is generally high; the treatment cycle of biometallurgy is long; and the hydrometallurgical process is accompanied by a large amount of leaching agents. In contrast, electrolysis technology is considered to be an economical and effective method for recovering metals from waste printed circuit boards.

[0004] However, the metal extraction rate of the traditional electrolytic method is still relatively low. Therefore, it is of great significance to develop an environmentally friendly and efficient step-by-step method for recovering gold and copper, improve the metal extraction rate in waste printed circuit boards, and maximize the available components. Summary of the invention

[0005] Based on this, the present invention provides a method for recovering gold and copper from waste printed circuit boards in steps with a high metal extraction rate.

[0006] A method for recovering gold and copper from waste printed circuit boards in steps, comprising flotation, electro-oxidation leaching and simultaneous electro-winning to recover copper, and electro-oxidation leaching and simultaneous electro-winning to recover gold;

[0007] The flotation step specifically comprises: crushing the waste printed circuit boards to a particle size of less than 0.425 mm, and then mixing with water and a wetting agent for flotation to obtain a foam product and a tank product; the foam product is a product enriched in plastic, and the tank product is a product enriched in gold and copper;

[0008] The electro-oxidation leaching and simultaneous electro-winning copper recovery step specifically comprises: placing the product in the cell into an electrolytic cell, performing electro-oxidation leaching with a copper-ammonia alkaline electrolyte, and simultaneously electro-winning copper recovery to obtain leaching slag and electro-winning copper; the copper-ammonia alkaline electrolyte comprises CuSO4, (NH4)2SO4, NH3·H2O and ethylenediamine;

[0009] When the electro-oxidation leaching and simultaneous electro-winning gold recovery step is after the electro-oxidation leaching and simultaneous electro-winning copper recovery step, the process specifically comprises: placing the leached residue obtained from the electro-oxidation leaching and simultaneous electro-winning copper recovery step into an electrolytic cell, performing electro-oxidation leaching with potassium iodide electrolyte, and simultaneously electro-winning gold recovery;

[0010] When the electro-oxidation leaching and simultaneous electro-winning gold recovery step is before the flotation step, it specifically includes: using the waste printed circuit board as the anode, electro-oxidation leaching gold in a thiourea-sodium chloride-chloroaurate electrolyte, and simultaneously electro-winning gold recovery, and in the same electro-winning cycle, replacing the waste printed circuit board of the anode at least 10 times to enrich the gold at the cathode.

[0011] In other words, two process flows can be formed by adjusting the timing and conditions of the electro-oxidation leaching and simultaneous electro-winning gold recovery steps. Scheme 1 is flotation - electro-oxidation leaching and simultaneous electro-winning copper recovery - electro-oxidation leaching and simultaneous electro-winning gold recovery:

[0012] SA1 flotation: The waste printed circuit boards are crushed to a particle size of less than 0.425 mm, and then mixed with water and a wetting agent for flotation to obtain a foam product and an in-tank product;

[0013] SA2 electro-oxidation leaching and simultaneous electro-winning of copper recovery: the product in the tank obtained in step SA1 is placed in an electrolytic tank, electro-oxidation leaching is performed with a copper-ammonia alkaline electrolyte, and copper is recovered by electro-winning at the same time to obtain leaching slag and electro-winning copper;

[0014] SA3 electro-oxidation leaching and simultaneous electrolytic recovery of gold: The leaching residue obtained in step SA2 is placed in an electrolytic cell, electro-oxidation leaching is performed with potassium iodide electrolyte, and gold is recovered simultaneously by electro-oxidation.

[0015] Scheme 2 is electro-oxidation leaching and simultaneous electro-winning to recover gold - flotation - electro-oxidation leaching and simultaneous electro-winning to recover copper:

[0016] SB1 electro-oxidation leaching and simultaneous electro-winning gold recovery: Using waste printed circuit boards as anodes, electro-oxidation leaching of gold is carried out in thiourea-sodium chloride-chloroaurate electrolyte, and gold is recovered by electro-winning at the same time. In the same electro-winning cycle, the waste printed circuit boards with anodes are replaced at least 10 times to enrich gold at the cathode;

[0017] SB2 flotation: the waste printed circuit boards treated in step SB1 are crushed to a particle size of less than 0.425 mm, and then mixed with water and a wetting agent for flotation to obtain a foam product and an in-tank product;

[0018] SB3 electro-oxidation leaching and simultaneous electrolytic recovery of copper: the product in the tank obtained in step SB2 is placed in an electrolytic tank, electro-oxidation leaching is performed with a copper-ammonia alkaline electrolyte, and copper is recovered by electrolytic deposition at the same time.

[0019] In one embodiment, in the copper ammonia alkaline electrolyte, the concentration of CuSO4 is 0.05-0.3 mol / L; preferably, the concentration of (NH4)2SO4 is 0.1-0.3 mol / L; preferably, the concentration of NH3·H2O is 0.1-0.3 mol / L; preferably, the concentration of ethylenediamine is 0.1-0.6 mol / L.

[0020] In one embodiment, in the electro-oxidation leaching and simultaneous electrowinning copper recovery step, the current density is 10-30 mA / cm 2 Preferably, the electrolysis time is 3 to 7 hours, and preferably, the solid-liquid ratio, i.e., the mass volume ratio of the product in the tank (calculated on a dry basis) to the electrolyte is 10 to 40 g / L.

[0021] In one embodiment, in the electro-oxidation leaching and simultaneous electrowinning copper recovery step, the anode is selected from any one of DSA, graphite and titanium mesh, and the cathode is a titanium plate.

[0022] In one embodiment, when the electro-oxidation leaching and simultaneous electrowinning step of recovering gold is after the electro-oxidation leaching and simultaneous electrowinning step of recovering copper, the concentration of potassium iodide in the potassium iodide electrolyte is 5 to 30 g / L; preferably, the electrolysis voltage is 2 to 6 V; preferably, the electrolysis time is 0.5 to 3 h; preferably, the solid-liquid ratio, i.e., the mass volume ratio of the leached residue (calculated on a dry basis) to the electrolyte is 100 to 200 g / L.

[0023] In one embodiment, when the electro-oxidation leaching and simultaneous electrowinning gold recovery step is after the electro-oxidation leaching and simultaneous electrowinning copper recovery step, the anode is selected from any one of DSA, graphite and titanium mesh, and the cathode is selected from any one of graphite, titanium mesh and carbon fiber.

[0024] In one embodiment, when the electro-oxidation leaching and simultaneous electrowinning gold recovery step is before the flotation step, the thiourea content in the thiourea-sodium chloride-chloroaurate electrolyte is 0.5wt% to 4wt%; preferably, the sodium chloride content is 0.5wt% to 4wt%; preferably, the chloroaurate concentration is 30 to 40mg / L; preferably, the cathode is selected from any one of graphite, titanium mesh and carbon fiber, and the distance between the anode and the cathode is 3 to 10cm; preferably, the electrolysis voltage is 1.5 to 4V; preferably, the electrolysis time for each waste printed circuit board is 5s to 18min.

[0025] In one embodiment, the chloroaurate ion comes from any one or more of tetrachloroauric acid, sodium chloroaurate or potassium chloroaurate.

[0026] In one embodiment, the wetting agent is one or more of ethanol, ethylene glycol and glycerol.

[0027] In one of the embodiments, in the flotation step, the volume mass ratio of the wetting agent to the waste printed circuit board is 0.5-2 ml / g, and the solid-liquid ratio, i.e., the mass volume ratio of the waste printed circuit board to ethanol and water is 50-150 g / L.

[0028] The basic principles of the present invention are as follows:

[0029] In the electro-oxidation leaching and simultaneous electrowinning copper recovery step, CuSO4 in the electrolyte can react with NH3·H2O, (NH4)2SO4, and ethylenediamine (en) to generate Cu(NH3)4 2+ 、Cu(en)2 2+ etc., Cu(en)2 2+ The stability constant (1×10 20 ) is much larger than Cu(NH3)4 2+ The stability constant (4.8×10 12 ), and the oxidation potential is higher than the latter, which improves the oxidation ability and stability of the electrolyte, Cu(en)2 2+ and Cu(NH3)4 2+ Reacts with copper in the circuit board to form Cu(en) + 、Cu(NH3)2 + The main reactions in the electrolytic cell are as follows:

[0030] Anode reaction:

[0031] Cu(en)2 2+ +Cu→2Cu(en) +

[0032] Cu(NH3)4 2+ +Cu→2Cu(NH3)2 +

[0033] 2NH4 + →N2+8H + +6e -

[0034] 4OH - →2H2O+O2+4e -

[0035] Cathode zone reaction:

[0036] Cu(NH3)4 2+ +e- →Cu(NH3)2 + +2NH3

[0037] Cu(NH3)2 + +e - →Cu+2NH3

[0038] Cu(en)2 2+ +e - →Cu(en) + +en

[0039] Cu(en) + +e - →Cu+en

[0040] 2H2O+2e - →H2+OH -

[0041] When the electro-oxidation leaching and simultaneous electrowinning step of recovering gold is performed after the electro-oxidation leaching and simultaneous electrowinning step of recovering copper, the electrolyte I - Electro-oxidation in the anode area generates I2, which reacts with potassium iodide in the electrolyte to generate I3 - , I3 - Can react with gold in circuit boards to generate AuI2 - 、AuI4 - , while in the cathode area, elemental gold is recovered by electrolysis. The main reactions in the electrolytic cell are as follows:

[0042] Anode reaction:

[0043] 2I - →I2+2e -

[0044] I2+I - →I3 -

[0045] 2H2O→O2+4H + +4e -

[0046] 2Au+I - +I3 - →2AuI2 -

[0047] 2Au+3I3 - →2AuI4 - +I -

[0048] Cathode zone reaction:

[0049] AuI2 - +e -→Au+2I -

[0050] AuI4 - +3e - →Au+4I -

[0051] 2H2O+2e - →H2+OH -

[0052] I3 - +2e - →3I -

[0053] When the electro-oxidation leaching and simultaneous electro-winning gold recovery step is carried out before the flotation step, the waste printed circuit board is used as the anode, and thiourea and sodium chloride are added to the electrolyte to achieve electro-oxidation leaching of gold. + The stability constant of the complex (9.1×10 21 ) is greater than AuCl2 - The stability constant of the complex (1.0×10 9 ), the electrolytic process gold is Au[CS(NH2)2]2 + In the form of leaching, sodium chloride acts as a conductive medium to accelerate the electromigration rate of ions in the solution and reduce resistance, thereby accelerating the leaching of anode gold and cathode electrodeposition. The main reactions in the electrolytic cell are as follows:

[0054] Anode reaction:

[0055] Au+2CS(NH2)2→Au[CS(NH2)2]2 + +e -

[0056] Cathode zone reaction:

[0057] Au[CS(NH2)2]2 + +e - →Au+2CS(NH2)2

[0058] 2H2O+2e - →H2+OH -

[0059] The above solution of the present invention has the following beneficial effects:

[0060] The present invention provides a technical solution for recovering gold and copper from waste printed circuit boards in steps, and two process flows can be formed by adjusting the timing and conditions of the electro-oxidation leaching and simultaneous electro-deposition recovery of gold steps, namely, flotation-electro-oxidation leaching and simultaneous electro-deposition recovery of copper-electro-oxidation leaching and simultaneous electro-deposition recovery of gold and electro-oxidation leaching and simultaneous electro-deposition recovery of gold-flotation-electro-oxidation leaching and simultaneous electro-deposition recovery of copper, thereby realizing the resource recovery of gold and copper from waste printed circuit boards and facilitating the improvement of resource utilization efficiency. In the recovery method of the present invention, by using flotation, electro-oxidation leaching and simultaneous electro-deposition recovery of copper, electro-oxidation leaching and simultaneous electro-deposition recovery of gold processes, and accurately controlling electrolysis parameters, a cathode product with high purity can be obtained on the cathode, thereby realizing the recovery of gold and copper in a green and efficient manner.

[0061] The present invention uses electrolytic kinetics research in the electro-oxidation leaching and simultaneous electrowinning gold recovery-flotation-electro-oxidation leaching and simultaneous electrowinning copper recovery process to find that in a thiourea-sodium chloride-chloroaurate electrolyte, by precisely controlling the electrolysis time of each waste printed circuit board, gold on the surface layer of the waste printed circuit boards can be preferentially recovered, and the loss of gold in the pretreatment process can be reduced. At this time, the leaching rates of copper and nickel are low, thereby achieving separation of gold from copper and nickel, and reducing the difficulty of separation in subsequent processes.

[0062] The present invention adopts flotation technology to separate plastics and enrich metals, which can reduce the amount of processed materials in subsequent processing steps and further reduce reagent and energy consumption.

[0063] The present invention adopts electro-oxidation leaching and simultaneous electrolytic copper recovery technology, the electrolyte contains CuSO4, NH3·H2O, (NH4)2SO4, and ethylenediamine, wherein CuSO4 can react with NH3·H2O, (NH4)2SO4, and ethylenediamine to generate Cu(NH3)4 2+ 、Cu(en)2 2+ By adding ethylenediamine to the electrolyte, not only can the amount of ammonia used be reduced, but also the copper recovery rate can be accelerated. A cathode copper-clad plate with a smooth and dense surface can be obtained at a low current density. The recovery rate of copper on the cathode plate is more than 90%, and the purity is more than 90%. Since the concentration of copper ions changes significantly during the electrolysis process, the present invention performs electrolysis in a constant current mode, controls the current to keep the current constant, so as to prevent Cu(NH3)4 in the solution from 2+ 、Cu(en)2 2+ The decrease in concentration reduces the electrodeposition efficiency, thereby ensuring uniform generation of cathode electrodeposition products.

[0064] The present invention adopts electro-oxidation leaching and synchronous electrowinning gold recovery technology, recovers gold in a constant voltage electrolysis mode, and accurately controls voltage parameters, that is, accurately controls electrode potential, so as to ensure that the electro-oxidation leaching process and the electrodeposition process are conducive to the occurrence of main reactions and reduce the occurrence of side reactions, thereby realizing selective electro-oxidation leaching of gold at the anode, and further realizing step-by-step recovery of gold and copper. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] Figure 1 A process flow chart of a method for recovering gold and copper from waste printed circuit boards in steps according to an embodiment of the present invention;

[0066] Figure 2 The XRD pattern of electroplated gold obtained in Example 1 of the present invention;

[0067] Figure 3 The XRD diagram of the electrodeposited copper obtained in Example 1 of the present invention;

[0068] Figure 4 A process flow chart of a method for recovering gold and copper from waste printed circuit boards in steps according to another embodiment of the present invention;

[0069] Figure 5 The electrolytic kinetics of electro-oxidation leaching and simultaneous electro-winning recovery of gold in the scheme of electro-oxidation leaching and simultaneous electro-winning recovery of gold-flotation-electro-oxidation leaching and simultaneous electro-winning recovery of copper of the present invention;

[0070] Figure 6 This is the EDS spectrum of the circuit board before electro-oxidation leaching and simultaneous electrowinning gold recovery in Example 5 of the present invention;

[0071] Figure 7 This is the EDS spectrum of the circuit board after electro-oxidation leaching and simultaneous electrowinning gold recovery in Example 5 of the present invention. DETAILED DESCRIPTION

[0072] In order to make the technical problems, technical solutions and advantages to be solved by the present invention clearer, the following will be described in detail with reference to the accompanying drawings and specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0073] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other. The reagents and instruments used in the examples are conventionally selected in the art unless otherwise specified. The experimental methods without specific conditions in the examples are implemented according to conventional conditions, such as the conditions described in the literature, books or methods recommended by the manufacturer.

[0074] Example 1

[0075] This embodiment provides a technical solution of flotation-electro-oxidation leaching synchronous electrowinning to recover copper-electro-oxidation leaching synchronous electrowinning to recover gold. The process flow is as shown in the attached figure. Figure 1 As shown, the following steps are included:

[0076] SA1 flotation: crush the waste printed circuit boards to a particle size of less than 0.425 mm, add ethanol to the flotation tank, the volume mass ratio of ethanol to the waste printed circuit boards is 1 ml / g, add water to make the solid-liquid ratio 100 g / L, flotation to obtain foam products and tank products, the yield of the tank products is 66.43%, and the recovery rates of gold and copper are 94.82% and 92.57% respectively;

[0077] SA2 electro-oxidation leaching and simultaneous electrowinning to recover copper: add the product in the tank to the anode chamber of the electrolytic cell. A double-layer acid-base resistant filter cloth is used to separate the anode chamber and the cathode chamber in the electrolytic cell. Titanium plate and DSA plate are used as cathode and anode respectively. An alkaline solution containing 0.2mol / L CuSO4, 0.25mol / L (NH4)2SO4, 0.2mol / L NH3·H2O and 0.4mol / L ethylenediamine is used as the electrolyte. The solid-liquid ratio is 20g / L. Turn on the power supply and set the current density to 15mA / cm 2 After 5 hours of electrolysis, the electrodeposited copper was recovered on the cathode plate to obtain a copper product with a purity of 99.96%, and the recovery rate of the electrodeposited copper reached 98.03%.

[0078] SA3 electro-oxidation leaching and simultaneous electrowinning recovery of gold: The leaching residue obtained in step SA2 is placed in an electrolytic cell, and carbon fiber and DSA plate are used as cathode and anode respectively. In an electrolyte of 25g / L potassium iodide, the electrolysis voltage is set to 4V, and the solid-liquid ratio is 125g / L. After electrolysis for 2h, the electrodeposited gold is recovered on the cathode plate. The leaching rate of electro-oxidized gold is 99.18%, and the recovery rate of electrodeposited gold is 91.59%.

[0079] like Figure 2 The XRD diagram of the electroplated gold obtained in this embodiment is shown as follows: Figure 3 The XRD diagram of electrolytic copper obtained in this embodiment is: Figure 2 and Figure 3 It was proved that high purity gold and copper were obtained respectively.

[0080] Example 2

[0081] The steps are the same as those in Example 1. Compared with Example 1, the difference is that the concentration of (NH4)2SO4 in step SA2 is 0.20 mol / L, and the electrolysis voltage in step SA3 is 5 V. It is found that copper with a purity of 99.87% is obtained on the cathode plate, and the recovery rate of cathode electrodeposited copper is 93.34%; the leaching rate of electro-oxidized gold is 97.77%, and the recovery rate of electrodeposited gold is 85.99%.

[0082] Example 3

[0083] The steps are the same as those in Example 1. The difference from Example 1 is that the current density in step SA2 is 20 mA / cm 2The concentration of potassium iodide in step SA3 was 20 g / L. The results showed that copper with a purity of 99.91% was obtained on the cathode plate, and the recovery rate of cathode electrodeposited copper reached 96.05%; the leaching rate of electro-oxidized gold was 90.28%, and the recovery rate of electrodeposited gold reached 81.52%.

[0084] Example 4

[0085] The steps are the same as those in Example 1. Compared with Example 1, the difference is that the concentration of ammonia water in step SA2 is 3 mol / L, and the solid-liquid ratio in step SA3 is 200 g / L. It is found that copper with a purity of 99.95% is obtained on the cathode plate, and the recovery rate of cathode electrodeposited copper is 94.33%; the leaching rate of electro-oxidized gold is 89.37%, and the recovery rate of electrodeposited gold is 85.39%.

[0086] Example 5

[0087] This embodiment provides a technical solution of electro-oxidation leaching and synchronous electro-winning to recover gold - flotation - electro-oxidation leaching and synchronous electro-winning to recover copper. The process flow is as shown in the attached figure. Figure 4 As shown, the following steps are included:

[0088] SB1 electro-oxidation leaching and simultaneous electrowinning recovery of gold: The metal surface layer of the waste printed circuit board is used as the anode and the carbon brazing fiber is used as the cathode. 2wt% thiourea and 2wt% sodium chloride and 35mg / L AuCl4 - The mixed solution was used as the electrolyte, the distance between the anode and the cathode was adjusted to 5 cm, the DC power supply voltage was 2 V, the electrolysis time of each waste printed circuit board was 10 s, and a total of 15 waste printed circuit boards were replaced. The electro-oxidation leaching rate of gold reached 98.00%, and the recovery rate of electro-deposited gold reached 91.36%;

[0089] like Figure 5 As shown in FIG. 1 , through electrolysis kinetics research, it is found that in the thiourea-sodium chloride-chloroaurate electrolyte, the electrolysis time of each waste printed circuit board is precisely controlled to be 5 to 15 seconds, which can achieve the priority recovery of gold on the surface layer of the waste printed circuit board and reduce the loss of gold in the pretreatment process. At this time, the concentration of copper and nickel is still low, thereby achieving the separation of gold from copper and nickel and reducing the difficulty of separation in subsequent processes; Figure 6 and Figure 7 The following are the EDS spectra of the circuit board before and after the electro-oxidation leaching and simultaneous electrowinning gold recovery in this embodiment. Figure 6 and Figure 7 It can be seen that after electro-oxidation leaching, the gold on the outermost layer of the waste printed circuit board is basically completely leached;

[0090] SB2 flotation: The waste printed circuit boards treated in step SB1 are taken out and crushed to a particle size of less than 0.425 mm. Ethanol is added to the flotation tank, and the volume mass ratio of ethanol to the waste printed circuit boards is 1 ml / g. Water is added to make the solid-liquid ratio 100 g / L. The foam product and the in-tank product are obtained by flotation. The yield of the in-tank product is 65.78%, and the recovery rates of gold and copper are 95.07% and 93.05%, respectively.

[0091] SB3 electro-oxidation leaching and synchronous electrowinning to recover copper: the product in step SB3 is added to the anode chamber of the electrolytic cell. A double-layer acid-base resistant filter cloth is used to separate the anode chamber and the cathode chamber in the electrolytic cell. The titanium plate and the DSA plate are used as the cathode and the anode, respectively. An alkaline solution containing 0.2 mol / L CuSO4, 0.25 mol / L (NH4)2SO4, 0.2 mol / L NH3·H2O and 0.4 mol / L ethylenediamine is used as the electrolyte, and the solid-liquid ratio is 20 g / L. The power is turned on and the current density is set to 15 mA / cm 2 After 5 hours of electrolysis, the electrodeposited copper was recovered on the cathode plate to obtain a copper product with a purity of 99.95%, and the recovery rate of the electrodeposited copper reached 98.96%.

[0092] Example 6

[0093] The steps are the same as those in Example 5. Compared with Example 5, the difference is that the sodium chloride content in step SB1 is 1wt%, and the ethylenediamine concentration in step SB3 is 0.5mol / L. The results show that the gold leaching rate in a single electrolysis process reaches 90.84%, and the recovery rate of electrolytic gold reaches 82.39%; copper with a purity of 99.82% is obtained on the cathode plate, and the recovery rate of cathode electrodeposited copper reaches 93.38%.

[0094] Example 7

[0095] The steps are the same as those in Example 5. Compared with Example 5, the difference is that the voltage in step SB1 is 1.8V, and the solid-liquid ratio in step SB3 is 15g / L. The results show that the gold leaching rate in a single electrolysis process reaches 93.43%, and the recovery rate of electrolytic gold reaches 85.96%; copper with a purity of 99.90% is obtained on the cathode plate, and the recovery rate of cathode electrodeposited copper reaches 99.27%.

[0096] Example 8

[0097] The steps are the same as those in Example 5. Compared with Example 5, the difference is that the electrolysis time of each waste printed circuit board in step SB1 is 15 seconds, a total of 15 waste printed circuit boards are replaced, and the electrolysis time in step SB3 is 5.5 hours. The results show that the gold leaching rate in a single electrolysis process reaches 99.91%, and the recovery rate of electrolytic gold reaches 89.37%; copper with a purity of 99.85% is obtained on the cathode plate, and the recovery rate of cathode electrodeposited copper reaches 99.24%.

[0098] Comparative Example 1

[0099] Compared with Example 1, the difference is that ethylenediamine is not added in step SA2, and other operations and parameters are the same as Example 1. It is found that copper with a purity of 99.93% is obtained on the cathode plate, and the recovery rate of cathode electrodeposited copper is only 8.63%, indicating that ethylenediamine has little effect on the electro-oxidation process, but in the electrowinning process, ethylenediamine coordinates with copper ions in the solution, which can effectively promote the electrowinning reaction. The lack of ethylenediamine seriously affects the electrowinning of copper.

[0100] Comparative Example 2

[0101] Compared with Example 5, the difference is that thiourea is not added to the electrolyte in step SB1, and other operations and parameters are the same as Example 5. The results show that the gold leaching rate in a single electrolysis process is almost 0, and gold cannot be recovered by electroplating, indicating that the coordination of thiourea with gold in the electrolysis process is the dominant role in leaching gold.

[0102] Comparative Example 3

[0103] Compared with Example 5, the difference is that sodium chloride is not added to the electrolyte in step SB1, and other operations and parameters are the same as Example 5. The results show that the electro-oxidation leaching rate of gold is only 54.92%, and the recovery rate of electro-deposited gold is only 63.58%. Both the leaching rate and the recovery rate are lower than those in Example 5. The main reason is that sodium chloride can enhance the conductivity of the electrolyte. Without adding sodium chloride, the conductivity of the electrolyte decreases, which affects the electro-oxidation leaching process.

[0104] Comparative Example 4

[0105] Compared with Example 5, the difference is that the DC voltage in step SB1 is 1.4V, and the other operations and parameters are the same as Example 5. The results show that the gold leaching rate in a single electrolysis process is only 6.82%, and the recovery rate of electrodeposited gold is only 0.013%, indicating that a sufficiently high DC voltage must be maintained in this step to leach the gold.

[0106] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for recovering gold and copper from waste printed circuit boards in steps, It is characterized in that Including flotation, electro-oxidation leaching and simultaneous electro-winning to recover copper and electro-oxidation leaching and simultaneous electro-winning to recover gold; The flotation step specifically includes: crushing the waste printed circuit boards to a particle size of less than 0.425 mm, and then mixing with water and a wetting agent for flotation to obtain a foam product and a tank product; The electro-oxidation leaching and simultaneous electro-winning copper recovery step specifically comprises: placing the product in the cell into an electrolytic cell, performing electro-oxidation leaching with a copper-ammonia alkaline electrolyte, and simultaneously electro-winning copper recovery to obtain leaching slag and electro-winning copper; the copper-ammonia alkaline electrolyte contains CuSO 4 NH 4 ) 2 SO 4 NH 3 ·H 2 O and ethylenediamine; When the electro-oxidation leaching and simultaneous electro-winning gold recovery step is after the electro-oxidation leaching and simultaneous electro-winning copper recovery step, the process specifically comprises: placing the leached residue obtained from the electro-oxidation leaching and simultaneous electro-winning copper recovery step into an electrolytic cell, performing electro-oxidation leaching with potassium iodide electrolyte, and simultaneously electro-winning gold recovery; When the electro-oxidation leaching and simultaneous electro-winning gold recovery step is before the flotation step, it specifically includes: using the waste printed circuit board as the anode, electro-oxidation leaching gold in a thiourea-sodium chloride-chloroaurate electrolyte, and simultaneously electro-winning gold recovery, and in the same electro-winning cycle, replacing the waste printed circuit board of the anode at least 10 times to enrich the gold at the cathode.

2. The method according to claim 1, It is characterized in that In the copper ammonia alkaline electrolyte, CuSO 4 The concentration is 0.05~0.3mol / L, (NH 4 ) 2 SO 4 The concentration is 0.1~0.3mol / L, NH 3 ·H 2 The O concentration is 0.1-0.3 mol / L, and the ethylenediamine concentration is 0.1-0.6 mol / L.

3. The method according to claim 1, It is characterized in that In the electro-oxidation leaching and simultaneous electro-winning copper recovery step, the current density is 10-30 mA / cm 2 The electrolysis time is 3 to 7 hours, and the solid-liquid ratio is 10 to 40 g / L.

4. The method according to claim 1, It is characterized in that In the electro-oxidation leaching and simultaneous electro-winning copper recovery step, the anode is selected from any one of DSA, graphite and titanium mesh, and the cathode is a titanium plate.

5. The method according to claim 1, It is characterized in that When the electro-oxidation leaching and simultaneous electrowinning step of recovering gold is after the electro-oxidation leaching and simultaneous electrowinning step of recovering copper, the concentration of potassium iodide in the potassium iodide electrolyte is 5-30 g / L, the electrolysis voltage is 2-6 V, the electrolysis time is 0.5-3 h, and the solid-liquid ratio is 100-200 g / L.

6. The method according to claim 1, It is characterized in that When the electro-oxidation leaching and simultaneous electrowinning step of recovering gold is after the electro-oxidation leaching and simultaneous electrowinning step of recovering copper, the anode is selected from any one of DSA, graphite and titanium mesh, and the cathode is selected from any one of graphite, titanium mesh and carbon fiber.

7. The method according to claim 1, It is characterized in that When the electro-oxidation leaching and simultaneous electrowinning step of recovering gold is before the flotation step, in the thiourea-sodium chloride-chloroaurate electrolyte, the thiourea content is 0.5wt%-4wt%, the sodium chloride content is 0.5wt%-4wt%, and the chloroaurate concentration is 30-40mg / L; the cathode is selected from any one of graphite, titanium mesh and carbon fiber, the distance between the anode and the cathode is 3-10cm, the electrolysis voltage is 1.5-4V, and the electrolysis time of each waste printed circuit board is 5s-18min.

8. The method according to any one of claims 1 to 7, It is characterized in that The chloroaurate ion comes from any one or more of tetrachloroauric acid, sodium chloroaurate or potassium chloroaurate.

9. The method according to any one of claims 1 to 7, It is characterized in that The wetting agent is one or more of ethanol, ethylene glycol and glycerol.

10. The method according to any one of claims 1 to 7, It is characterized in that In the flotation step, the volume mass ratio of the wetting agent to the waste printed circuit board is 0.5-2 ml / g, and the solid-liquid ratio is 50-150 g / L.

Citation Information

Patent Citations

  • Method for recovering pure copper from waste circuit board

    CN108677021A

  • Method for preparing electro deposited copper through alkaline etching effluent

    CN109371422A

  • Method of selective electrolytic leaching recycling gold and copper from waste memory strips

    CN109797407A

  • Method for recovering circuit board metal on basis of drum type anode rotary electrolysis device

    CN110438337A

  • Environmentally friendly process to optimize copper dissolution and recover copper and gold from electronic waste