Method for recovering gallium from high-acidity hydrochloric acid solution by using P204
By using P204 as the extraction agent in a high acidity hydrochloric acid solution, combined with countercurrent extraction, impurity removal and electrolysis steps, the recycling efficiency and selectivity of gallium are successfully improved, and the problems of gallium resource waste and environmental pollution in the prior art are solved, thus achieving the realization of the problem of gallium resource waste and environmental pollution in the existing technology. Low-cost and efficient gallium recycling process.
Patent Information
- Application Number
- CN202411039996.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
In the existing gallium recovery methods, the recycling efficiency of gallium in high acidity hydrochloric acid solution is low, resource waste is serious, and the process is complex, environmental pollution and cost are high, the selectivity is poor, and the impurity separation is incomplete.
P204 is used as the extraction agent, and anionic GaCl4- is formed with Ga3+ under high acidity conditions through countercurrent extraction. Combined with sodium sulfide removal, sodium sulfite reduction and sodium hydroxide dissolution, and finally electrolyzed to obtain metal gallium.
It has achieved efficient recycling of gallium, simple process, low cost, and environmentally friendly. The direct yield of gallium reaches more than 90%, and the direct yield of germanium reaches more than 80%, which is suitable for industrial promotion.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hydrometallurgy, and in particular to a method for recovering gallium from a high-acidity hydrochloric acid solution by using P204. Background Art
[0002] Gallium is an important rare and dispersed metal, which is widely used in semiconductor light-emitting diodes, LEDs, integrated circuits, chemical catalysts, low-melting alloys, new energy, optics, thermodynamics and other fields. Gallium has no independent deposits and is highly dispersed in nature. It has a strong affinity with sulfur and often coexists with aluminum, silicon, iron, zinc, indium, germanium, tin, titanium, chromium and other elements in other metal mines. It is mainly recovered as a by-product from the metallurgical process of minerals such as bauxite, lead-zinc ore, ilmenite, and apatite. P204 (2-[2-ethylhexyl] phosphoric acid) is a colorless, transparent and viscous liquid, mostly used as an organic solvent and an acidic extractant. It exists in kerosene as a hydrogen-bonded dimer structure to cover its polar phosphate group. When complexed with metal ions, it usually participates in the reaction in the form of dimers.
[0003] At present, the main methods for recovering gallium are: chlorination distillation, electrolysis, ion exchange, resin adsorption, tannin, and extraction. Among them, chlorination distillation and tannin have high requirements for equipment and are easy to pollute the environment; electrolysis has high cost and low efficiency; ion exchange and resin adsorption require a lot of water and increase emissions due to inherent process limitations, and are costly and difficult to industrialize. In contrast, the extraction method has lower equipment requirements, simple operation, and can achieve a higher recovery rate, with a broad application prospect.
[0004] However, in the past, the high-acidity hydrochloric acid solution was simply recovered from the hydrochloric acid, and then lime and other precipitants were used for wastewater treatment. Gallium was not effectively recovered, resulting in a waste of resources. Although gallium, indium, and germanium in high-acidity hydrochloric acid solutions are gradually being recovered to achieve resource reuse. However, ethyl acetate, tributyl phosphate, etc. are mostly used as extractants to recover the valuable metals therein, which has poor selectivity, imperfect impurity separation, and a small gallium enrichment multiple. For example, a Chinese patent (publication number: CN101717868A) discloses a method for comprehensive recovery of indium and gallium from distilled waste acid, and the extractant is expensive, volatile, and has a poor operating environment; a Chinese patent (publication number: CN100396804C) discloses a method for extracting metallic gallium from lead-zinc ore tailings by extraction-electrolysis, which has a long process flow and is unfavorable to production costs and the environment. Summary of the invention
[0005] The present invention is intended to provide a method for recovering gallium from a high-acidity hydrochloric acid solution using P204, wherein P204 is used for extraction under high-acidity conditions. 3+With P204 in water phase to coordinate anion GaCl4 - The extraction is carried out by exchanging and associating extractants in the form of ions. It has a more perfect separation of impurities, a simple process flow, no pollution to the environment, and low production cost.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] A method for recovering gallium from a high-acidity hydrochloric acid solution using P204 comprises the following steps:
[0008] S1. Using countercurrent extraction method, P204-kerosene is used as an extractant to directly extract high-acidity hydrochloric acid solution;
[0009] S2, the obtained gallium-loaded organic phase is washed with tap water at level 1, the washing water level is connected to the extraction level, and the washing water enters the extraction section;
[0010] S3, add the stripping agent into the extraction box, stir it with the original solution, and add sodium sulfide to remove impurities;
[0011] S4, regeneration of the lean organic phase with hydrofluoric acid;
[0012] S5, first adjusting the pH of the solution after impurity removal, then adding a reducing agent for reduction, and detecting the trivalent iron in the solution; after passing the test, adjusting the pH of the solution again to precipitate gallium, and producing a crude gallium cake;
[0013] S6, dissolving the crude gallium cake to obtain an electrolytic mother solution;
[0014] S7. The electrolyte is electrolyzed to obtain metallic gallium.
[0015] Furthermore, in S1, the volume ratio of P204 to kerosene in P204-kerosene is 3:7; and the concentration of hydrochloric acid in the high-acidity hydrochloric acid solution is 4-7.5 mol / L.
[0016] Furthermore, in S1, the number of extraction stages is 3, the extraction time is 2 to 5 minutes, and the volume ratio of the aqueous phase to the organic phase is 2 to 10:1.
[0017] Furthermore, in S2, the volume ratio of water to organic phase is 1:20-40.
[0018] Furthermore, in S4, the method for regenerating the lean organic phase with hydrofluoric acid is: washing the organic phase with 2 mol / L hydrofluoric acid or 8 mol / L hydrochloric acid to recycle it; the extraction level is 3, the extraction time is 3 minutes, and the volume ratio of the aqueous phase to the organic phase is 1:5 to 15.
[0019] Furthermore, in S3, 0.25-0.5 mol / L sulfuric acid is selected as the organic phase reverse extraction agent.
[0020] Further, in S3, a stripping agent is added into the extraction box, and the extraction stage is 4, the extraction time is 4 minutes, and the volume ratio of the aqueous phase to the organic phase is 1:10-40.
[0021] Further, in S5, the pH of the solution after impurity removal is adjusted to 1.0; sodium sulfite is selected as the reducing agent, and the reduction time is 30 minutes; 5% potassium thiocyanate solution is used to detect trivalent iron; and sodium bicarbonate is used to adjust the pH of the solution to 4.0-4.5 when precipitating gallium.
[0022] Furthermore, in S6, 300 g / L of sodium hydroxide is used or residual liquid is electrolyzed to dissolve the crude gallium cake.
[0023] Furthermore, in S7, stainless steel is used as the cathode and anode, and the electrolyte is electrolyzed at a voltage of 2.5 to 3.5 volts and a current density of 300 to 450 amperes per square meter.
[0024] The principle and beneficial effects of the technical solution are:
[0025] P204 is used as an extractant, kerosene is used as a diluent, and countercurrent extraction is used to directly extract the distillation residue. Sodium sulfide is added to the back-extracted liquid to further remove impurities, sodium sulfite is reduced and precipitated, sodium hydroxide is dissolved, and electrolysis is performed to obtain metallic gallium.
[0026] The method provided by the present invention has the advantages of simple process, short flow, low cost, high direct recovery rate, no pollution to the environment, and easy to promote and apply in factories; experimental data show that the direct recovery rate of gallium by this method is more than 90%, and the direct recovery rate of germanium can also reach more than 80%. DETAILED DESCRIPTION
[0027] The following specific embodiments further describe the present invention in detail:
[0028] A method for recovering gallium from a high-acidity hydrochloric acid solution using P204 comprises the following steps:
[0029] S1. Using countercurrent extraction method to directly extract high-acidity hydrochloric acid solution with P204-kerosene as an extractant; wherein the volume ratio of P204 to kerosene in P204-kerosene is 3:7, and the concentration of hydrochloric acid in the high-acidity hydrochloric acid solution is 4-7.5 mol / L; the extraction level is 3, the extraction time is 2-5 minutes, and the volume ratio of aqueous phase to organic phase is 2-10:1;
[0030] S2, the obtained gallium-loaded organic phase is washed with tap water at level 1, the washing water level is connected to the extraction level, and the washing water enters the extraction section, and the volume ratio of water to organic phase is 1:20-40;
[0031] S3, adding a stripping agent into the extraction box, stirring it with the original solution, and adding sodium sulfide to remove impurities; wherein the organic phase stripping agent is 0.25-0.5 mol / L sulfuric acid; and using a liquid pump to add the stripping agent into the reaction barrel, the extraction level is 4, the extraction time is 4 minutes, and the volume ratio of the aqueous phase to the organic phase is 1:10-40;
[0032] S4, regenerating the lean organic phase with hydrofluoric acid; wherein the specific method is: washing the organic phase with 2 mol / L hydrofluoric acid or 8 mol / L hydrochloric acid to recycle it; the extraction level is 3, the extraction time is 3 minutes, and the volume ratio of the aqueous phase to the organic phase is 1:5-15;
[0033] S5, first adjust the pH of the solution after impurity removal to 1.0, then add a reducing agent for reduction, and detect the trivalent iron in the solution; after passing the test, adjust the pH of the solution to 4.0-4.5 to precipitate gallium and produce a crude gallium cake; wherein the reducing agent is sodium sulfite, and the reduction time is 30 minutes; use 5% potassium thiocyanate solution to detect trivalent iron; use sodium bicarbonate to adjust the solution pH when precipitating gallium;
[0034] S6, dissolving the crude gallium cake to obtain an electrolytic mother solution; wherein the crude gallium cake is dissolved by using 300 g / L of sodium hydroxide or electrolytic residual solution;
[0035] S7. The electrolyte uses stainless steel as the cathode and anode, and is electrolyzed at a voltage of 2.5 to 3.5 volts and a current density of 300 to 450 amperes per square meter to obtain metallic gallium.
[0036] Embodiment 1
[0037] The gallium-containing high-acidity hydrochloric acid solution used in this embodiment comes from the germanium distillation residue of a smelter, and its main components are: Ga: 2.1 g / L, Ge: 0.08 g / L, Sn: 3.5 g / L, Fe: 13 g / L, Cu; 2.0 g / L, HCl: 6.5 mol / L.
[0038] The specific methods for recycling gallium and germanium are as follows:
[0039] Take 2000L of gallium-containing distillation residue and pump it into the high-level tank. P204, stripping solution and organic phase regeneration solution are all prepared in advance. Turn on the 30-liter extractor and extract according to the distillation residue flow rate of 7.5L / min, organic phase flow rate of 2.5L / min, washing water flow rate of 0.1L / min, stripping solution flow rate of 0.25L / min and regeneration solution flow rate of 0.25L / min. 60L of stripping solution containing Ga: 69.4g / L; Ge: 2.2g / L, gallium extraction plus stripping The recovery rate is 99%, and the germanium recovery rate is 85%; the stripping solution is impurity-removed by adding Na2S to obtain 3300g of sulfide slag, containing Ga: 0.1%; Ge: 3.96%; the impurity-removed solution is reduced with sodium sulfite and precipitated with sodium carbonate to obtain a crude gallium cake; the crude gallium cake is dissolved with sodium hydroxide at a dissolution temperature of 90°C for 4 hours, and 45 liters of electrolytic mother liquor is filtered to obtain 86.16g / L Ga and 125g / L NaOH; 3799.5g of metallic gallium is obtained by electrolysis, and the direct gallium yield is 90.5%.
[0040] Embodiment 2
[0041] The gallium-containing high-acidity hydrochloric acid solution used in this embodiment comes from the germanium distillation residue of a smelter, and its main components are: Ga: 2.1 g / L, Ge: 0.08 g / L, Sn: 3.5 g / L, Fe: 13 g / L, Cu; 2.0 g / L, HCl: 6.5 mol / L.
[0042] The specific methods for recycling gallium and germanium are as follows:
[0043] Take 2000L of gallium-containing distillation residue and add 1500L of 10mol / L HCI to make the solution HCI reach 8mol / L, pump it into the high-level tank, P204, stripping solution and organic phase regeneration solution are all prepared in advance, open the extraction machine with a volume of 30L, extract according to the flow rate of prepared solution 7.5L / min, organic phase flow rate 1.5L / min, washing water flow rate 0.12L / min, stripping solution flow rate 0.15L / min, regeneration solution flow rate 0.2L / min; get 70L stripping solution containing Ga: 59.52g / L; Ge: 1.9g / L, the gallium extraction and stripping recovery rate is 99.2%, and the germanium recovery rate is 86%; the stripping solution is impurity-removed by adding Na2S to obtain 3000g of sulfide slag, containing Ga: 0.1%; Ge: 4.39%; the impurity-removed solution is reduced with sodium sulfite and precipitated with sodium carbonate to obtain a crude gallium cake; the crude gallium cake is dissolved with sodium hydroxide at a dissolution temperature of 90°C for 4 hours, and 45 liters of electrolytic mother liquor is filtered, containing Ga: 87.1g / L, NaOH: 128g / L; 3840.1g of metallic gallium is obtained by electrolysis, and the direct gallium yield is 91.4%.
[0044] Embodiment 3
[0045] The gallium-containing high-acidity hydrochloric acid solution used in this embodiment comes from the germanium distillation residue of a smelter, and its main components are: Ga: 2.1 g / L, Ge: 0.08 g / L, Sn: 3.5 g / L, Fe: 13 g / L, Cu; 2.0 g / L, HCl: 6.5 mol / L.
[0046] The specific methods for recycling gallium and germanium are as follows:
[0047] Take 2000L of gallium-containing distillation residue and add 340L of H2O to make the solution HCl 5.5mol / L, pump it into the high-level tank, prepare P204, stripping solution and organic phase regeneration solution in advance, start the 30L extraction machine, extract according to the distillation residue flow rate of 7.5L / min, organic phase flow rate of 2.5L / min, washing water flow rate of 0.1L / min, stripping solution flow rate of 0.25L / min, and regeneration solution flow rate of 0.25L / min; get 78L of stripping solution containing Ga: 49.5g / L; Ge: 1.6g / L, gallium The extraction and stripping recovery rate is 92%, and the germanium recovery rate is 78%. The stripping solution is impurity-removed by adding Na2S to obtain 4200g of sulfide slag, containing Ga: 0.1%; Ge: 2.94%. The impurity-removed solution is reduced with sodium sulfite and precipitated with sodium carbonate to obtain a crude gallium cake. The crude gallium cake is dissolved with sodium hydroxide at a dissolution temperature of 90°C for 4 hours, and 45 liters of electrolytic mother liquor is filtered to obtain Ga: 80.7g / L, NaOH: 125g / L; 3558.6g of metallic gallium is obtained by electrolysis, and the direct gallium yield is 84.7%.
[0048] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, several modifications and improvements can be made without departing from the technical solution of the present invention, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.
Claims
1. A method for recovering gallium from a highly acidic hydrochloric acid solution using P204, characterized in that: The following steps are involved: S1. Using countercurrent extraction method, P204-kerosene is used as an extractant to directly extract high-acidity hydrochloric acid solution; S2, the obtained gallium-loaded organic phase is washed with tap water at level 1, the washing water level is connected to the extraction level, and the washing water enters the extraction section; S3, after washing, the organic phase is stripped by adding a stripping agent, and the stripping solution is stripped by adding sodium sulfide to remove impurities; S4, regeneration of the lean organic phase with hydrofluoric acid; S5, first adjusting the pH of the solution after impurity removal, then adding a reducing agent for reduction, and detecting the trivalent iron in the solution; after passing the test, adjusting the pH of the solution again to precipitate gallium, and producing a crude gallium cake; S6, dissolving the crude gallium cake to obtain an electrolytic mother solution; S7. The electrolyte is electrolyzed to obtain metallic gallium.
2. The method for recovering gallium from a high-acidity hydrochloric acid solution using P204 according to claim 1, characterized in that: In S1, the volume ratio of P204 to kerosene in P204-kerosene is 3:7; the concentration of hydrochloric acid in the high-acidity hydrochloric acid solution is 4-7.5 mol / L.
3. The method for recovering gallium from a high-acidity hydrochloric acid solution using P204 according to claim 1, characterized in that: In S1, the number of extraction stages is 3, the extraction time is 2 to 5 minutes, and the volume ratio of the aqueous phase to the organic phase is 2 to 10:
1.
4. The method for recovering gallium from a high-acidity hydrochloric acid solution using P204 according to claim 1, characterized in that: In S2, the volume ratio of water to organic phase is 1:20-40.
5. The method for recovering gallium from a high-acidity hydrochloric acid solution using P204 according to claim 1, characterized in that: In S4, the method of regenerating the lean organic phase with hydrofluoric acid is: washing the organic phase with 2 mol / L hydrofluoric acid or 8 mol / L hydrochloric acid to recycle it; the extraction stage is 3, the extraction time is 3 minutes, and the volume ratio of the aqueous phase to the organic phase is 1:5-15.
6. The method for recovering gallium from a high-acidity hydrochloric acid solution using P204 according to claim 1, characterized in that: In S3, 0.25-0.5 mol / L sulfuric acid is selected as the organic phase reverse extraction agent.
7. The method for recovering gallium from a high-acidity hydrochloric acid solution using P204 according to claim 1, characterized in that: In S3, a stripping agent is added into the extraction box, and the extraction stage is 4, the extraction time is 4 minutes, and the volume ratio of the aqueous phase to the organic phase is 1:10-40.
8. The method for recovering gallium from a high-acidity hydrochloric acid solution using P204 according to claim 1, characterized in that: In S5, the pH of the solution after impurity removal is adjusted to 1.0; sodium sulfite is selected as a reducing agent, and the reduction time is 30 minutes; 5% potassium thiocyanate solution is used to detect trivalent iron; and sodium bicarbonate is used to adjust the pH of the solution to 4.0-4.5 when precipitating gallium.
9. The method for recovering gallium from a high-acidity hydrochloric acid solution using P204 according to claim 1, characterized in that: In S6, 300 g / L of sodium hydroxide or electrolysis of residual liquid is used to dissolve the crude gallium cake.
10. The method for recovering gallium from a high-acidity hydrochloric acid solution using P204 according to claim 1, characterized in that: In S7, stainless steel is used as the cathode and anode, and the electrolyte is electrolyzed at a voltage of 2.5 to 3.5 volts and a current density of 300 to 450 amperes per square meter.
Citation Information
Patent Citations
Multi-metal recovery processing technique of waste liquid generated in germanium producing process
CN101671777A
Method for comprehensively recovering indium and gallium from distilled waste acid containing indium and gallium
CN101717868A
Method of enriching and purifying gallium from alkaline solution
CN110184483A
Method for extracting and separating gallium from zinc replaced residue sulfate leaching solution and application of method
CN111254295A
Technology for extracting Gallium metal from lead-zine tail ore slug smelting by extracting-electrolytic method
CN1775972A