Annealing-free medium-carbon cold heading steel wire rod for 10.9-grade bolt and production method of annealing-free medium-carbon cold heading steel wire rod
By controlling the Si content and final slag alkalinity, the heating temperature of the heat-hospital section is increased, and Steyrmo air-cooled line control is adopted to solve the problem of annealing process in the production of 10.9-level bolts, and the annealing-free cold heading steel strips are realized The production reduces costs and energy consumption, improves product quality and environmental performance.
Patent Information
- Application Number
- CN202411042554.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
The existing technology requires annealing process when producing 10.9-level bolts, resulting in a long steel annealing process cycle, high cost, large energy consumption and high greenhouse gas CO2 carbon emissions, which also affects product quality and increases production costs, which violates energy-saving and environmental protection policies.
By controlling the Si content and final slag alkalinity in the top-bottom reblowing converter and refining furnace, strictly controlling the peeling quality of the billet, increasing the heating temperature of the billet homogenization section, reducing the final rolling temperature, and using Steyrmo air-cooled line to control the cooling. Segmented cooling and slow cooling, control the thickness of the iron oxide sheet, reduce scratch defects, and realize the annealing-free production of cold heading steel strips.
The production of annealing-free cold heading steel strips for grade 10.9 bolts has been achieved, which reduces the hardness and tensile strength of the material, ensures the surface and internal quality of the cold heading steel, reduces production costs, and improves the plasticity and molding applicability of the product. , meets energy conservation and environmental protection requirements.
Smart Images

Figure CN118957441A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steel production and manufacturing, and specifically relates to an annealing-free medium-carbon cold-heading steel wire rod for 10.9-grade bolts and a production method thereof. Background Art
[0002] Cold heading steel wire is mainly used for cold heading to produce bolts, nuts and other fasteners or cold-formed parts, and has a wide range of uses. At present, the hot-rolled wire rods used to produce 10.9 grade bolts are mostly low-alloy medium-carbon cold heading steels containing Cr or CrMo. The tensile strength and hardness in the hot-rolled state are high, which is not suitable for the annealing-free direct drawing process. Therefore, it is necessary to anneal once before cold heading and then draw to make the material strength or hardness meet the drawing requirements. The steel annealing process has a long cycle, high production cost, high energy consumption and high greenhouse gas CO2 carbon emissions. At the same time, the annealing process will also increase the risk of decarbonization quality on the surface of the material. Moreover, the annealing process will also affect product quality, increase production costs, and violate the national carbon neutrality environmental protection policy. Therefore, in the current sluggish steel market and fierce homogeneous competition, and under the background of the country's "dual carbon", the development and promotion of energy-saving, green and environmentally friendly annealing-free cold heading steel is of far-reaching significance, which can improve the market competitiveness of products and achieve a win-win situation for manufacturers and customers.
[0003] At present, it is reported that some steel mills at home and abroad use hot machine rolling or low temperature rolling technology to produce annealing-free or simple annealing-free cold heading steel. On the one hand, the investment is large and the equipment requirements are high. On the other hand, the low temperature rolling technology will also bring negative effects such as scratches and unevenness on the surface of the wire. The Chinese patent with publication number CN104593679A discloses a 10.9-grade high-strength screw annealing-free cold heading steel wire and its production process. The annealing-free cold heading steel wire contains alloy elements such as Mo and Cr in a high content. At the same time, the production cost is high. With the addition of Cr and Mo, bainite (B) and martensite (M) structures are not easy to eliminate during the production process, and the hardness is high. The Chinese patent with the announcement number CN113877960B discloses a 10.9-grade annealing-free cold heading steel and a rolling method thereof, wherein the chemical composition of the 10.9-grade annealing-free cold heading steel includes: C, Si, Mn, P, S, Cr, Alt, Ti, B, V, Nb, Ni, rare earth elements, and the rest is Fe and unavoidable impurities, wherein the percentage of C in the composition is 0.42-0.44%, and precious alloy elements such as V, Nb and Ni are added at the same time, and the production cost is relatively high. The Chinese patent with the announcement number CN102321851B discloses a 10.9-grade boron-containing annealing-free cold heading steel wire rod and a manufacturing method thereof, wherein precious alloy elements such as V, Cr and Ni are added by reducing the content of C and Mn, and the production cost is relatively high. Therefore, how to reduce the tensile strength and hardness of the material through technological innovation and optimization of the controlled cooling process without increasing the production cost, combined with process equipment, while giving full play to the hardenability of alloy elements such as Ti, Cr and B in the 10B33 composition, without changing the tempering heat treatment process, to produce 10.9 grade high-strength annealing-free cold heading steel, meet the customer's annealing-free direct drawing process, reduce the customer's production cost and solve energy-saving and environmental protection problems, is the inevitable development trend to improve the competitiveness of the company's cold heading steel products in the future. Summary of the invention
[0004] In order to solve the deficiencies in the prior art, the object of the present invention is to provide an annealing-free medium carbon cold heading steel wire rod for 10.9 grade bolts and a production method thereof. The production method controls Si content and final slag basicity in a top and bottom combined blowing converter and a refining furnace, controls component elements Si and large particle inclusions that affect the deformation of cold heading steel wire rods, strictly controls the quality of steel billet peeling, especially the quality of corners, and increases the heating temperature of the steel billet soaking section, improves rolling plasticity, reduces the final rolling temperature, increases the wire laying temperature, controls the thickness of iron oxide scale and reduces scratch defects. At the same time, the Stelmor air cooling line adopts segmented cooling, with air cooling in the front section and slow cooling in the back section, controls the generation of full decarburization and the smoothness of the wire rod, and controls the cooling phase change by subsequent slow cooling, so that the cold heading steel wire rods produce more ferrite in the air cooling line to reduce the hardness of the material, ensure that the surface defects of the cold heading steel wire rods are few and the structure is uniform, the flange is uniformly deformed during the cold heading process, and the size is qualified, so as to ensure that the internal quality, surface quality and material plasticity of the annealing-free cold heading steel meet the cold heading, cost reduction and forming requirements of customers.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] The invention discloses an annealing-free medium carbon cold heading steel wire rod for 10.9 grade bolts. The chemical composition of the wire rod, measured by mass percentage, comprises: C 0.30-0.36%, Si≤0.10%, Mn 0.60-0.80%, P≤0.015%, S≤0.010%, Cr 0.10-0.30%, B 0.0008-0.0035%, Ti 0.020-0.050%, Al 0.020-0.050%, N≤0.0050%, and the rest is Fe and unavoidable impurity elements.
[0007] Furthermore, the chemical composition of the wire rod, measured in mass percentage, includes: C 0.32%, Si 0.06%, Mn 0.73%, P 0.012%, S 0.008%, Cr 0.13%, B 0.0018%, Ti 0.028%, Al 0.025%, N 0.0036%, and the rest is Fe and unavoidable impurity elements.
[0008] Furthermore, the production method comprises the following steps:
[0009] (1) using a top-bottom combined blowing converter to smelt the raw materials, and then adding lime, calcium slag balls and wollastonite to the smelted top-bottom combined blowing converter slag;
[0010] (2) After smelting, refining is carried out in an LF refining furnace;
[0011] (3) After refining, a continuous casting machine is used to continuously cast 150 mm × 150 mm square billets;
[0012] (4) After continuous casting, the steel billet is peeled and finished, and then the peeled and finished steel billet is heated;
[0013] (5) After the billet is heated, it is descaled by high-pressure water, and the billet after high-pressure water descaling is rolled by a short stress rolling mill and a reducing mill;
[0014] (6) The rolled steel billet is cooled by Stelmor air cooling line, and the phase change and wire rod passability are controlled by segmented cooling;
[0015] (7) The steel billet after controlled cooling in the Stelmore air-cooling line is coiled to obtain the annealing-free medium carbon cold heading steel wire rod.
[0016] Furthermore, the method of using a top and bottom combined blowing converter to melt the raw materials in the step (1) is as follows: a high-draw supplementary blowing method is used in a 120t top and bottom combined blowing converter to control the oxygen content, and the mass percentage of element C is controlled to be 0.08-0.25%, and the mass percentage of P is controlled to be ≤0.015%, the terminal temperature during smelting in the top and bottom combined blowing converter is controlled to be 1580-1680°C, and the amount of high carbon ferromanganese added is 9.29kg / t; the top and bottom combined blowing converter is alloyed after the furnace, and the mass percentage of each element is controlled to be C: 0.20-0.27%, Mn: 0.61-0.71%, Cr: 0.08-0.13%; 100±20kg / furnace of slag lime, 700±30kg / furnace of calcium slag balls, and 250±20kg / furnace of wollastonite are added to the top and bottom combined blowing converter after smelting.
[0017] Furthermore, during refining in step (2), the final slag basicity is controlled at 4.0-6.5, the white slag retention time is controlled at 15-45 min, the argon soft blowing flow rate is controlled at 14-30 NL / min, and the soft blowing time is controlled at 15-40 min.
[0018] Furthermore, in the step (3), the amount of secondary cooling water during continuous casting is 0.30 L / kg, the argon pressure at the long water inlet of the continuous casting ladle is controlled at 90-130 mbar, the middle ladle height is ≥400 mm, the continuous casting speed is controlled at 1.8-2.0 m / min, the current intensity of the electromagnetic stirring of the crystallizer is controlled at 330-370 A, and the current frequency is 3.5 Hz.
[0019] Furthermore, the specific method for peeling and finishing the steel billet in the step (4) is as follows: a fully automatic square billet grinding machine is used to fully grind the steel billet, a grinding wheel of 16 mesh or above is used, the face grinding depth is ≥1.0mm, the corner grinding depth is ≥7mm, the grinded steel billet surface and the junction between the corner and the face should be smooth, without edges or sharp corners, and there should be no burrs adhering to blocks. After grinding, magnetic particle inspection is performed. For local defects after grinding, the grinding depth is based on the defect being completely removed; the grinding width shall not be less than 6 times the grinding depth, and the grinding length shall not be less than 10 times the grinding depth. No un-grinded black edges or unremoved continuous casting billet defects shall appear on the steel billet surface; during heating in the step (4), the temperature of the first heating section is controlled at 600-800°C, the temperature of the second heating section is controlled at 950-1010°C, the temperature of the soaking section is controlled at 1060-1100°C, and the heating time is controlled at 80-130min.
[0020] Furthermore, in the step (5), the pressure of high-pressure water descaling is ≥20 MPa; the starting rolling temperature of the rolling is controlled at 930-1030°C, the sizing temperature is controlled at 820-840°C, and the spinning temperature is controlled at 780-860°C.
[0021] Furthermore, in step (6), the air volume of the first three fans during the Stelmor air-cooling line controlled cooling is 9900m 3 / h, the rear 7 fans are all closed, the front 3 insulation covers are open, and the rear insulation covers are all closed. The roller speed is 0.24m / s-0.26m / s-0.28m / s-0.30m / s-0.32m / s-0.34m / s-0.36m / s-0.38m / s-0.38m / s-0.38m / s-0.38m / s-0.42m / s-0.44m / s.
[0022] Furthermore, the specification of the wire rod obtained in step (7) is φ10-16mm; the tensile strength of the wire rod is ≤600MPa, and the 1 / 2 radius hardness of the wire rod is ≤83HRB.
[0023] Compared with the prior art, the present invention has the following positive and beneficial effects:
[0024] The present invention reduces the content of Si element in the cold heading steel wire rod by controlling the addition of silicon raw materials, improves the plasticity of the cold heading steel wire rod, is beneficial to cold heading deformation, and controls the final slag basicity to be between 4.0 and 6.5 during refining. The final slag basicity variation includes the low melting point region in the quaternary phase diagram. The refined slag with a large area has good fluidity, is beneficial to deoxidation, reduces the generation of large particle inclusions, and is beneficial to the processing and forming of parts with large deformation amount by cold heading. At the same time, the present invention also adopts a peeling finishing process for the steel billet, eliminates the surface defects of the steel billet, improves the heating temperature of the soaking section when the steel billet is heated, reduces the rolling deformation resistance of the steel billet and reduces the deformation uniformity of the corner of the steel billet in the box-shaped hole, can reduce the wrinkles or cluster scratches at the corner of the steel billet, and adopts a low-temperature rolling process to inhibit the crystallization of austenite and the growth of grains, thereby obtaining a fine austenite structure and increasing the nucleation probability of ferrite. On the other hand, the presence of deformation bands in austenite also increases The nucleation probability of ferrite is increased, the ferrite content is increased, the strength of the cold heading steel wire rod is reduced, and the plasticity of the cold heading steel wire rod is improved, so as to achieve the effect of cold heading steel wire rod without annealing and drawing; at the same time, after increasing the wire drawing temperature, the deformation resistance of the cold heading steel wire rod is reduced, and it is easy to form in the wire drawing tube, and the thickness of the iron oxide scale is increased, and the risk of scratching the cold heading steel wire rod in the wire drawing tube is reduced; the Stelmo roller adopts a suitable roller speed, turns off the fan and turns off the Close the insulation cover and adopt a slow cooling rate to increase the ferrite content, reduce the tensile strength and hardness of the cold heading steel wire rod and the uniformity of the wire rod, and at the same time improve the complete decarburization of the overlap point of the cold heading steel wire rod on the SM roller. After inspection, the annealing-free cold heading steel wire rod for 10.9 grade bolts can not only achieve 1 / 4 cold forging without cracking and a hardness of ≤82HRB, but also the uniformity of the cold heading steel wire rod is stable, which improves the applicability of the cold heading steel wire rod and reduces the production cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a comparison diagram of the structures of the annealing-free medium carbon cold heading steel wire rod 10B33M (right figure) of the present invention and the ordinary annealing-required medium carbon cold heading steel wire rod 10B33 (left figure);
[0026] Figure 2 This is a hardness comparison diagram of different specifications of the annealing-free medium carbon cold heading steel wire rod 10B33M of the present invention and the ordinary annealing-required medium carbon cold heading steel wire rod 10B33;
[0027] Figure 3 It is a 10.9 grade flange bolt produced from annealed medium carbon cold heading steel wire rod 10B33;
[0028] Figure 4 This is a 10.9 grade flange bolt produced by the annealing-free medium carbon cold heading steel wire rod 10B33M of the present invention;
[0029] Figure 5 The present invention is a 10.9 grade square head bolt produced by annealing-free medium carbon cold heading steel wire rod 10B33M. DETAILED DESCRIPTION
[0030] The technical solution of the present invention is further described below in conjunction with the embodiments, but is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention should be included in the protection scope of the present invention.
[0031] Example 1
[0032] The invention discloses an annealing-free medium-carbon cold heading steel wire rod for 10.9-grade bolts. The chemical composition of the wire rod, measured by mass percentage, comprises C: 0.32%, Si: 0.06%, Mn: 0.73%, P: 0.012%, S: 0.008%, Cr: 0.13%, B: 0.0018%, Ti: 0.028%, Al: 0.025%, N: 0.0036%, and the rest is Fe and unavoidable impurity elements.
[0033] A method for producing annealing-free medium carbon cold heading steel wire rod for 10.9 grade bolts comprises the following steps:
[0034] (1) A top-bottom combined blowing converter is used to smelt the raw materials, and then lime and wollastonite are added to the smelted slag of the top-bottom combined blowing converter. The specific method of smelting the raw materials by the top-bottom combined blowing converter is as follows: a high-draw supplementary blowing method is used in a 120t top-bottom combined blowing converter to control the oxygen content, and the mass percentage of element C is controlled to be 0.08-0.25%, and the mass percentage of P is controlled to be ≤0.015%. The terminal temperature during smelting in the top-bottom combined blowing converter is controlled to be 1580-1680°C, and the amount of high-carbon ferromanganese added is 9.29kg / t; the top-bottom combined blowing converter is alloyed after the furnace, and the mass percentage of each element is controlled to be C: 0.20-0.27%, Mn: 0.61-0.71%, and Cr: 0.08-0.13%; 100kg / furnace of slag lime, 697kg / furnace of calcium slag balls, and 242kg / furnace of wollastonite are added to the top-bottom combined blowing converter after smelting.
[0035] (2) After smelting, the LF refining furnace is used for refining. During refining, the final slag basicity is 5.5, the white slag retention time is controlled at 19 minutes, the argon soft blowing flow rate is controlled at 20NL / min, and the soft blowing time is controlled at 28 minutes;
[0036] (3) After refining, a continuous casting machine is used to continuously cast 150 mm × 150 mm square billets. During continuous casting, the amount of secondary cooling water is 0.30 L / kg, the argon pressure at the long water inlet of the continuous casting ladle is controlled at 116 mbar, the height of the middle ladle is 420 mm, the continuous casting speed is controlled at 1.9 m / min, the current intensity of the electromagnetic stirring of the crystallizer is controlled at 320 A, and the current frequency is 3.5 Hz;
[0037] (4) After continuous casting, the steel billet is peeled and finished, and then the peeled and finished steel billet is heated; wherein, the specific method of peeling and finishing the steel billet is as follows: the steel billet is fully ground by a fully automatic square billet grinding machine, a grinding wheel of 16 mesh or above is used, the grinding depth of the face is ≥1.0mm, the grinding depth of the corner is ≥7mm, the surface of the grinded steel billet and the joints between the corner and the face should be smooth, without edges or sharp corners, and there should be no burrs adhering to blocks; after grinding, magnetic particle inspection is performed, and for local defects after grinding, the grinding depth is based on the defect being completely removed; the grinding width shall not be less than 6 times the grinding depth, and the grinding length shall not be less than 10 times the grinding depth. There shall be no un-grinded black edges on the steel billet surface and the continuous casting billet defects that have not been completely removed; during heating, the temperature of the first heating section is controlled at 727°C, the temperature of the second heating section is controlled at 988°C, the temperature of the soaking section is controlled at 1074°C, and the heating time is controlled at 98min.
[0038] (5) After the billet is heated, high-pressure water is used to descale the billet, and the billet after high-pressure water descaling is rolled by a short stress rolling mill and a sizing mill; the pressure during high-pressure water descaling is 26 MPa; the rolling start temperature is 1020°C, the sizing temperature is 828°C, and the wire laying temperature is controlled at 850°C;
[0039] (6) The steel billet after rolling is cooled by Stelmore air cooling line, and the phase change and wire rod passability are controlled by segmented cooling. The air volume of the first three fans during Stelmore air cooling line is 9900m 3 / h, the rear 7 fans are all closed, the front 3 insulation covers are open, and the rear insulation covers are all closed, and the roller speed is 0.24m / s-0.26m / s-0.28m / s-0.30m / s-0.32m / s-0.34m / s-0.36m / s-0.38m / s-0.38m / s-0.38m / s-0.38m / s-0.42m / s-0.44m / s;
[0040] (7) The steel billet after Stelmor air-cooling line controlled cooling is coiled to obtain the annealing-free medium carbon cold heading steel wire rod. The specification of the obtained wire rod is φ11 mm, the tensile strength of the hot-rolled wire rod is 566.5 MPa, and the hardness at 1 / 2 radius is 79.3 HRB.
[0041] Example 2
[0042] The invention discloses an annealing-free medium-carbon cold heading steel wire rod for 10.9-grade bolts. The chemical composition of the wire rod, measured by mass percentage, comprises C: 0.33%, Si: 0.07%, Mn: 0.743%, P: 0.011%, S: 0.007%, Cr: 0.12%, B: 0.0020%, Ti: 0.036%, Al 0.028%, N: 0.0040%, and the rest is Fe and unavoidable impurity elements.
[0043] A method for producing annealing-free medium carbon cold heading steel wire rod for 10.9 grade bolts comprises the following steps:
[0044] (1) A top-bottom combined blowing converter is used to smelt the raw materials, and then lime and wollastonite are added to the smelted slag of the top-bottom combined blowing converter. The specific method of smelting the raw materials in the top-bottom combined blowing converter is as follows: a high-draw supplementary blowing method is used in a 120t top-bottom combined blowing converter to control the oxygen content, and the mass percentage of element C is controlled to be 0.08-0.25%, and the mass percentage of P is controlled to be ≤0.015%. The terminal temperature during smelting in the top-bottom combined blowing converter is controlled to be 1580-1680°C, and the amount of high-carbon ferromanganese added is 9.29kg / t; the top-bottom combined blowing converter is alloyed after the furnace, and the mass percentage of each element is controlled to be C: 0.20-0.27%, Mn: 0.61-0.71%, and Cr: 0.08-0.13%; 101kg / furnace of slag lime, 703kg / furnace of calcium slag balls, and 237kg / furnace of wollastonite are added to the top-bottom combined blowing converter after smelting.
[0045] (2) After smelting, the LF refining furnace is used for refining. During refining, the final slag basicity is 5.6, the white slag retention time is 23 minutes, the argon soft blowing flow rate is 22NL / min, and the soft blowing time is controlled at 27.3 minutes;
[0046] (3) After refining, a continuous casting machine is used to continuously cast 150 mm × 150 mm square billets. During continuous casting, the amount of secondary cooling water is 0.30 L / kg, the argon pressure of the long water inlet of the continuous casting ladle is controlled at 113 mbar, the height of the middle ladle is 430 mm, the continuous casting speed is controlled at 1.9 m / min, the current intensity of the electromagnetic stirring of the crystallizer is controlled at 320 A, and the current frequency is 3.5 Hz;
[0047] (4) After continuous casting, the steel billet is peeled and finished, and then the peeled and finished steel billet is heated; wherein, the specific method of peeling and finishing the steel billet is as follows: the steel billet is fully ground by a fully automatic square billet grinding machine, a grinding wheel of 16 mesh or above is used, the grinding depth of the face is ≥1.0mm, the grinding depth of the corner is ≥7mm, the surface of the grinded steel billet and the joints between the corner and the face should be smooth, without edges or sharp corners, and there should be no burrs adhering to blocks; after grinding, magnetic particle inspection is carried out, and for local defects after grinding, the grinding depth is based on the defect being completely removed; the grinding width shall not be less than 6 times the grinding depth, and the grinding length shall not be less than 10 times the grinding depth. There shall be no un-grinded black edges on the steel billet surface and the continuous casting billet defects that have not been completely removed; during heating, the temperature of the first heating section is controlled at 721°C, the temperature of the second heating section is controlled at 973°C, the temperature of the soaking section is controlled at 1074°C, and the heating time is controlled at 103min.
[0048] (5) After the billet is heated, high-pressure water is used to descale the billet, and the billet after high-pressure water descaling is rolled by a short stress rolling mill and a sizing mill; the pressure during high-pressure water descaling is 29 MPa; the rolling start temperature is controlled at 1020°C, the sizing temperature is 825°C, and the wire laying temperature is 849°C;
[0049] (6) The steel billet after rolling is cooled by Stelmore air cooling line, and the phase change and wire rod passability are controlled by segmented cooling. The air volume of the first three fans during Stelmore air cooling line is 9900m 3 / h, the rear 7 fans are all closed, the front 3 insulation covers are open, and the rear insulation covers are all closed, and the roller speed is 0.24m / s-0.26m / s-0.28m / s-0.30m / s-0.32m / s-0.34m / s-0.36m / s-0.38m / s-0.38m / s-0.38m / s-0.38m / s-0.42m / s-0.44m / s;
[0050] (7) The steel billet after Stelmor air-cooling line controlled cooling is coiled to obtain the annealing-free medium carbon cold heading steel wire rod. The specification of the obtained wire rod is φ10mm, the tensile strength of the hot-rolled wire rod is 569MPa, and the 1 / 2 radius hardness is 78.7HRB.
[0051] Example 3
[0052] The invention discloses an annealing-free medium-carbon cold heading steel wire rod for 10.9-grade bolts. The chemical composition of the wire rod, measured by mass percentage, comprises C: 0.34%, Si: 0.06%, Mn: 0.724%, P: 0.013%, S: 0.006%, Cr: 0.14%, B: 0.0017%, Ti: 0.026%, Al 0.035%, N: 0.0034%, and the rest is Fe and unavoidable impurity elements.
[0053] A method for producing annealing-free medium carbon cold heading steel wire rod for 10.9 grade bolts comprises the following steps:
[0054] (1) A top-bottom combined blowing converter is used to smelt the raw materials, and then lime and wollastonite are added to the smelted slag of the top-bottom combined blowing converter. The specific method of smelting the raw materials in the top-bottom combined blowing converter is as follows: a high-draw supplementary blowing method is used in a 120t top-bottom combined blowing converter to control the oxygen content, and the mass percentage of element C is controlled to be 0.08-0.25%, and the mass percentage of P is controlled to be ≤0.015%. The terminal temperature during smelting in the top-bottom combined blowing converter is controlled to be 1580-1680°C, and the amount of high-carbon ferromanganese added is 9.29kg / t; the top-bottom combined blowing converter is alloyed after the furnace, and the mass percentage of each element is controlled to be C: 0.20-0.27%, Mn: 0.61-0.71%, and Cr: 0.08-0.13%; 101kg / furnace of slag lime, 696kg / furnace of calcium slag balls, and 245kg / furnace of wollastonite are added to the top-bottom combined blowing converter after smelting.
[0055] (2) After smelting, the LF refining furnace is used for refining. During refining, the final slag basicity is 6, the white slag retention time is 28 minutes, the argon soft blowing flow rate is 19NL / min, and the soft blowing time is 17 minutes;
[0056] (3) After refining, a continuous casting machine is used to continuously cast 150 mm × 150 mm square billets. During continuous casting, the amount of secondary cooling water is 0.30 L / kg, the argon pressure of the long water inlet of the continuous casting ladle is 117 mbar, the height of the middle ladle is 420 mm, the continuous casting speed is 1.9 m / min, the current intensity of the electromagnetic stirring of the crystallizer is 320 A, and the current frequency is 3.5 Hz;
[0057] (4) After continuous casting, the steel billet is peeled and finished, and then the peeled and finished steel billet is heated; wherein, the specific method of peeling and finishing the steel billet is as follows: the steel billet is fully ground by a fully automatic square billet grinding machine, a grinding wheel of 16 mesh or above is used, the surface grinding depth is ≥1.0mm, the corner grinding depth is ≥7mm, the surface of the grinded steel billet and the joints between the corners and the surface should be smooth, without edges or sharp corners, and there should be no burrs adhering to blocks. After grinding, magnetic particle inspection is performed. For local defects after grinding, the grinding depth is based on the defect being completely removed; the grinding width shall not be less than 6 times the grinding depth, and the grinding length shall not be less than 10 times the grinding depth. There shall be no un-grinded black edges on the steel billet surface and the continuous casting billet defects that have not been completely removed; during heating, the temperature of the first heating section is controlled at 704°C, the temperature of the second heating section is controlled at 978°C, the temperature of the soaking section is controlled at 1069°C, and the heating time is controlled at 100min.
[0058] (5) After the billet is heated, high-pressure water is used to descale the billet, and the billet after high-pressure water descaling is rolled by a short stress rolling mill and a sizing mill; the pressure during high-pressure water descaling is 30 MPa; the rolling start temperature is controlled at 1015°C, the sizing temperature is 826°C, and the wire laying temperature is 853°C;
[0059] (6) The steel billet after rolling is cooled by Stelmore air cooling line, and the phase change and wire rod passability are controlled by segmented cooling. The air volume of the first three fans during Stelmore air cooling line is 9900m 3 / h, the rear 7 fans are all closed, the front 3 insulation covers are open, and the rear insulation covers are all closed, and the roller speed is 0.24m / s-0.26m / s-0.28m / s-0.30m / s-0.32m / s-0.34m / s-0.36m / s-0.38m / s-0.38m / s-0.38m / s-0.38m / s-0.42m / s-0.44m / s;
[0060] (7) The steel billet after Stelmor air-cooling line controlled cooling is coiled to obtain the annealing-free medium carbon cold heading steel wire rod. The specification of the obtained wire rod is φ12mm, the tensile strength of the hot-rolled wire rod is 570.5MPa, and the 1 / 2 radius hardness is 80.7HRB.
[0061] Example 4
[0062] The invention discloses an annealing-free medium-carbon cold heading steel wire rod for 10.9-grade bolts. The chemical composition of the wire rod, measured by mass percentage, comprises C: 0.323%, Si: 0.05%, Mn: 0.73%, P: 0.009%, S: 0.009%, Cr: 0.12%, B: 0.0023%, Ti: 0.034%, Al 0.029%, N: 0.0044%, and the rest is Fe and unavoidable impurity elements.
[0063] A method for producing annealing-free medium carbon cold heading steel wire rod for 10.9 grade bolts comprises the following steps:
[0064] (1) A top-bottom combined blowing converter is used to smelt the raw materials, and then lime and wollastonite are added to the smelted slag of the top-bottom combined blowing converter. The specific method of smelting the raw materials by the top-bottom combined blowing converter is as follows: a high-draw supplementary blowing method is used in a 120t top-bottom combined blowing converter to control the oxygen content, and the mass percentage of element C is controlled to be 0.08-0.25%, and the mass percentage of P is controlled to be ≤0.015%. The terminal temperature during smelting in the top-bottom combined blowing converter is controlled to be 1580-1680°C, and the amount of high-carbon ferromanganese added is 9.29kg / t; the top-bottom combined blowing converter is alloyed after the furnace, and the mass percentage of each element is controlled to be C: 0.20-0.27%, Mn: 0.61-0.71%, and Cr: 0.08-0.13%; 111kg / furnace of slag lime, 697kg / furnace of calcium slag balls, and 249kg / furnace of wollastonite are added to the top-bottom combined blowing converter after smelting.
[0065] (2) After smelting, the LF refining furnace is used for refining. During refining, the final slag basicity is 4.8, the white slag retention time is 42 minutes, the argon soft blowing flow rate is 20NL / min, and the soft blowing time is 17 minutes;
[0066] (3) After refining, a continuous casting machine is used to continuously cast 150 mm × 150 mm square billets. During continuous casting, the amount of secondary cooling water is 0.30 L / kg, the argon pressure of the long water inlet of the continuous casting ladle is 122 mbar, the height of the middle ladle is 410 mm, the continuous casting speed is 1.9 m / min, the current intensity of the electromagnetic stirring of the crystallizer is 320 A, and the current frequency is 3.5 Hz;
[0067] (4) After continuous casting, the steel billet is peeled and finished, and then the peeled and finished steel billet is heated; wherein, the specific method of peeling and finishing the steel billet is as follows: the steel billet is fully ground by a fully automatic square billet grinding machine, a grinding wheel of 16 mesh or above is used, the surface grinding depth is ≥1.0mm, the corner grinding depth is ≥7mm, the surface of the grinded steel billet and the joints between the corners and the surface should be smooth, without edges or sharp corners, and there should be no burrs adhering to blocks. After grinding, magnetic particle inspection is performed. For local defects after grinding, the grinding depth is based on the defect being completely removed; the grinding width shall not be less than 6 times the grinding depth, and the grinding length shall not be less than 10 times the grinding depth. There shall be no un-grinded black edges on the steel billet surface and the continuous casting billet defects that have not been completely removed; during heating, the temperature of the first heating section is controlled at 716°C, the temperature of the second heating section is controlled at 980°C, the temperature of the soaking section is controlled at 1076°C, and the heating time is controlled at 98min.
[0068] (5) After the billet is heated, high-pressure water is used to descale the billet, and the billet after high-pressure water descaling is rolled by a short stress rolling mill and a sizing mill; the pressure during high-pressure water descaling is 25 MPa; the rolling start temperature is controlled at 1020°C, the sizing temperature is 826°C, and the wire laying temperature is controlled at 860°C;
[0069] (6) The steel billet after rolling is cooled by Stelmore air cooling line, and the phase change and wire rod passability are controlled by segmented cooling. The air volume of the first three fans during Stelmore air cooling line is 9900m 3 / h, the rear 7 fans are all closed, the front 3 insulation covers are open, and the rear insulation covers are all closed, and the roller speed is 0.24m / s-0.26m / s-0.28m / s-0.30m / s-0.32m / s-0.34m / s-0.36m / s-0.38m / s-0.38m / s-0.38m / s-0.38m / s-0.42m / s-0.44m / s;
[0070] (7) The steel billet after Stelmor air-cooling line controlled cooling is coiled to obtain the annealing-free medium carbon cold heading steel wire rod. The specification of the obtained wire rod is φ14mm, the tensile strength of the hot-rolled wire rod is 569MPa, and the hardness at 1 / 2 radius is 80HRB.
[0071] Example 5
[0072] The invention discloses an annealing-free medium-carbon cold heading steel wire rod for 10.9-grade bolts. The chemical composition of the wire rod, measured by mass percentage, comprises C: 0.334%, Si: 0.06%, Mn: 0.724%, P: 0.011%, S: 0.006%, Cr: 0.12%, B: 0.0018%, Ti: 0.030%, Al 0.026%, N: 0.0036%, and the rest is Fe and unavoidable impurity elements.
[0073] A method for producing annealing-free medium carbon cold heading steel wire rod for 10.9 grade bolts comprises the following steps:
[0074] (1) A top-bottom combined blowing converter is used to smelt the raw materials, and then lime and wollastonite are added to the smelted slag of the top-bottom combined blowing converter. The specific method of smelting the raw materials in the top-bottom combined blowing converter is as follows: a high-draw supplementary blowing method is used in a 120t top-bottom combined blowing converter to control the oxygen content, and the mass percentage of element C is controlled to be 0.08-0.25%, and the mass percentage of P is controlled to be ≤0.015%. The terminal temperature during smelting in the top-bottom combined blowing converter is controlled to be 1580-1680°C, and the amount of high-carbon ferromanganese added is 9.29kg / t; the top-bottom combined blowing converter is alloyed after the furnace, and the mass percentage of each element is controlled to be C: 0.20-0.27%, Mn: 0.61-0.71%, and Cr: 0.08-0.13%; 111kg / furnace of slag lime, 699kg / furnace of calcium slag balls, and 249kg / furnace of wollastonite are added to the top-bottom combined blowing converter after smelting.
[0075] (2) After smelting, the LF refining furnace is used for refining. During refining, the final slag basicity is 5.6, the white slag retention time is 16 minutes, the argon soft blowing flow rate is controlled at 21NL / min, and the soft blowing time is controlled at 19 minutes;
[0076] (3) After refining, a continuous casting machine is used to continuously cast 150 mm × 150 mm square billets. During continuous casting, the amount of secondary cooling water is 0.30 L / kg, the argon pressure of the long water inlet of the continuous casting ladle is 120 mbar, the height of the middle ladle is 420 mm, the continuous casting speed is 1.9 m / min, the current intensity of the electromagnetic stirring of the crystallizer is 320 A, and the current frequency is 3.5 Hz;
[0077] (4) After continuous casting, the steel billet is peeled and finished, and then the peeled and finished steel billet is heated; wherein, the specific method of peeling and finishing the steel billet is as follows: the steel billet is fully ground by a fully automatic square billet grinding machine, a grinding wheel of 16 mesh or above is used, the grinding depth of the face is ≥1.0mm, the grinding depth of the corner is ≥7mm, the surface of the grinded steel billet, the joints between the corner and the face should be smooth, without edges or sharp corners, and there should be no burrs adhering to blocks; after grinding, magnetic particle inspection is performed, and for local defects after grinding, the grinding depth is based on the defect being completely removed; the grinding width shall not be less than 6 times the grinding depth, and the grinding length shall not be less than 10 times the grinding depth. There shall be no un-grinded black edges on the steel billet surface and the continuous casting billet defects that have not been completely removed; during heating, the temperature of the first heating section is controlled at 700°C, the temperature of the second heating section is controlled at 978°C, the temperature of the soaking section is controlled at 1077°C, and the heating time is controlled at 96min.
[0078] (5) After the billet is heated, it is descaled by high-pressure water, and the billet after high-pressure water descaling is rolled by a short stress rolling mill and a sizing mill; the pressure during high-pressure water descaling is 27 MPa; the starting rolling temperature is 1010°C, the sizing temperature is 823°C, and the wire drawing temperature is 849°C.
[0079] (6) The steel billet after rolling is cooled by Stelmore air cooling line, and the phase change and wire rod passability are controlled by segmented cooling. The air volume of the first three fans during Stelmore air cooling line is 9900m 3 / h, the rear 7 fans are all closed, the front 3 insulation covers are open, and the rear insulation covers are all closed, and the roller speed is 0.24m / s-0.26m / s-0.28m / s-0.30m / s-0.32m / s-0.34m / s-0.36m / s-0.38m / s-0.38m / s-0.38m / s-0.38m / s-0.42m / s-0.44m / s;
[0080] (7) The steel billet after Stelmor air-cooling line controlled cooling is coiled to obtain the annealing-free medium carbon cold heading steel wire rod. The specification of the obtained wire rod is φ16mm, the tensile strength of the hot-rolled wire rod is 572MPa, and the hardness at 1 / 2 radius is 80.4HRB.
[0081] The temperatures at various stages during the rolling of the steel billets in Examples 1-5 are shown in Table 1.
[0082] Table 1 Temperature of the steel billet at each stage of rolling in Examples 1-5
[0083]
[0084] The sizing temperature in Table 1 is the final rolling temperature. The present invention adopts a low-temperature rolling process, increases the ferrite ratio of the wire rod, reduces the hardness of the wire rod, increases the thickness of the oxide scale after increasing the spinning temperature, and the measured thickness is 0.007 mm higher than the original thickness. The hood entry temperature is reduced, the formation of proeutectoid ferrite is suppressed, and the generation of the full decarburization layer is effectively eliminated.
[0085] The mechanical properties of the finished medium carbon cold heading steel wire rods obtained in Examples 1-5 and the user usage were tested, and the specific results of the tests are shown in Table 2.
[0086] Table 2 Mechanical properties of the finished medium carbon cold heading steel wire rods obtained in Examples 1-5 and user usage
[0087]
[0088]
[0089] It can be seen from the test results in Table 2 that the 10.9 grade bolt annealing-free medium carbon cold heading steel wire rod obtained by the production method of the present invention not only has low hardness, stable tensile strength, and small decarburization, but also achieves annealing-free processing performance after cold heading by customers, while also ensuring good quenching and tempering heat treatment performance and material forming performance. Figure 1-5 As shown, it also reduces production costs for customers.
[0090] Obviously, the above embodiments are only examples for clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from them are still within the protection scope of the invention.
Claims
1. A medium carbon cold heading steel wire rod without annealing for grade 10.9 bolts, characterized in that: The chemical composition of the wire rod, measured in mass percentage, includes: C 0.30-0.36%, Si≤0.10%, Mn 0.60-0.80%, P≤0.015%, S≤0.010%, Cr 0.10-0.30%, B 0.0008-0.0035%, Ti 0.020-0.050%, Al0.020-0.050%, N≤0.0050%, and the rest are Fe and unavoidable impurity elements.
2. The annealing-free medium carbon cold heading steel wire rod for 10.9 grade bolts according to claim 1, characterized in that: The chemical composition of the wire rod, measured in mass percentage, includes: C 0.32%, Si 0.06%, Mn 0.73%, P 0.012%, S 0.008%, Cr 0.13%, B 0.0018%, Ti 0.028%, Al 0.025%, N 0.0036%, and the rest is Fe and unavoidable impurity elements.
3. The method for producing annealing-free medium carbon cold heading steel wire rod for 10.9 grade bolts according to any one of claims 1 or 2, characterized in that: The production method comprises the following steps: (1) using a top-bottom combined blowing converter to smelt the raw materials, and then adding lime, calcium slag balls and wollastonite to the smelted top-bottom combined blowing converter slag; (2) After smelting, refining is carried out in an LF refining furnace; (3) After refining, a continuous casting machine is used to continuously cast 150 mm × 150 mm square billets; (4) After continuous casting, the steel billet is peeled and finished, and then the peeled and finished steel billet is heated; (5) After the billet is heated, it is descaled by high-pressure water, and the billet after high-pressure water descaling is rolled by a short stress rolling mill and a reducing mill; (6) The rolled steel billet is cooled by Stelmor air cooling line, and the phase change and wire rod passability are controlled by segmented cooling; (7) The steel billet after controlled cooling in the Stelmore air-cooling line is coiled to obtain the annealing-free medium carbon cold heading steel wire rod.
4. The method for producing annealing-free medium carbon cold heading steel wire rod for 10.9 grade bolts according to claim 3 is characterized in that: The method for smelting the raw materials in the top and bottom combined blowing converter in the step (1) is as follows: in a 120t top and bottom combined blowing converter, a high-draw supplementary blowing method is used to control the oxygen content, and the mass percentage of the element C is controlled to be 0.08-0.25%, and the mass percentage of P is controlled to be ≤0.015%. The terminal temperature during smelting in the top and bottom combined blowing converter is controlled to be 1580-1680°C, and the amount of high carbon ferromanganese added is 9.29kg / t; the top and bottom combined blowing converter is alloyed after the furnace, and the mass percentage of each element is controlled to be C: 0.20-0.27%, Mn: 0.61-0.71%, and Cr 0.08-0.13%; 100±20kg / furnace of slag lime, 700±30kg / furnace of calcium slag balls, and 250±20kg / furnace of wollastonite are added to the top and bottom combined blowing converter after smelting.
5. The method for producing annealing-free medium carbon cold heading steel wire rod for 10.9 grade bolts according to claim 3, characterized in that: During refining in the step (2), the final slag basicity is controlled at 4.0-6.5, the white slag retention time is controlled at 15-45 min, the argon soft blowing flow rate is controlled at 14-30 NL / min, and the soft blowing time is controlled at 15-40 min.
6. The method for producing annealing-free medium carbon cold heading steel wire rod for 10.9 grade bolts according to claim 3, characterized in that: In the step (3), the amount of secondary cooling water during continuous casting is 0.30 L / kg, the argon pressure at the long water inlet of the continuous casting ladle is controlled at 90-130 mbar, the middle ladle height is ≥400 mm, the continuous casting speed is controlled at 1.8-2.0 m / min, the current intensity of the electromagnetic stirring of the crystallizer is controlled at 330-370 A, and the current frequency is 3.5 Hz.
7. The method for producing annealing-free medium carbon cold heading steel wire rod for 10.9 grade bolts according to claim 3, characterized in that: The specific method for peeling and finishing the steel billet in the step (4) is as follows: a fully automatic square billet grinding machine is used to fully grind the steel billet, a grinding wheel of 16 mesh or above is used, the grinding depth of the face is ≥1.0mm, the grinding depth of the corner is ≥7mm, the surface of the grinded steel billet and the junction between the corner and the face should be smooth, without edges or sharp corners, and there should be no burrs adhering to blocks. After grinding, magnetic particle inspection is carried out. For local defects after grinding, the grinding depth is based on the defect being completely removed; the grinding width shall not be less than 6 times the grinding depth, and the grinding length shall not be less than 10 times the grinding depth. No un-grinded black edges or unremoved continuous casting billet defects shall appear on the steel billet surface; during heating in the step (4), the temperature of the first heating section is controlled at 600-800°C, the temperature of the second heating section is controlled at 950-1010°C, the temperature of the soaking section is controlled at 1060-1100°C, and the heating time is controlled at 80-130min.
8. The method for producing annealing-free medium carbon cold heading steel wire rod for 10.9 grade bolts according to claim 3, characterized in that: The pressure of high-pressure water descaling in step (5) is ≥20MPa; the starting rolling temperature of the rolling is controlled at 930-1030°C, the sizing temperature is controlled at 820-840°C, and the spinning temperature is controlled at 780-860°C.
9. The method for producing annealing-free medium carbon cold heading steel wire rod for 10.9 grade bolts according to claim 3, characterized in that: In step (6), the air volume of the first three fans during the Stelmor air-cooling line control cooling is 9900m 3 / h, the rear 7 fans are all closed, the front 3 insulation covers are open, and the rear ones are all closed, the roller speed is 0.24m / s-0.26m / s-0.28m / s-0.30m / s-0.32 m / s-0.34m / s-0.36m / s-0.38m / s-0.38m / s-0.38m / s-0.38m / s-0.42m / s-0.44m / s.
10. The method for producing annealing-free medium carbon cold heading steel wire rod for 10.9 grade bolts according to claim 3, characterized in that: The specification of the wire rod obtained in the step (7) is φ10-16mm; the tensile strength of the wire rod is ≤600MPa, and the 1 / 2 radius hardness of the wire rod is ≤83HRB.
Citation Information
Cited By
Annealing-free carbon cold heading steel wire rod and production method thereof
CN120485646A