550MPa-grade weather-proof bridge steel with low yield-tensile ratio as well as manufacturing method and application of 550MPa-grade weather-proof bridge steel
By using specific chemical composition and manufacturing processes in weathering bridge steel to form multiphase composite microstructure, the problem of insufficient low temperature and high toughness in high cold environments is solved, and high strength, high toughness and low bending are achieved The strong ratio matches and reduces the sensitivity of welding cracks, meeting the material needs of bridge steel in high-altitude environment.
Patent Information
- Application Number
- CN202410940795.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-15
AI Technical Summary
The existing weather-resistant bridge steel cannot meet the needs of low-temperature and high-toughness materials in high cold environments, and the high carbon content increases welding crack sensitivity and yield strength ratio, and the increased Cr, Ni, Cu, and Mo elements increase cost and increase brittleness.
Using 550MPa grade low yield strength-resistance weathering bridge steel, it adopts specific chemical composition and manufacturing processes, including C: 0.04-0.08%, Si: 0.15-0.55%, Mn: 1.40-1.65%, Cr: 0.35-0.55%, Ni : 0.35-0.60%, Cu: 0.25-0.50%, Mo: ≤0.03% and other elements to form a multiphase composite microstructure of ferrite, bainite, M/A components and MX precipitation phase, and control The yield strength ratio is ≤0.85, elongation is ≥20%, and V-type impact work is ≥220J in -40℃. Combined with the second-stage controlled rolling and cooling technology, the design yield strength is ≥550MPa and the tensile strength is ≥690MPa.
It achieves matching of high strength, high toughness and low yield and strength ratio, reduces welding crack sensitivity, meets the demand for low-temperature and high-toughness materials of high-cold environmental bridge steel, and improves weather resistance and welding performance.
Smart Images

Figure CN118957444A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of steel for bridge structures, and in particular to a 550MPa-grade low-yield-to-strength ratio weather-resistant bridge steel and a manufacturing method and application thereof. Background Art
[0002] Weathering steel is widely used in railway, river-crossing, sea-crossing and other key bridge construction projects. In the face of high-cold environment, extreme weather, earthquake disasters and other service requirements, and in order to meet the characteristics of light, large-span, high-frequency and heavy-load steel bridges, ordinary weathering steel cannot meet the material requirements.
[0003] Existing weather-resistant bridge steels are mainly made by increasing the carbon content and adding elements such as Cr, Ni, Cu, and Mo. As the carbon content increases, the strength of weather-resistant bridge steel can be improved. However, a higher carbon content will significantly increase the welding crack sensitivity index of weather-resistant bridge steel, which is not conducive to welding. At the same time, it has a higher yield strength ratio. In addition, adding Cr, Ni, and Cu improves the weather resistance of steel plates. However, higher Cr, Ni, Cu, and Mo increase the cost of steel plates. Improper addition of Cr will increase the brittleness of steel, making the -40℃ V-type impact energy of bridge steel less than 120J, which cannot meet the demand for low-temperature and high-toughness materials for bridge steel in high-cold environments. Summary of the invention
[0004] In response to the above technical problems, the present invention provides a 550MPa-grade low yield ratio weather-resistant bridge steel and its manufacturing method and application to meet the demand for low-temperature and high-toughness materials for bridge steel in high-cold environments, thereby achieving a match between high strength, high toughness and low yield ratio. The obtained weather-resistant bridge steel has a yield strength of ≥550MPa, a tensile strength of ≥690MPa, a yield ratio of ≤0.85, an elongation of ≥20%, and a -40°C V-type impact energy of ≥220J, thereby meeting the demand for low-temperature and high-toughness materials for bridge steel in high-cold environments.
[0005] In the first aspect, the present invention provides a 550MPa grade low yield ratio weathering bridge steel, which includes the following chemical components, measured by mass percentage: C: 0.04-0.08%, Si: 0.15-0.55%, Mn: 1.40-1.65%, Cr: 0.35-0.55%, Ni: 0.35-0.60%, Cu: 0.25-0.50%, Mo: ≤0.03%, Nb: 0.025-0.045%, V: 0.020-0.040, Ti: 0.012-0.020%, Al: 0.015-0.045%, P≤0.015%, S≤0.005%, N≤0.005%, O≤0.005%, and the rest is Fe and unavoidable impurities.
[0006] Furthermore, the weather-resistant bridge steel has a multiphase composite microstructure of ferrite, bainite, M / A components and MX precipitated phases, wherein the bainite structure has a good match between strength and toughness. When the bridge steel matrix structure is mainly bainite (volume fraction is 80-90%), higher strength and low-temperature toughness can be obtained. In addition to the bainite structure, the bridge steel microstructure also contains ferrite. A small amount of ferrite in the bridge steel can reduce the yield strength ratio of the steel and improve the plasticity of the high-strength bridge steel.
[0007] Furthermore, in the microstructure, the volume fraction of ferrite is 6%-10%, and the volume fraction of bainite is 80%-90%.
[0008] Furthermore, the average grain size of the weather-resistant bridge steel is ≤7.0 μm.
[0009] Further, the particle size of the MX precipitated phase is ≤300nm, and the proportion of the MX precipitated phase with a particle size of 30-120nm is ≥75%. It should be noted that the purpose of introducing the MX precipitated phase is to compensate for the strength loss caused by the ferrite soft phase by the precipitation strengthening effect of fine particles without reducing toughness. The second phase strengthening mechanism in the present invention is mainly the Orowan mechanism, that is, the second phase strengthening effect is inversely proportional to the size of the second phase particles, and the smaller the particle size, the greater the strengthening effect. Therefore, in the present invention, the particle size distribution of the MX precipitated phase is controlled to be ≤300nm, and the MX precipitated phase with a particle size of 30-120nm accounts for ≥75%.
[0010] Furthermore, the weather resistance index I of the weather-resistant bridge steel is greater than 6.5, and the welding crack sensitivity index Pcm is less than or equal to 0.22%.
[0011] Furthermore, the yield strength of the weather-resistant bridge steel is ≥550MPa, the tensile strength is ≥690MPa, the yield strength ratio is ≤0.85, the elongation is ≥20%, the -40°C V-type impact energy is ≥220J, and the cross-sectional fiber rate is ≥80%.
[0012] In a second aspect, the present invention provides a method for manufacturing 550MPa grade low yield strength ratio weathering bridge steel, which is applied to the weathering bridge steel described in any one of the schemes in the first aspect, comprising the following steps:
[0013] Smelting: according to the chemical composition, materials are prepared, smelted in converter, refined outside the furnace, and continuously cast to obtain 220mm / 370mm thick continuous casting slabs or continuous casting slabs of other thickness specifications;
[0014] Controlled rolling: the continuous casting slab is subjected to two-stage controlled rolling, and then controlled cooling, the total reduction ratio of the two-stage rolling of rough rolling and finishing rolling is 6.1-18.3, the starting rolling temperature of rough rolling is ≥1050°C, and the reduction rate is 60-70% of the total deformation; the starting rolling temperature of finishing rolling is 890-970°C, the final rolling temperature of finishing rolling is 820±20°C, and the reduction rate is 30-40% of the total deformation;
[0015] Controlled cooling: Cooling is carried out in two stages. In the first stage, the water temperature of the steel plate is controlled at 730-790℃ to generate a small amount of ferrite in the steel plate. At the same time, laminar cooling is adopted with a cooling rate of 15-20℃ / s to make the steel plate quickly enter the medium temperature transformation zone and undergo phase transformation at a lower temperature. The second stage is air cooling with a cooling rate of 7-15℃ / s and a red-return temperature of 530-620℃. The first stage adopts the method of low water entry + rapid cooling, the purpose of which is to make the steel plate generate a small amount of soft phase ferrite after rolling and then quickly enter the bainite phase transformation temperature zone to obtain a large amount of bainite structure. A slower cooling rate is designed in the second stage to reduce the high internal stress caused by rapid cooling.
[0016] The weather-resistant bridge steel is obtained by performing heat treatment after controlled cooling.
[0017] It should be noted that the starting rolling temperature of the rough rolling is controlled at above 1050°C to ensure rolling in the austenite recrystallization zone, which can fully recrystallize the austenite. After repeated rolling and recrystallization, the austenite grains are refined. The reduction rate is 70% of the total deformation. Under the action of high temperature and large reduction rate, the austenite grains are fully refined to improve strength and toughness. The finishing rolling temperature is controlled at 890-970°C to ensure rolling in the austenite non-recrystallization zone temperature, which can flatten the austenite grains, and a large number of deformation substructures are accumulated inside the austenite grains, which increases the number of nuclei of the supercooled austenite phase transformation, so as to obtain a fine organizational structure during the cooling process after rolling.
[0018] Furthermore, before the two-stage rolling, the continuous casting slab is heated, the continuous casting slab rolling heating temperature is 1180-1220°C, and the holding time is 2-3h. The heat treatment includes tempering, specifically, reheating the rolled slab after controlled cooling to 500-650°C, holding for 30-40min, and air cooling to room temperature after being taken out of the furnace.
[0019] When the red-returning temperature is low (530℃), the matrix structure is mainly lath-shaped bainite. This type of structure has high strength and meets the strength requirements of 550MPa yield strength grade bridge steel. A lower tempering temperature (500-550℃) is designed. The main purpose is to release the stress of rolled weather-resistant bridge steel plate and increase the service life of the steel plate; the second is to reduce the dislocation density, thereby improving the low-temperature impact toughness of weather-resistant bridge steel.
[0020] When the tempering temperature is high (620℃), the matrix structure is mainly lath-shaped bainite + a small amount of granular bainite. A higher tempering temperature (550-650℃) is designed. On the one hand, the amount of second phase precipitation increases, which can significantly improve the strength level of bridge steel; on the other hand, tempering treatment is conducive to the improvement of plasticity and toughness. When the tempering temperature is higher than 650℃, the second phase precipitation particles grow rapidly, which on the one hand reduces the plasticity and toughness of the steel, and on the other hand increases the yield strength ratio of the steel, affecting the safe service of the bridge steel plate.
[0021] Before the two-stage rolling, the continuous casting slab needs to be heated. The heating temperature for rolling the continuous casting slab is 1180-1220℃, and the holding time is 2-3h. On the one hand, it improves the plasticity of the steel, reduces the deformation resistance, and is conducive to the subsequent rolling; on the other hand, it makes the austenite grain size more uniform, and the micro-alloying elements such as Nb are fully dissolved, which is conducive to the regulation of organizational properties. When the heating temperature is lower than 1180℃, the degree of homogenization of the billet is slightly poor; when the heating temperature is higher than 1220℃, it will cause the original austenite grain size to grow abnormally, the austenite grains to coarsen, and the performance of the weather-resistant bridge steel to deteriorate.
[0022] In the third aspect, the present invention also provides an application of weather-resistant bridge steel as structural steel in bridges, wherein the weather-resistant bridge steel is specifically the 550MPa grade low yield ratio weather-resistant bridge steel described in any one of the first aspects or is obtained according to the manufacturing method described in any one of the second aspects.
[0023] The beneficial effects of the present invention are:
[0024] (1) The 550MPa-grade low-yield-to-strength ratio weather-resistant bridge steel provided by the present invention and its manufacturing method and application adopt a composite phase structure component design. Under the premise of ensuring the toughness, plasticity and strength of the bridge steel through low water entry + rapid cooling technology, the steel plate has a lower yield ratio, achieving the matching of high strength, high toughness and low yield ratio. The obtained weather-resistant bridge steel has a yield strength of ≥550MPa, a tensile strength of ≥690MPa, a yield ratio of ≤0.85, an elongation of ≥20%, and a -40℃ V-type impact energy of ≥220J, which meets the demand for low-temperature and high-toughness materials for bridge steel in high-cold environments;
[0025] (2) The ultra-low carbon component design of the present invention has a welding crack sensitivity index Pcm≤0.22%. While the weather resistance index is relatively high (I>6.5), low welding crack sensitivity is ensured, thus realizing the design of highly weather-resistant and easy-to-weld bridge steel materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is the metallographic structure diagram of the weather-resistant bridge steel in Example 3 of the present invention. DETAILED DESCRIPTION
[0027] As one of the optional embodiments of the present invention, 550MPa grade low yield ratio weathering bridge steel includes the following chemical components, measured in mass percentage: C: 0.04-0.08%, Si: 0.15-0.55%, Mn: 1.40-1.65%, Cr: 0.35-0.55%, Ni: 0.35-0.60%, Cu: 0.25-0.50%, Mo: ≤0.03%, Nb: 0.025-0.045%, V: 0.020-0.040, Ti: 0.012-0.020%, Al: 0.015-0.045%, P≤0.015%, S≤0.005%, N≤0.005%, O≤0.005%, and the rest is Fe and unavoidable impurities. The microstructure of the weather-resistant bridge steel includes ferrite, bainite, M / A components and MX precipitation phases, wherein the volume fraction of ferrite in the microstructure is 6-10%, and the volume fraction of bainite is 80%-90%.
[0028] Compared with the prior art, the microstructure of the weather-resistant bridge steel in this embodiment is composed of ferrite, bainite, M / A components (martensite / austenite components) and MX precipitation phases, which ensures the strength and toughness of the bridge steel while making the steel plate have a lower yield ratio; and the weather-resistant bridge steel adopts a lower carbon content, and at the same time adds elements such as Cr, Ni, Cu and Mo, which ensures that the weather resistance index I of the weather-resistant bridge steel is greater than 6.5, and the welding crack sensitivity index Pcm≤0.22%, so that it has higher weather resistance and welding performance, and can be used as structural steel in bridges.
[0029] The functions and proportions of the various elements in the embodiment of the present invention are as follows:
[0030] C: An important strengthening element in steel, which can ensure the toughness, plasticity, strength and weldability of bridge steel. However, when the carbon content is too high, the toughness and plasticity of bridge steel decrease, and the welding performance of steel deteriorates, affecting the safety of bridge steel. Therefore, the carbon content of the present invention is in the range of 0.04-0.08wt%.
[0031] Si: The addition of silicon can remove part of the oxygen during the smelting process, improve or enhance the corrosion resistance of bridge steel, and thus ensure that the bridge steel has high weather resistance. However, too high Si content will deteriorate the welding performance of bridge steel and reduce the safety factor of bridge steel. The silicon content of the present invention is in the range of 0.15-0.55wt%.
[0032] Mn: The addition of manganese effectively delays the ferrite and pearlite phase transformation, which is beneficial to obtain bainite structure in bridge steel. However, too high manganese content causes central segregation problems, which easily forms banded structure in bridge steel, affecting the strength, toughness and corrosion resistance of bridge steel. Therefore, the manganese content of the present invention is in the range of 1.40-1.65wt%.
[0033] Cr: On the one hand, chromium can improve the hardenability of bridge steel and improve the strength of steel through solid solution strengthening; on the other hand, chromium and iron can easily form a dense iron-chromium oxide rust layer, which significantly improves the corrosion resistance of bridge steel. However, too high chromium content will reduce the metallurgical quality of the weld and deteriorate the welding performance of chromium. The chromium content of the present invention is in the range of 0.35-0.55wt%.
[0034] Ni: Nickel can improve the toughness and plasticity of bridge steel and enhance the corrosion resistance of bridge steel. However, Ni is a precious metal and too high a Ni content will significantly increase production costs. Therefore, the nickel content of the present invention is in the range of 0.35-0.60wt%.
[0035] Cu: Copper can significantly improve the corrosion resistance of bridge steel, thereby improving the weather resistance of bridge steel and extending the service life of bridge steel. However, when the Cu content is too high, copper brittle defects are easily generated on the surface of bridge steel, which damages the surface quality and becomes a breakthrough for corrosion, reducing the safety of bridge steel. The copper content of the present invention is in the range of 0.25-0.50wt%.
[0036] Mo: Molybdenum effectively delays the phase transformation of ferrite and pearlite, promotes the phase transformation of bainite, and increases the amount of bainite in bridge steel. Mo can also improve the compactness of the rust layer, thereby improving the corrosion resistance of bridge steel. However, molybdenum is expensive, and excessive addition increases production costs. The range of the molybdenum content of the present invention is ≤0.03wt%.
[0037] Nb: Nb is added to bridge steel to refine the grains. On the other hand, the precipitation of Nbnm phase during tempering significantly improves the strength of bridge steel. The niobium content of the present invention is in the range of 0.025-0.045wt%.
[0038] Ti: Adding trace titanium to bridge steel can easily form small and stable Ti-containing particles, which effectively inhibits the growth of austenite grains during the reheating process of bridge steel. The titanium content of the present invention ranges from 0.012 to 0.020 wt%.
[0039] Al: Aluminum is a strong deoxidizing element. Trace amounts of aluminum can effectively reduce the inclusion content in steel. When the aluminum content is too high, it will lead to an increase in aluminum oxide inclusions, which will reduce the purity of the steel. The present invention controls the aluminum content to 0.015-0.045wt%.
[0040] Specifically, the volume fraction of ferrite in the microstructure is 6-10%, and the volume fraction of bainite is 80-90%. It should be noted that the bainite structure has a good match between strength and toughness. When the matrix structure of the bridge steel is mainly bainite (volume fraction is 80-90%), higher strength and low-temperature toughness can be obtained. In addition to the bainite structure, the bridge steel microstructure also contains ferrite. A small amount of ferrite in the bridge steel can reduce the yield strength ratio of the steel and improve the plasticity of the high-strength bridge steel.
[0041] It should be noted that the purpose of introducing the MX precipitate phase is to compensate for the strength loss caused by the ferrite soft phase by the precipitation strengthening effect of fine particles without reducing toughness. The second phase strengthening mechanism in the present invention is mainly the Orowan mechanism, that is, the second phase strengthening effect is inversely proportional to the size of the second phase particles, and the smaller the particle size, the greater the strengthening effect. Therefore, in the present invention, the particle size distribution of the MX precipitate phase is controlled to be ≤300nm, and the MX precipitate phase with a phase particle size of 30-120nm accounts for ≥75%.
[0042] Specifically, the weathering index I of the weather-resistant bridge steel is greater than 6.5, and the welding crack sensitivity index Pcm is less than or equal to 0.22%. It should be noted that alloy elements play an important role in the corrosion resistance of weather-resistant bridge steel, and the weathering index is a comprehensive evaluation index for the service of weather-resistant bridge steel in different environments. When the weathering index I of weather-resistant bridge steel is less than 6.5, it cannot meet the corrosion resistance requirements of high-performance bridge steel, especially in weather-resistant bridge steel with a yield strength of 550MPa, which cannot serve for a long time in a complex environment of high cold.
[0043] At present, most welding research uses Pcm to evaluate the cold crack sensitivity of low-alloy high-strength steel welding. When the welding crack sensitivity index Pcm (%) of weather-resistant bridge steel is greater than 0.22, it is easy to cause cold cracks and hot cracking problems caused by impurity segregation. The low-temperature toughness of the welding heat-affected zone is significantly deteriorated, reducing the safety factor of weather-resistant bridge steel.
[0044] Based on one of the optional embodiments of the present invention, the manufacturing method of 550MPa grade low yield ratio weathering bridge steel comprises the following steps:
[0045] Step 1: Smelting: batching according to chemical composition, converter smelting, refining outside the furnace, continuous casting, and obtaining 370mm thick continuous casting slab;
[0046] Step 2: subjecting the continuous casting slab to two-stage controlled rolling and then controlled cooling; the total reduction ratio of the two-stage rolling of rough rolling and finishing rolling is 6.1-18.3: the starting rolling temperature of rough rolling is ≥1050°C, and the reduction rate is 60-70% of the total deformation; the starting rolling temperature of finishing rolling is 890-970°C, the final rolling temperature of finishing rolling is 820±20°C, and the reduction rate is 30-40% of the total deformation;
[0047] Step 3: Control the cooling of the steel plate and use two stages for cooling; in the first stage, the water inlet temperature of the steel plate is controlled (730-790℃) to generate a small amount of ferrite in the steel plate, while laminar cooling is used with a cooling rate of 15-20℃ / s to allow the steel plate to quickly enter the medium temperature transformation zone and undergo phase change at a lower temperature; the second stage of cooling is air cooling with a cooling rate of 7-15℃ / s and a red-return temperature of 530-620℃.
[0048] Step 4: heat-treating the rolled billet to obtain weather-resistant bridge steel.
[0049] It should be noted that the starting rolling temperature of the rough rolling is controlled above 1050℃ to ensure rolling in the austenite recrystallization zone, which can fully recrystallize the austenite. After repeated rolling and recrystallization, the austenite grains are refined. The reduction rate is 70% of the total deformation. Under the action of high temperature and large reduction rate, the austenite grains are fully refined and the strength and toughness are improved.
[0050] The finishing rolling temperature is controlled at 890-970℃ to ensure that the rolling is carried out at the temperature of the non-recrystallization zone of austenite, which can flatten the austenite grains and accumulate a large number of deformation substructures inside the austenite grains, thereby increasing the number of nuclei for the supercooled austenite phase transformation, so as to obtain a fine microstructure during the cooling process after rolling.
[0051] Specifically, the continuous casting slab rolling heating temperature is 1180-1220℃, and the holding time is 2-3h. It should be noted that before the two-stage rolling, the continuous casting slab needs to be heated. On the one hand, it improves the plasticity of the steel, reduces the deformation resistance, and is conducive to the subsequent rolling; on the other hand, it makes the austenite grain size more uniform, and micro-alloy elements such as Nb are fully dissolved, which is conducive to the regulation of organizational properties. When the heating temperature is lower than 1180℃, the degree of homogenization of the billet is slightly poor; when the heating temperature is higher than 1220℃, it will cause the original austenite grain size to grow abnormally, the austenite grains to coarsen, and the performance of weather-resistant bridge steel to deteriorate.
[0052] Specifically, in step 3, the cooling of the steel plate is controlled and cooled in two stages; in the first stage, the water inlet temperature of the steel plate is controlled (730-790°C) to generate a small amount of ferrite in the steel plate, while laminar cooling is adopted with a cooling rate of 15-20°C / s to allow the steel plate to quickly enter the medium temperature transformation zone and undergo phase change at a lower temperature; in the second stage, air cooling is used with a cooling rate of 7-15°C / s and a red-return temperature of 530-620°C.
[0053] It should be noted that the first stage adopts the method of low water entry + rapid cooling, the purpose of which is to make the steel plate generate a small amount of soft phase ferrite and then quickly enter the bainite phase transformation temperature zone to obtain a large amount of bainite structure. The second stage is designed with a slower cooling speed, on the one hand, to reduce the high internal stress caused by rapid cooling.
[0054] Specifically, when the red-returning temperature is 530-620℃, the tempering heating temperature is 500-650℃. When the red-returning temperature is low (530℃), the matrix structure is mainly lath-shaped bainite. This type of structure has high strength and meets the strength requirements of 550MPa-grade bridge steel with yield strength. The main purpose of designing a lower tempering temperature (500-550℃) is to release the stress of the rolled weather-resistant bridge steel plate and increase the service life of the steel plate; the second is to reduce the dislocation density, thereby improving the low-temperature impact toughness of the weather-resistant bridge steel. When the red-returning temperature is high (620℃), the matrix structure is mainly lath-shaped bainite + a small amount of granular bainite. The design of a higher tempering temperature (550-650℃) can increase the amount of second phase precipitation on the one hand, which can significantly improve the strength level of the bridge steel; on the other hand, the tempering treatment is conducive to the improvement of plasticity and toughness. When the tempering temperature is higher than 650℃, the second phase precipitated particles grow rapidly, which on the one hand reduces the plasticity and toughness of the steel, and on the other hand increases the yield strength ratio of the steel, affecting the safe service of the bridge steel plate.
[0055] The following will be verified and explained through specific examples. The chemical composition, process parameters and performance of Examples 1-5 are shown in Tables 1, 2 and 3 below.
[0056] Table 1 Chemical composition of the examples (wt.%)
[0057]
[0058] Table 2 Specific process parameters of the embodiment
[0059]
[0060] Table 3 Performance of the embodiment
[0061]
[0062] In the present invention Figure 1 It is the metallographic structure diagram of 40mm thick steel plate, the microstructure type of the steel plate is "bainite + ferrite" structure. Referring to the performance parameters of each embodiment in Table 3, it can be seen that the Q550qENH bridge steel plate produced by the present invention has excellent longitudinal tensile and transverse impact properties, the yield strength is greater than 550MPa, the tensile strength is greater than 690MPa, the yield strength ratio is ≤0.85, the elongation is ≥20%, the -40℃ V-type impact energy is greater than 220J, and the impact fiber section rate is ≥80%, which fully meets the demand for low-temperature and high-toughness materials for bridge steel in high-cold environments.
[0063] In addition to the above embodiments, the present invention may also have other implementation modes. Any technical solution formed by equivalent replacement or equivalent transformation falls within the protection scope required by the present invention.
Claims
1. A 550MPa grade low yield strength ratio weathering bridge steel, characterized in that: Measured in mass percentage, it includes the following chemical components: C: 0.04-0.08%, Si: 0.15-0.55%, Mn: 1.40-1.65%, Cr: 0.35-0.55%, Ni: 0.35-0.60%, Cu: 0.25-0.50%, Mo: ≤0.03%, Nb: 0.025-0.045%, V: 0.020-0.040, Ti: 0.012-0.020%, Al: 0.015-0.045%, P≤0.015%, S≤0.005%, N≤0.005%, O≤0.005%, and the rest are Fe and unavoidable impurities.
2. The 550MPa grade low yield strength ratio weathering bridge steel according to claim 1 is characterized in that: The weather-resistant bridge steel has a microstructure of ferrite, bainite, M / A components and MX precipitation phase.
3. The 550MPa grade low yield strength ratio weathering bridge steel according to claim 2 is characterized in that: In the microstructure, the volume fraction of ferrite is 6%-10%, and the volume fraction of bainite is 80%-90%.
4. The 550MPa grade low yield strength ratio weathering bridge steel according to claim 2 is characterized in that: The average grain size of the weather-resistant bridge steel is ≤7.0 μm.
5. The 550MPa grade low yield strength ratio weathering bridge steel according to claim 2 is characterized in that: The particle size of the MX precipitated phase is ≤300 nm, and the MX precipitated phase with a particle size of 30-120 nm accounts for ≥75%.
6. The 550MPa grade low yield strength ratio weathering bridge steel according to claim 1, characterized in that: The weather resistance index I of the weather resistant bridge steel is greater than 6.5, and the welding crack sensitivity index Pcm is less than or equal to 0.22%.
7. The 550MPa grade low yield strength ratio weathering bridge steel according to claim 1 is characterized in that: The weather-resistant bridge steel has a yield strength of ≥550MPa, a tensile strength of ≥690MPa, a yield strength ratio of ≤0.85, an elongation of ≥20%, a -40°C V-type impact energy of ≥220J, and a cross-sectional fiber rate of ≥80%.
8. A method for manufacturing 550MPa grade low yield strength ratio weathering bridge steel, characterized in that: The weather-resistant bridge steel used in any one of claims 1 to 7 comprises the following steps: Smelting: batching according to chemical composition, converter smelting, refining outside the furnace, continuous casting to obtain continuous casting slab; Controlled rolling: the continuous casting slab is subjected to two-stage controlled rolling, and then controlled cooling, the total reduction ratio of the two-stage rolling of rough rolling and finishing rolling is 6.1-18.3, the starting rolling temperature of rough rolling is ≥1050°C, and the reduction rate is 60-70% of the total deformation; the starting rolling temperature of finishing rolling is 890-970°C, the final rolling temperature of finishing rolling is 820±20°C, and the reduction rate is 30-40% of the total deformation; Controlled cooling: Two stages of cooling are used. In the first stage, the water temperature of the steel plate is controlled at 730-790℃, so that a small amount of ferrite is generated in the steel plate. At the same time, laminar cooling is used with a cooling rate of 15-20℃ / s, so that the steel plate quickly enters the medium temperature transformation zone and undergoes phase change at a lower temperature. The second stage of cooling is air cooling with a cooling rate of 7-15℃ / s and a red-return temperature of 530-620℃. The weather-resistant bridge steel is obtained by performing heat treatment after controlled cooling.
9. The manufacturing method according to claim 8, characterized in that: Before two-stage rolling, the continuous casting slab is heated, the continuous casting slab rolling heating temperature is 1180-1220°C, and the holding time is 2-3h. The heat treatment includes tempering, specifically, the rolled slab after controlled cooling is reheated to 500-650°C, kept for 30-40min, and air-cooled to room temperature after being taken out of the furnace.
10. Use of a 550MPa grade low yield strength ratio weathering bridge steel as described in any one of claims 1 to 7 or a weathering bridge steel obtained by the manufacturing method as described in any one of claims 8 to 9 as structural steel in bridges.