Soft metal doped tungsten disulfide-based composite film and preparation method and application thereof
By introducing titanium and copper into the molybdenum disulfide film, forming a titanium/tungsten disulfide/nickel/copper gradient layer and a tungsten disulfide/nickel/copper layer, the friction of the molybdenum disulfide coating in high temperature and high load environments is solved. Poor performance problems, high hardness and good friction and wear performance are achieved, and are suitable for protection and long-life applications of space devices.
Patent Information
- Application Number
- CN202411025844.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-29
AI Technical Summary
Existing molybdenum disulfide (MoS2) coatings have poor friction performance in high and low temperatures, high loads and high radiation environments, and a single solid film is difficult to meet the growing demand for durability and high torque sensitivity applications.
Magneto-controlled sputtering technology is used to deposit titanium transition layer, titanium/tungsten disulfide/nickel/copper gradient layer and tungsten disulfide/nickel/copper layer on the substrate surface in sequence to form a composite film with soft metal doped tungsten disulfide group. The doping modification design of Ni and Cu improves the hardness and environmental adaptability of the film.
It achieves high hardness, good friction and wear performance and temperature adaptability, the binding force reaches 20N, and the friction coefficient is reduced in high temperature environment. It is suitable for protection of space devices and extends the service life of aerospace vehicles.
Smart Images

Figure CN118957495A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of surface treatment, and in particular relates to a soft metal-doped tungsten disulfide-based composite film and a preparation method and application thereof. Background Art
[0002] Spacecraft often work under special working conditions, such as high / low temperature or high load, so it is necessary to improve the life and reliability of rotating parts such as bearings to ensure the safe operation of spacecraft, among which ensuring the lubrication of rotating parts is the key. Transition metal sulfides (MS2, M is molybdenum or tungsten) are widely used in the aerospace field because of their interlayer weak van der Waals bonds to form a layered structure that is easy to slide. However, sometimes ground testing or storage must be carried out before the launch of the spacecraft. Since MS2 solid lubricating coatings are very sensitive to the environment, there are dangling bonds or unsaturated bonds on the edge surface of its layered structure, which easily reacts with oxygen to cause the tribological properties to deteriorate, thus greatly limiting its engineering application. Even in a vacuum, sputtered pure MS2 films show poor wear resistance due to their porous structure. Nowadays, the rapid development of space technology has put forward higher requirements for lubricating materials, requiring them to have good applications in harsh environments such as high and low temperature cycles, high loads, and high radiation. Therefore, it is necessary to improve the friction performance of MS2 coatings.
[0003] For ground or high-temperature applications, MoS2 quickly loses its lubricity and is accompanied by high wear. Therefore, other materials need to be applied to improve the friction performance of the coating in harsh environments. Among them, WS2 has higher thermal stability and oxidation resistance than MoS2. The layered coating prepared on this basis can effectively reduce the friction and wear of rotating parts such as bearings in harsh environments. However, WS2-based coatings cannot replenish themselves like liquid lubricants, especially under harsh operating conditions. Durability issues hinder their use in longer service life and higher torque sensitivity applications, such as rolling element precision bearings. This means that a single solid film is difficult to meet the growing durability requirements. Summary of the invention
[0004] The main purpose of the present invention is to provide a soft metal doped tungsten disulfide-based composite film and its preparation method and application, so as to overcome the shortcomings of the prior art.
[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0006] The embodiment of the present invention provides a soft metal-doped tungsten disulfide-based composite film, which includes: a titanium transition layer, a titanium / tungsten disulfide / nickel / copper gradient layer and a tungsten disulfide / nickel / copper layer sequentially formed on the surface of a substrate;
[0007] Among them, in the direction gradually away from the substrate, the titanium content in the titanium / tungsten disulfide / nickel / copper gradient layer gradually decreases, the molybdenum disulfide content gradually increases, the nickel content gradually increases, and the copper content gradually increases; at the same time, the tungsten disulfide / nickel / copper layer is formed by alternatingly stacking nickel-tungsten disulfide layers and copper-tungsten disulfide layers.
[0008] The embodiment of the present invention further provides a method for preparing the aforementioned soft metal-doped tungsten disulfide-based composite film, which comprises:
[0009] A titanium transition layer, a titanium / tungsten disulfide / nickel / copper gradient layer and a tungsten disulfide / nickel / copper layer are sequentially deposited on the substrate surface by magnetron sputtering technology to obtain a soft metal-doped tungsten disulfide-based composite film.
[0010] The embodiment of the present invention also provides the use of the aforementioned soft metal-doped tungsten disulfide-based composite film in the field of surface protection of aerospace devices in high temperature environments or high and low temperature alternating environments.
[0011] The embodiment of the present invention further provides a device, comprising a substrate, on which the aforementioned soft metal-doped tungsten disulfide-based composite film is also disposed.
[0012] Compared with the prior art, the present invention has the following beneficial effects:
[0013] The present invention adopts magnetron sputtering technology and obtains a soft metal-doped tungsten disulfide-based composite film through Ni and Cu doping modification design. The composite film has high hardness (greater than 6.5GPa) and elastic modulus, and can be suitable for surface protection of components in high-impact environments, especially for surface protection of components in aerospace pyrotechnic separation environments. The strong bonding force reaches 20N, and the environmental friction coefficient reaches 0.04 after high-temperature treatment. It has good friction and wear performance in atmospheric environment, high and low temperature alternating environment and different temperature environments, can meet the use requirements of various environmental components, has good temperature adaptability and high temperature oxidation resistance, and improves the service life of aerospace vehicles. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0015] Figure 1 is a cross-sectional SEM image of the tungsten disulfide-based doped soft metal composite film prepared in Example 3 of the present invention;
[0016] Figure 2This is a bonding strength test diagram of the tungsten disulfide-based doped soft metal composite film prepared in Example 3 of the present invention;
[0017] Figure 3 is a graph of hardness and elastic modulus of a tungsten disulfide-based doped soft metal composite film prepared in Example 3 of the present invention;
[0018] Figure 4 It is a friction curve diagram of the tungsten disulfide-based doped soft metal composite film prepared in Example 3 of the present invention at room temperature, after high temperature annealing at 600° C., and after thermal vacuum testing;
[0019] Figure 5 This is a wear rate diagram of the tungsten disulfide-based doped soft metal composite film prepared in Example 3 of the present invention at room temperature, after high-temperature annealing at 600°C, and after thermal vacuum testing. DETAILED DESCRIPTION
[0020] At present, improving the load-bearing capacity and environmental adaptability of the film by doping is a common means to achieve its practical application. Soft metal doping can significantly improve the mechanical properties and lubrication properties of the film. Since metal elements can undergo tribochemical reactions on the friction surface under high temperature conditions to improve friction and wear performance, metal elements can preferentially interact with O2, protecting the structure of the WS2 film from being destroyed, and can effectively improve the environmental adaptability of the film. However, the doped film performance obtained by co-doping tungsten disulfide with soft metals cannot achieve high hardness and ultra-low friction. Therefore, the present application prepares WS2-based nanocomposite films doped with high-hardness soft metals Ni and Cu by reactive magnetron sputtering, which can achieve high hardness, high load-bearing and excellent high temperature and high and low temperature alternating environmental adaptability.
[0021] In view of the defects of the prior art, the inventors of this case, after long-term research and extensive practice, were able to propose the technical solution of the present invention, which mainly uses unbalanced magnetron sputtering technology to introduce titanium and tungsten carbide into molybdenum disulfide, so that this type of composite coating can achieve ultra-low friction and wear in a vacuum environment and have good oxidation resistance.
[0022] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Specifically, as one aspect of the technical solution of the present invention, a soft metal-doped tungsten disulfide-based composite film includes: a titanium transition layer, a titanium / tungsten disulfide / nickel / copper gradient layer and a tungsten disulfide / nickel / copper layer sequentially formed on the surface of a substrate;
[0024] Among them, in the direction gradually away from the substrate, the titanium content in the titanium / tungsten disulfide / nickel / copper gradient layer gradually decreases, the molybdenum disulfide content gradually increases, the nickel content gradually increases, and the copper content gradually increases; at the same time, the tungsten disulfide / nickel / copper layer is formed by alternatingly stacking nickel-tungsten disulfide layers and copper-tungsten disulfide layers.
[0025] In the present invention, when preparing the tungsten disulfide / nickel / copper layer, due to different rotation speeds during the preparation process, the target positions are placed opposite each other, and a thin layer is deposited at different target positions to form a nano multi-layer alternating deposition.
[0026] In some preferred embodiments, the atomic content of nickel atoms in the soft metal-doped tungsten disulfide-based composite film is 8 to 12 at%, and the atomic content of copper atoms is 1 to 4 at%.
[0027] In some preferred embodiments, the thickness of the titanium transition layer is 100-200 nm.
[0028] In some preferred embodiments, the thickness of the titanium / tungsten disulfide / nickel / copper gradient layer is 100-300 nm.
[0029] In some preferred embodiments, the thickness of the tungsten disulfide / nickel / copper layer is 1.5-2.5 μm.
[0030] In some preferred embodiments, the thickness of the composite film is 1.5N3.0 μm.
[0031] In some preferred embodiments, the material of the substrate includes any one of 316L, 9Cr18, and single crystal silicon, but is not limited thereto.
[0032] In some preferred embodiments, the hardness of the composite film is greater than 6.5 GPa.
[0033] In some preferred embodiments, the composite film is subjected to a temperature of -60N80°C and an ambient pressure of ≤≤6.65×10 -3 The friction coefficient after thermal vacuum test was 0.06-0.07 under the conditions of Pa, 2.5 cycles and ≥11.5h of residence time, and the wear rate was 16×10 -7 18×10 -7 mm 3 / Nm.
[0034] In some preferred embodiments, the friction coefficient of the composite film after annealing at 600°C for 0.5h is 0.041-0.058, and the wear rate is 2.78×10 -7 N11.6×10 -7 mm 3 / Nm.
[0035] Another aspect of the embodiments of the present invention further provides a method for preparing the aforementioned soft metal-doped tungsten disulfide-based composite film, which comprises:
[0036] A titanium transition layer, a titanium / tungsten disulfide / nickel / copper gradient layer and a tungsten disulfide / nickel / copper layer are sequentially deposited on the substrate surface by magnetron sputtering technology to obtain a soft metal-doped tungsten disulfide-based composite film.
[0037] In some preferred embodiments, the preparation method specifically includes: using magnetron sputtering technology, using a titanium target as a cathode target material, using an inert gas as a working gas, applying a target current to the titanium target, and applying a negative bias voltage to the substrate, thereby depositing a titanium transition layer on the substrate surface, wherein the target current is 3.0 to 5.0 A, the substrate bias voltage is -70 to -100 V, the working gas flow rate is 30 to 35 sccm, the substrate temperature is 80 to 120 ° C, and the reaction chamber pressure is 1.0 to 3.0 × 10 -3 torr, and the deposition time is 600 to 900 s.
[0038] Further, the inert gas includes argon, but is not limited thereto.
[0039] In some preferred embodiments, the preparation method specifically includes: using magnetron sputtering technology, using titanium target, tungsten disulfide / nickel target, tungsten disulfide / copper target as cathode target material, using inert gas as working gas, applying target current to titanium target, tungsten disulfide / nickel target, tungsten disulfide / copper target, applying negative bias to the substrate, so as to deposit and form titanium / tungsten disulfide / nickel / copper gradient layer on the surface of the titanium transition layer; wherein, the target current applied to the titanium target gradually decreases from 3.0 to 5.0 A to 0, the target current applied to the tungsten disulfide / nickel target gradually increases from 0 to 0.8 to 1.6 A, the target current applied to the tungsten disulfide / copper target gradually increases from 0 to 0.8 to 1.6 A, the substrate bias is -30 to -70 V, the working gas flow rate is 30 to 35 sccm, the substrate temperature is 80 to 120 ° C, and the reaction chamber pressure is 1.0 to 3.0×10 -3 torr, and the deposition time is 600 to 900 s.
[0040] Further, the inert gas includes argon, but is not limited thereto.
[0041] In some preferred embodiments, the preparation method specifically includes: using magnetron sputtering technology, using tungsten disulfide / nickel target and tungsten disulfide / copper target as cathode target materials, using inert gas as working gas, applying target current to tungsten disulfide / nickel target and tungsten disulfide / copper target, and applying negative bias to the substrate, so as to deposit tungsten disulfide / nickel / copper layer on the surface of the titanium / tungsten disulfide / nickel / copper gradient layer; wherein the target current applied to the tungsten disulfide / nickel target is 0.8N1.6A, the target current applied to the tungsten disulfide / copper target is 0.8~1.6A, the substrate bias is -30~-70V, the working gas flow rate is 30~35sccm, the substrate temperature is 80~120°C, and the reaction chamber pressure is 1.0~3.0×10 -3 torr, and the deposition time is 9900~10300s.
[0042] Further, the inert gas includes argon, but is not limited thereto.
[0043] In some preferred embodiments, the preparation method further comprises: evacuating the reaction chamber to a vacuum degree of 3×10- 5 torr, the substrate surface is first cleaned and plasma etched.
[0044] Furthermore, the conditions of the plasma etching treatment include: applying a bias voltage of -400 to -500 V to the substrate, a substrate temperature of 100 to 150° C., and an etching time of 1200 to 1800 s.
[0045] In some more specific embodiments, the method for preparing the soft metal-doped tungsten disulfide-based composite film comprises the following steps:
[0046] (1) The titanium target sputtering current is 3-5 A, the substrate bias voltage is -70-100 V, the working gas is Ar, the working gas flow rate is 30-35 sccm, the deposition substrate temperature is 80-120 °C, and the reaction chamber pressure is 1.0-3.0×10 -3 torr, the deposition time is 600-900s, and a titanium transition layer is deposited on the substrate surface;
[0047] (2) The target current on the titanium target was gradually reduced from 3.0 to 5.0 A to 0, and the sputtering current applied to the tungsten disulfide / nickel target and the tungsten disulfide / copper target was gradually increased from 0 to 0.8 to 1.6 A. The substrate bias voltage was -30 to -70 V, the working gas flow rate was 30 to 35 sccm, the substrate temperature was 80 to 120 °C, and the reaction chamber pressure was 1.0 to 3.0 × 10 -3 torr, the deposition time is 99000-112000s, and a titanium / tungsten disulfide / nickel / copper gradient layer is deposited on the surface of the titanium transition layer;
[0048] (3) The sputtering current of the tungsten disulfide / nickel target and the tungsten disulfide / copper target was maintained at 0.8 to 1.6 A, the substrate bias voltage was -30 to -70 V, the working gas flow rate was 30 to 35 sccm, the substrate temperature was 80 to 120 °C, and the reaction chamber pressure was 1.0 to 3.0 × 10 -3 torr, and the deposition time is 9900-10300 s, and a tungsten disulfide / nickel / copper layer is formed on the titanium / tungsten disulfide / nickel / copper gradient layer.
[0049] Furthermore, the preparation method further comprises: pre-evacuating the reaction chamber to a vacuum degree of 3×10 -5 torr or less.
[0050] Furthermore, the preparation method further comprises: evacuating the reaction chamber to a predetermined vacuum degree (3×10 -5 torr or less), the substrate surface is first cleaned, and then plasma etching is performed. The specific etching method is to apply a bias voltage of -400 to -500V to the substrate, the etching substrate temperature is 100 to 150°C, and the etching time is 1200 to 1800s.
[0051] Another aspect of the embodiments of the present invention further provides the use of the aforementioned soft metal-doped tungsten disulfide-based composite film in the field of surface protection of aerospace devices in high temperature environments or high and low temperature alternating environments.
[0052] Furthermore, the material of the aerospace device includes 316L, 9Cr18 or single crystal silicon wafer, but is not limited thereto.
[0053] Another aspect of the embodiments of the present invention further provides a device, including a substrate, on which the aforementioned soft metal-doped tungsten disulfide-based composite film is also disposed.
[0054] Furthermore, the material of the substrate includes 316L, 9Cr18 or single crystal silicon wafer, but is not limited thereto.
[0055] Further, the device includes an aerospace vehicle.
[0056] The inventors of this case also conducted the following performance tests on the soft metal-doped tungsten disulfide-based composite film prepared above:
[0057] (1) The film thickness was tested using a scanning electron microscope, and the test results showed that the coating was 1.5 to 3.0 μm.
[0058] (2) Using nanoindentation instrument The hardness and elastic modulus of the film were measured with a diamond indenter, the indentation depth was 500 nm, and the average value was taken at six points. Test results: The nanohardness of the tungsten disulfide-based doped soft metal composite film of the present invention was greater than 6.5 GPa.
[0059] (4) The film bonding strength was tested by using the Revetest scratch test system (CSM, Revetest). The scratch test was performed three times at different positions according to the scratch test machine operating procedure. The experimental conditions were loading speed: 3 mm / min, scratch length: 5 mm, and loading force: 20 N. The test results showed that the bonding strength of the soft metal-doped tungsten disulfide-based composite film of the present invention reached 20 N (see Figure 4 ).
[0060] (5) Friction and wear test: A friction tester (TRB3) was used to conduct reciprocating dry friction tests on the films without annealing, after annealing at different temperatures and thermal vacuum testing in an atmospheric environment. The test was repeated 2 to 3 times. A 316L steel ball was used as the counterpart, and a reciprocating sliding method was adopted with a frequency of 5 Hz, a track length of 5 mm, a running distance of 90 m, and a normal load of 5 N. A surface profiler (ASTQ) was used to obtain the wear cross section, which was multiplied by the running step length to obtain the wear volume, and the wear volume was divided by the load and stroke to obtain the wear rate. Test results: After the thermal vacuum test, the friction coefficient was 0.06 to 0.07, and the wear rate was 16×10-7 to 18×10-7 mm. 3 / Nm, the friction coefficient after annealing at different temperatures is 0.041~0.058, and the wear rate is 2.78×10-7~11.6×10-7mm 3 / Nm.
[0061] In summary, by means of the above technical scheme, the soft metal doped tungsten disulfide-based composite film provided by the present invention has good hardness and elastic modulus, good friction and wear performance at different temperatures in the atmospheric environment, good temperature adaptive performance, high temperature oxidation resistance, and can meet the requirements of aerospace aircraft lubrication stability and long service life. The technical scheme of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical scheme of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.
[0062] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.
[0063] Example 1
[0064] In this embodiment, the substrate material is 316L, 9Cr18 or a single crystal silicon wafer. The tungsten disulfide-based doped soft metal composite film is prepared on the substrate surface by using magnetron sputtering technology, which mainly includes the following steps:
[0065] The substrate surface was mechanically polished, and the substrate material was placed in an acetone solution for ultrasonic cleaning for 15 minutes, dried with nitrogen, placed in an anhydrous ethanol solution for ultrasonic cleaning for 15 minutes, and dried with nitrogen.
[0066] The cleaned substrate was placed in the magnetron sputtering chamber and evacuated to a vacuum degree of less than 5×10 -5 torr, and then sputter clean the target for 30 minutes, with the substrate temperature at 100-150°C. The cleaned substrate is placed in the magnetron sputtering chamber and evacuated to a vacuum degree of less than 5×10 -5 torr, and then sputter clean the target for 30 minutes, the substrate temperature is 100-150 ° C. Preparation and deposition of tungsten disulfide-based doped soft metal composite film, the cavity is filled with high-purity argon, Ti target (purity 99.99at.%), WS2 / Ni target (purity 99.9at.%, weight ratio 90:10) and WS2 / Cu target (purity 99.9at.%, weight ratio 90:10) are used for control and setting, and magnetron sputtering technology is used. The specific steps are as follows:
[0067] (1) Plasma etching: a bias voltage of -500 V was applied to the substrate, the program running time was 25 min, and the substrate temperature was 150 °C.
[0068] (2) The titanium target sputtering current was 3.0 A, the substrate bias voltage was -80 V, the working gas was Ar, the gas flow rate was 35 sccm, the deposition substrate temperature was 100 °C, and the pressure was 1.1 × 10 -3 torr, the deposition time was 900s, the rotation speed was 2r / min, and a titanium transition layer with a thickness of about 100nm was deposited on the substrate surface;
[0069] (3) Gradually reduce the titanium target sputtering current to 0 A, and gradually increase the WS2 / Ni target and WS2 / Cu target sputtering current to 1.6 A. The working gas is Ar, the gas flow rate is 35 sccm, the substrate bias is -50 V, the deposition substrate temperature is 80 °C, and the pressure is 1.0×10 -3 torr, the deposition time was 900 s, the rotation speed was 0.5 r / min, and a titanium / tungsten disulfide / nickel / copper gradient layer was deposited on the surface of the titanium transition layer;
[0070] (4) The sputtering current of WS2 / Ni target and WS2 / Cu target was kept at 1.6 A, the working gas was Ar, the gas flow rate was 35 sccm, the substrate bias was -50 V, the deposition substrate temperature was 80 °C, and the pressure was 1.0 × 10 -3 torr, the deposition time was 9900 s, the rotation speed was 0.5 r / min, and a titanium / tungsten disulfide / nickel / copper layer was deposited on the surface of the titanium / tungsten disulfide / nickel / copper gradient layer until the total thickness of the composite film reached 2.0 μm.
[0071] The specific composition parameters of the prepared soft metal doped tungsten disulfide-based composite film samples are shown in Table 1.
[0072] The soft metal-doped tungsten disulfide-based composite film prepared after the above deposition treatment was subjected to the following tests:
[0073] (1) The film thickness was measured using a scanning electron microscope.
[0074] (2) Using nanoindenter The nanohardness and elastic modulus of the film were measured. Six different areas were collected for each sample, with an indentation depth of 500 nm. The average value was calculated and the hardness and elastic modulus results of the coating were shown in Table 2.
[0075] (4) The bonding performance of the film was tested using the Revetest scratch test system (CSM, Revetest). Three scratch tests were performed at different positions. The experimental conditions were loading speed: 3 mm / min, scratch length: 5 mm, and loading force: 20 N. The test results are shown in Table 2.
[0076] (5) A friction tester (TRB3) was used to conduct reciprocating dry friction tests on the films that had not been annealed, annealed at different temperatures, and tested in a thermal vacuum environment. The test was repeated 2 to 3 times. A 316L steel ball was used as the counterpart, and a reciprocating sliding method was adopted with a frequency of 5 Hz, a track length of 5 mm, a running distance of 90 m, and a normal load of 5 N. A surface profiler (ASTQ) was used to obtain the wear cross section, which was multiplied by the running step length to obtain the wear volume. The wear volume was divided by the load and stroke to obtain the wear rate. The test results of the friction coefficient and wear rate are shown in Tables 3 and 4, respectively.
[0077] Example 2
[0078] In this embodiment, the substrate material is 316L, 9Cr18 or a single crystal silicon wafer. The soft metal doped tungsten disulfide based composite film is prepared on the substrate surface by using magnetron sputtering technology, which mainly includes the following steps:
[0079] The substrate surface was mechanically polished, and the substrate material was placed in an acetone solution for ultrasonic cleaning for 15 minutes, dried with nitrogen, placed in an anhydrous ethanol solution for ultrasonic cleaning for 15 minutes, and dried with nitrogen.
[0080] The cleaned substrate was placed in the magnetron sputtering chamber and evacuated to a vacuum degree of less than 5×10 -5 torr, and then sputter clean the target for 30 minutes, with the substrate temperature at 100-150°C. The cleaned substrate is placed in the magnetron sputtering chamber and evacuated to a vacuum degree of less than 5×10 -5torr, and then sputter clean the target for 30 minutes, the substrate temperature is 100-150 ° C. Preparation and deposition of tungsten disulfide-based doped soft metal composite film, the cavity is filled with high-purity argon, Ti target (purity 99.99at.%), WS2 / Ni target (purity 99.9at.%, weight ratio 90:10) and WS2 / Cu target (purity 99.9at.%, weight ratio 90:10) are used for control and setting, and magnetron sputtering technology is used. The specific steps are as follows:
[0081] (1) Plasma etching: a bias voltage of -500 V was applied to the substrate, the program running time was 25 min, and the substrate temperature was 150 °C.
[0082] (2) The titanium target sputtering current was 3.0 A, the substrate bias voltage was -80 V, the working gas was Ar, the gas flow rate was 35 sccm, the deposition substrate temperature was 100 °C, and the pressure was 1.1 × 10 -3 torr, the deposition time was 900s, the rotation speed was 2r / min, and a titanium transition layer with a thickness of about 100nm was deposited on the substrate surface;
[0083] (3) The sputtering current of the titanium target was gradually reduced to 0 A, and the sputtering current of the WS2 / Ni target and the WS2 / Cu target was gradually increased to 1.6 A. The working gas was Ar, the gas flow rate was 35 sccm, the substrate bias was -50 V, the deposition substrate temperature was 80 °C, and the pressure was 1.0 × 10 -3 torr, the deposition time was 900s, the rotation speed was 1.0r / min, and a titanium / tungsten disulfide / nickel / copper gradient layer was deposited on the surface of the titanium transition layer;
[0084] (4) The sputtering current of WS2 / Ni target and WS2 / Cu target was kept at 1.6 A, the working gas was Ar, the gas flow rate was 35 sccm, the substrate bias was -50 V, the deposition substrate temperature was 80 °C, and the pressure was 1.0 × 10 -3 torr, the deposition time was 9900 s, the rotation speed was 1.0 r / min, and the titanium / tungsten disulfide / nickel / copper layer was deposited on the surface of the titanium / tungsten disulfide / nickel / copper gradient layer until the total thickness of the composite film reached 2.0 μm.
[0085] The specific composition parameters of the prepared soft metal doped tungsten disulfide-based composite film samples are shown in Table 1.
[0086] The soft metal-doped tungsten disulfide-based composite film prepared after the above deposition treatment was subjected to the following tests:
[0087] (1) The film thickness was measured using a scanning electron microscope.
[0088] (2) Using nanoindentation instrument The nanohardness and elastic modulus of the film were measured. Six different areas were collected for each sample, with an indentation depth of 500 nm. The average value was calculated and the hardness and elastic modulus results of the coating were shown in Table 2.
[0089] (4) The bonding performance of the film was tested using the Revetest scratch test system (CSM, Revetest). Three scratch tests were performed at different positions. The experimental conditions were loading speed: 3 mm / min, scratch length: 5 mm, and loading force: 20 N. The test results are shown in Table 2.
[0090] (5) A friction tester (TRB3) was used to conduct reciprocating dry friction tests on the films that had not been annealed, annealed at different temperatures, and tested in a thermal vacuum environment. The test was repeated 2 to 3 times. A 316L steel ball was used as the counterpart, and a reciprocating sliding method was adopted with a frequency of 5 Hz, a track length of 5 mm, a running distance of 90 m, and a normal load of 5 N. A surface profiler (ASTQ) was used to obtain the wear cross section, which was multiplied by the running step length to obtain the wear volume. The wear volume was divided by the load and stroke to obtain the wear rate. The test results of the friction coefficient and wear rate are shown in Tables 3 and 4, respectively.
[0091] Example 3
[0092] In this embodiment, the substrate material is 316L, 9Cr18 or a single crystal silicon wafer. The soft metal doped tungsten disulfide based composite film is prepared on the substrate surface by using magnetron sputtering technology, which mainly includes the following steps:
[0093] The substrate surface was mechanically polished, and the substrate material was placed in an acetone solution for ultrasonic cleaning for 15 minutes, dried with nitrogen, placed in an anhydrous ethanol solution for ultrasonic cleaning for 15 minutes, and dried with nitrogen.
[0094] The cleaned substrate was placed in the magnetron sputtering chamber and evacuated to a vacuum degree of less than 5×10 -5 torr, and then sputter clean the target for 30 minutes, with the substrate temperature at 100-150°C. The cleaned substrate is placed in the magnetron sputtering chamber and evacuated to a vacuum degree of less than 5×10 -5 torr, and then sputter clean the target for 30 minutes, the substrate temperature is 100-150 ° C. Preparation and deposition of tungsten disulfide-based doped soft metal composite film, the cavity is filled with high-purity argon, Ti target (purity 99.99at.%), WS2 / Ni target (purity 99.9at.%, weight ratio 90:10) and WS2 / Cu target (purity 99.9at.%, weight ratio 90:10) are used for control and setting, and magnetron sputtering technology is used. The specific steps are as follows:
[0095] (1) Plasma etching: a bias voltage of -500 V was applied to the substrate, the program running time was 25 min, and the substrate temperature was 150 °C.
[0096] (2) The titanium target sputtering current was 3.0 A, the substrate bias voltage was -80 V, the working gas was Ar, the gas flow rate was 35 sccm, the deposition substrate temperature was 100 °C, and the pressure was 1.1 × 10 -3 torr, the deposition time was 900s, the rotation speed was 2r / min, and a titanium transition layer with a thickness of about 100nm was deposited on the substrate surface;
[0097] (3) Gradually reduce the titanium target sputtering current to 0 A, and gradually increase the WS2 / Ni target and WS2 / Cu target sputtering current to 1.6 A. The working gas is Ar, the gas flow rate is 35 sccm, the substrate bias is -50 V, the deposition substrate temperature is 80 °C, and the pressure is 1.0×10 -3 torr, the deposition time was 900 s, the rotation speed was 2.0 r / min, and a titanium / tungsten disulfide / nickel / copper gradient layer was deposited on the surface of the titanium transition layer; (4) the sputtering current of the WS2 / Ni target and the WS2 / Cu target was kept at 1.6 A, the working gas was Ar, the gas flow rate was 35 sccm, the substrate bias was -50 V, the deposition substrate temperature was 80 °C, and the pressure was 1.0 × 10 -3 torr, the deposition time was 9900 s, the rotation speed was 2.0 r / min, and a titanium / tungsten disulfide / nickel / copper layer was deposited on the surface of the titanium / tungsten disulfide / nickel / copper gradient layer until the total thickness of the composite film reached 2.0 μm.
[0098] The specific composition parameters of the prepared soft metal doped tungsten disulfide-based composite film samples are shown in Table 1.
[0099] The soft metal-doped tungsten disulfide-based composite film prepared after the above deposition treatment was subjected to the following tests:
[0100] (1) The film thickness was measured using a scanning electron microscope.
[0101] (2) Using nanoindentation instrument The nanohardness and elastic modulus of the film were measured. Six different areas were collected for each sample, with an indentation depth of 500 nm. The average value was calculated and the hardness and elastic modulus results of the coating were shown in Table 2.
[0102] (4) The bonding performance of the film was tested using the Revetest scratch test system (CSM, Revetest). Three scratch tests were performed at different positions. The experimental conditions were loading speed: 3 mm / min, scratch length: 5 mm, and loading force: 20 N. The test results are shown in Table 2.
[0103] (5) A friction tester (TRB3) was used to conduct reciprocating dry friction tests on the films that had not been annealed, annealed at different temperatures, and tested in a thermal vacuum environment. The test was repeated 2 to 3 times. A 316L steel ball was used as the counterpart, and a reciprocating sliding method was adopted with a frequency of 5 Hz, a track length of 5 mm, a running distance of 90 m, and a normal load of 5 N. A surface profiler (ASTQ) was used to obtain the wear cross section, which was multiplied by the running step length to obtain the wear volume. The wear volume was divided by the load and stroke to obtain the wear rate. The test results of the friction coefficient and wear rate are shown in Tables 3 and 4, respectively.
[0104] Example 4
[0105] In this embodiment, the substrate material is 316L, 9Cr18 or a single crystal silicon wafer. The soft metal doped tungsten disulfide based composite film is prepared on the substrate surface by using magnetron sputtering technology, which mainly includes the following steps:
[0106] The substrate surface was mechanically polished, and the substrate material was placed in an acetone solution for ultrasonic cleaning for 15 minutes, dried with nitrogen, placed in an anhydrous ethanol solution for ultrasonic cleaning for 15 minutes, and dried with nitrogen.
[0107] The cleaned substrate was placed in the magnetron sputtering chamber and evacuated to a vacuum degree of less than 5×10 -5 torr, and then sputter clean the target for 30 minutes, with the substrate temperature at 100-150°C. The cleaned substrate is placed in the magnetron sputtering chamber and evacuated to a vacuum degree of less than 5×10 -5 torr, and then sputter clean the target for 30 minutes, the substrate temperature is 100-150 ° C. Preparation and deposition of tungsten disulfide-based doped soft metal composite film, the cavity is filled with high-purity argon, Ti target (purity 99.99at.%), WS2 / Ni target (purity 99.9at.%, weight ratio 90:10) and WS2 / Cu target (purity 99.9at.%, weight ratio 90:10) are used for control and setting, and magnetron sputtering technology is used. The specific steps are as follows:
[0108] (1) Plasma etching: a bias voltage of -500 V was applied to the substrate, the program running time was 25 min, and the substrate temperature was 150 °C.
[0109] (2) The titanium target sputtering current was 3.0 A, the substrate bias voltage was -80 V, the working gas was Ar, the gas flow rate was 35 sccm, the deposition substrate temperature was 100 °C, and the pressure was 1.1 × 10 -3 torr, the deposition time was 900s, the rotation speed was 2r / min, and a titanium transition layer with a thickness of about 100nm was deposited on the substrate surface;
[0110] (3) Gradually reduce the titanium target sputtering current to 0 A, and gradually increase the WS2 / Ni target and WS2 / Cu target sputtering current to 1.6 A. The working gas is Ar, the gas flow rate is 35 sccm, the substrate bias is -50 V, the deposition substrate temperature is 80 °C, and the pressure is 1.0×10 -3 torr, the deposition time was 900s, the rotation speed was 3.0r / min, and a titanium / tungsten disulfide / nickel / copper gradient layer was deposited on the surface of the titanium transition layer;
[0111] (4) The sputtering current of WS2 / Ni target and WS2 / Cu target was kept at 1.6 A, the working gas was Ar, the gas flow rate was 35 sccm, the substrate bias was -50 V, the deposition substrate temperature was 80 °C, and the pressure was 1.0 × 10 -3 torr, the deposition time was 9900 s, the rotation speed was 3.0 r / min, and a titanium / tungsten disulfide / nickel / copper layer was deposited on the surface of the titanium / tungsten disulfide / nickel / copper gradient layer until the total thickness of the composite film reached 2.0 μm.
[0112] The specific composition parameters of the prepared soft metal doped tungsten disulfide-based composite film samples are shown in Table 1.
[0113] The soft metal-doped tungsten disulfide-based composite film prepared after the above deposition treatment was subjected to the following tests:
[0114] (1) The film thickness was measured using a scanning electron microscope.
[0115] (2) Using nanoindentation instrument The nanohardness and elastic modulus of the film were measured. Six different areas were collected for each sample, with an indentation depth of 500 nm. The average value was calculated and the hardness and elastic modulus results of the coating were shown in Table 2.
[0116] (4) The bonding performance of the film was tested using the Revetest scratch test system (CSM, Revetest). Three scratch tests were performed at different positions. The experimental conditions were loading speed: 3 mm / min, scratch length: 5 mm, and loading force: 20 N. The test results are shown in Table 2.
[0117] (5) A friction tester (TRB3) was used to conduct reciprocating dry friction tests on the films that had not been annealed, annealed at different temperatures, and tested in a thermal vacuum environment. The test was repeated 2 to 3 times. A 316L steel ball was used as the counterpart, and a reciprocating sliding method was adopted with a frequency of 5 Hz, a track length of 5 mm, a running distance of 90 m, and a normal load of 5 N. A surface profiler (ASTQ) was used to obtain the wear cross section, which was multiplied by the running step length to obtain the wear volume. The wear volume was divided by the load and stroke to obtain the wear rate. The test results of the friction coefficient and wear rate are shown in Tables 3 and 4, respectively.
[0118] Comparative Example 1
[0119] In this embodiment, the substrate material is 316L, 9Cr18 or a single crystal silicon wafer. The tungsten disulfide coating is prepared on the substrate surface by using magnetron sputtering technology, which mainly includes the following steps:
[0120] The substrate surface was mechanically polished, and the substrate material was placed in an acetone solution for ultrasonic cleaning for 15 minutes, dried with nitrogen, placed in an anhydrous ethanol solution for ultrasonic cleaning for 15 minutes, and dried with nitrogen.
[0121] The cleaned substrate was placed in the magnetron sputtering chamber and evacuated to a vacuum degree of less than 5×10 -5 torr, and then sputter clean the target for 30 minutes, with the substrate temperature at 100-150°C.
[0122] To prepare and deposit tungsten disulfide thin film, high-purity argon gas is filled into the chamber, Ti target (purity of 99.99 at.%) and tungsten disulfide target (purity of 99.9 at.%) are used for layout and control, and magnetron sputtering technology is used. The specific steps are as follows:
[0123] (1) Plasma etching: a bias voltage of -450 V was applied to the substrate, the program running time was 30 min, and the substrate temperature was 120 °C.
[0124] (2) The titanium target sputtering current was 3.0 A, the substrate bias voltage was -70 V, the working gas was Ar, the gas flow rate was 35 sccm, the deposition substrate temperature was 80 °C, and the pressure was 1.0x10 -3 torr, the deposition time is 900s, and a 200nm titanium transition layer is deposited on the substrate surface;
[0125] (3) Gradually reduce the titanium target sputtering current to 0 A, and gradually increase the tungsten disulfide target sputtering current to 1.6 A. The working gas is Ar, the gas flow rate is 35 sccm, the substrate bias is -50 V, the deposition substrate temperature is 80 °C, the rotation speed is 2.0 r / min, and the pressure is 1.3x10 -3 torr, deposition time 9900s, titanium / tungsten disulfide gradient layer deposited on the titanium transition layer surface;
[0126] (4) The sputtering current of WS2 target was maintained at 1.6 A, the working gas was Ar, the gas flow rate was 35 sccm, the substrate bias was -50 V, the deposition substrate temperature was 80 °C, and the pressure was 1.0 × 10 -3 torr, the deposition time was 900 s, the rotation speed was 0.5 r / min, and a tungsten disulfide layer was deposited on the surface of the titanium / tungsten disulfide gradient layer until the total thickness of the composite film reached 2.0 μm.
[0127] The specific composition parameters of the prepared tungsten disulfide film sample are shown in Table 1.
[0128] The tungsten disulfide film prepared after the above deposition treatment was subjected to the following tests:
[0129] (1) The film thickness was measured using a scanning electron microscope.
[0130] (2) Using nanoindenter The nanohardness and elastic modulus of the film were measured. Six different areas were collected for each sample, with an indentation depth of 500 nm. The average value was calculated and the hardness and elastic modulus results of the coating were shown in Table 2.
[0131] (4) The bonding performance of the film was tested using the Revetest scratch test system (CSM, Revetest). Three scratch tests were performed at different positions. The experimental conditions were loading speed: 3 mm / min, scratch length: 5 mm, and loading force: 20 N. The test results are shown in Table 2.
[0132] (5) A friction tester (TRB3) was used to conduct reciprocating dry friction tests on the films that had not been annealed, annealed at different temperatures, and tested in a thermal vacuum environment. The test was repeated 2 to 3 times. A 316L steel ball was used as the counterpart, and a reciprocating sliding method was adopted with a frequency of 5 Hz, a track length of 5 mm, a running distance of 90 m, and a normal load of 5 N. A surface profiler (ASTQ) was used to obtain the wear cross section, which was multiplied by the running step length to obtain the wear volume. The wear volume was divided by the load and stroke to obtain the wear rate. The test results of the friction coefficient and wear rate are shown in Tables 3 and 4, respectively.
[0133] Comparative Example 2
[0134] The method is the same as Example 4, except that the tungsten disulfide / nickel target is missing.
[0135] Comparative Example 3
[0136] The method is the same as Example 4, except that the tungsten disulfide / copper target is missing.
[0137] Comparative Example 4
[0138] The method is the same as that of Example 4, except that the content of Ni and Cu in the tungsten disulfide / copper target is increased, and the target atomic ratio is increased from 70:30% to 50:50%.
[0139] Table 1: Composition parameters of film samples
[0140]
[0141] The nanoindentation equipment was used to press six points with a depth of 500 nm on the surface of the five film samples to measure the hardness and elastic modulus. The results are shown in Table 2. As can be seen from Table 2, the hardness of the four tungsten disulfide-based doped soft metal composite films is not less than 6.5 GPa, among which WS2-Ni-Cu-3 has the best mechanical properties.
[0142] Figure 1 This is a cross-sectional SEM image of the WS2-Ni-Cu-3 film obtained in Example 3 of the present invention.
[0143] Figure 2 This is a bonding force morphology diagram of the WS2-Ni-Cu-3 film prepared in Example 3 of the present invention.
[0144] Figure 3 This is a test chart of hardness and elastic modulus of the WS2-Ni-Cu-3 film prepared in Example 3 of the present invention.
[0145] Table 2: Hardness and elastic modulus of film samples
[0146]
[0147]
[0148] The friction coefficients and wear rates of the eight films in the atmospheric environment are shown in Table 3. WS2-Ni-Cu-3 in Example 3 has the best friction coefficient.
[0149] Figure 4 It is a friction curve diagram of the WS2-Ni-Cu-3 film prepared in Example 3 of the present invention at room temperature, after high temperature annealing at 600°C and after thermal vacuum testing.
[0150] Table 3: Friction and wear table of film samples in atmospheric environment
[0151]
[0152] The friction coefficients and wear rates of the eight films under high and low temperature alternation and at different temperatures are shown in Table 4. WS2-Ni-Cu-3 in Example 3 has the smallest friction coefficient.
[0153] Figure 5 This is a wear rate diagram of the WS2-Ni-Cu-3 film prepared in Example 3 of the present invention at room temperature, after high-temperature annealing at 600°C, and after thermal vacuum testing.
[0154] Table 4: Friction and wear of WS2-Ni-Cu-3 film samples under high and low temperature alternation and at different temperatures
[0155]
[0156]
[0157] In summary, the composite film provided by the present invention has good hardness (not less than 6.5 GPa) and elastic modulus, a bonding force of 20 N, a friction coefficient of 0.04 after heat treatment at 600°C, and good friction and wear properties under atmospheric alternation environments and under different temperature and humidity environments. It has good temperature adaptability and high temperature oxidation resistance, and can meet the requirements of lubrication stability and long service life of aerospace vehicles.
[0158] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0159] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.
Claims
1. A soft metal doped tungsten disulfide-based composite film, characterized in that: include: A titanium transition layer, a titanium / tungsten disulfide / nickel / copper gradient layer and a tungsten disulfide / nickel / copper layer are sequentially formed on the surface of the substrate; Among them, in the direction gradually away from the substrate, the titanium content in the titanium / tungsten disulfide / nickel / copper gradient layer gradually decreases, the molybdenum disulfide content gradually increases, the nickel content gradually increases, and the copper content gradually increases; at the same time, the tungsten disulfide / nickel / copper layer is formed by alternatingly stacking nickel-tungsten disulfide layers and copper-tungsten disulfide layers.
2. The composite film according to claim 1, characterized in that: The atomic content of nickel atoms in the soft metal-doped tungsten disulfide-based composite film is 8 to 12 at%, and the atomic content of copper atoms is 1 to 4 at%; and / or, the thickness of the titanium transition layer is 100-200 nm; and / or, the thickness of the titanium / tungsten disulfide / nickel / copper gradient layer is 100-300 nm; and / or, the thickness of the tungsten disulfide / nickel / copper layer is 1.5-2.5 μm; and / or, the thickness of the composite film is 1.5-3.0 μm; And / or, the material of the substrate includes any one of 316L, 9Cr18, and single crystal silicon.
3. The composite film according to claim 1, characterized in that: The hardness of the composite film is greater than 6.5 GPa; And / or, the composite film is at a temperature of -60 to 80°C and an ambient pressure of ≤6.65×10 -3 The friction coefficient after thermal vacuum test under the conditions of pa, 2.5 cycles and ≥11.5h is 0.06-0.07, and the wear rate is 16×10 -7 ~18×10 -7 mm 3 / Nm; And / or, the friction coefficient of the composite film after annealing at 600°C for 0.5h is 0.041-0.058, and the wear rate is 2.78×10 -7 ~11.6×10 -7 mm 3 / Nm.
4. The method for preparing a soft metal-doped tungsten disulfide-based composite film according to any one of claims 1 to 3, characterized in that: include: A titanium transition layer, a titanium / tungsten disulfide / nickel / copper gradient layer and a tungsten disulfide / nickel / copper layer are sequentially deposited on the substrate surface by magnetron sputtering technology to obtain a soft metal-doped tungsten disulfide-based composite film.
5. The preparation method according to claim 4, characterized in that: Specifically include: The magnetron sputtering technology is used, with titanium target as cathode target material, inert gas as working gas, target current applied to the titanium target, and negative bias applied to the substrate, so as to deposit and form a titanium transition layer on the substrate surface, wherein the target current is 3.0-5.0A, the substrate bias is -70--100V, the working gas flow rate is 30-35sccm, the substrate temperature is 80-120℃, and the reaction chamber pressure is 1.0-3.0×10 -3 torr, and the deposition time is 600-900 s; preferably, the inert gas includes argon.
6. The preparation method according to claim 4, characterized in that: Specifically include: The magnetron sputtering technology is adopted, titanium target, tungsten disulfide / nickel target, and tungsten disulfide / copper target are used as cathode target materials, inert gas is used as working gas, target current is applied to the titanium target, tungsten disulfide / nickel target, and tungsten disulfide / copper target, and negative bias voltage is applied to the substrate, so as to deposit and form a titanium / tungsten disulfide / nickel / copper gradient layer on the surface of the titanium transition layer; wherein the target current applied to the titanium target gradually decreases from 3.0 to 5.0 A to 0, the target current applied to the tungsten disulfide / nickel target gradually increases from 0 to 0.8 to 1.6 A, the target current applied to the tungsten disulfide / copper target gradually increases from 0 to 0.8 to 1.6 A, the substrate bias voltage is -30 to -70 V, the working gas flow rate is 30 to 35 sccm, the substrate temperature is 80 to 120 ° C, and the reaction chamber pressure is 1.0 to 3.0×10 -3 torr, and the deposition time is 600-900 s; preferably, the inert gas includes argon.
7. The preparation method according to claim 4, characterized in that: Specifically include: The magnetron sputtering technology is adopted, tungsten disulfide / nickel target and tungsten disulfide / copper target are used as cathode target materials, inert gas is used as working gas, target current is applied to the tungsten disulfide / nickel target and tungsten disulfide / copper target, and negative bias voltage is applied to the substrate, so as to deposit and form a tungsten disulfide / nickel / copper layer on the surface of the titanium / tungsten disulfide / nickel / copper gradient layer; wherein the target current applied to the tungsten disulfide / nickel target is 0.8-1.6A, the target current applied to the tungsten disulfide / copper target is 0.8-1.6A, the substrate bias voltage is -30--70V, the working gas flow rate is 30-35sccm, the substrate temperature is 80-120°C, and the reaction chamber pressure is 1.0-3.0×10 -3 torr, the time for depositing the tungsten disulfide / nickel / copper layer is 9900-10300s; preferably, the inert gas includes argon.
8. The preparation method according to claim 4, characterized in that: Also includes: The reaction chamber was evacuated to a vacuum degree of 3 × 10 -5 torr or less, firstly clean the substrate surface and perform plasma etching; preferably, the conditions of the plasma etching treatment include: applying a bias voltage of -400 to -500 V to the substrate, the substrate temperature is 100 to 150° C., and the etching time is 1200 to 1800 s.
9. Use of the soft metal-doped tungsten disulfide-based composite film according to any one of claims 1-3 in the field of surface protection of aerospace devices in high temperature environments or high and low temperature alternating environments; preferably, the material of the aerospace device includes 316L, 9Cr18 or single crystal silicon wafer.
10. A device comprising a substrate, characterized in that: The substrate is also provided with a soft metal-doped tungsten disulfide-based composite film as described in any one of claims 1 to 3; preferably, the material of the substrate includes 316L, 9Cr18 or a single crystal silicon wafer; preferably, the device includes an aerospace vehicle.
Citation Information
Patent Citations
Molybdenum disulfide sulfide / copper composite film and preparation method and application thereof
CN114574826A
Ni-cu alloy composite plating solution
JP2002180297A
Solid lubricating film and solid lubricating bearing
JP2007063362A
Self-lubricating wear-resistant composite materials
US3956146A
Cited By
WS2-based composite coating and preparation method thereof
CN122105314A