Zirconium-based alloy target material as well as preparation method and application thereof

Through aerosolization and hot press sintering processes, the density and uniformity of zirconium-based alloy targets are solved, and high-performance getter film materials are prepared, which simplifies the process flow and reduces costs.

CN118957519AInactive Publication Date: 2024-11-15KONFOONG MATERIALS INTERNATIONAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411042848.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing zirconium-based alloy target preparation process, the density is insufficient, the uniformity is poor, the thermal isostatic operation is difficult and the cost is high, which affects the performance and application range of the getter film.

Method used

By aerosolizing and hot press sintering, the zirconium-based alloy raw materials are melted and formed into a uniform powder. Then, through hot press sintering, a high density and high purity alloy target is obtained to ensure the uniformity and low of the getter film. Activate temperature.

Benefits of technology

The preparation of zirconium-based alloy targets with high density and high purity has been achieved, which significantly improves the performance and application convenience of getter films, is easy to operate, reduces production costs, and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a zirconium-based alloy target as well as a preparation method and application thereof. The preparation method comprises the following steps: carrying out vacuum melting on a target raw material containing a zirconium elementary substance in a protective atmosphere, and cooling to obtain a zirconium-based alloy ingot; the zirconium-based alloy ingot is fused and then subjected to gas atomization, and zirconium-based alloy powder is obtained; and the zirconium-based alloy powder is subjected to hot pressed sintering and then machined, and the zirconium-based alloy target material is obtained. According to the method, target raw materials are smelted to obtain alloy, then the alloy is crushed and solidified in a gas atomization mode to form alloy powder, contact diffusion of powder particles is promoted in a hot pressing sintering mode, and therefore the high-density and high-purity alloy target is obtained, the grain structure uniformity is high, and when the alloy target is used for preparing a getter film, the service life of the getter film is prolonged. The film is high in uniformity, and the getter is low in activation temperature, convenient to use and excellent in getter performance by controlling the alloy material and content; the method is easy and convenient to operate and low in cost, and mass production is easy to achieve.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of alloy target material preparation, and relates to a zirconium-based alloy target material and a preparation method and application thereof. Background Art

[0002] In recent years, as electronic vacuum devices develop towards miniaturization, integration and flattening, the requirements for getter materials are getting higher and higher, gradually changing from evaporative type to non-evaporative type, and the shape has developed from traditional cylindrical to thin film. Non-evaporable getters have been widely used in scientific research and industrial production in electronic vacuum devices, ultra-high vacuum acquisition, atomic energy industry, etc. due to their low equilibrium pressure, large air absorption capacity and high air absorption rate.

[0003] There is a dense oxide film on the surface of non-evaporable getters, which needs to be activated under vacuum conditions to allow oxygen atoms to migrate into the interior of the getter material, thereby exposing the more active getter surface. However, the early non-evaporable getters could not be used in some devices with thermosensitive elements due to their high activation temperature, which affected their application range. Therefore, it is necessary to study getter materials with low activation temperatures. Existing non-evaporable getter materials mainly include zirconium-based alloy getters, including zirconium-aluminum getters, zirconium-cobalt rare earth getters, zirconium-vanadium getters, etc. Zirconium-vanadium getters have been widely used in many fields due to their low activation temperature. However, zirconium-vanadium getters are usually made of targets of corresponding materials, and the characteristics of the target materials will seriously affect the getter performance of the getter film material.

[0004] CN 115679274A discloses a ZrVFe alloy target material and its preparation method and application. The preparation method comprises: alloy suspension smelting to obtain ZrVFe alloy ingot, then suspension refining, casting and molding, cooling to obtain alloy target blank, cutting and preliminary processing, hot isostatic pressing, and grinding to obtain ZrVFe alloy target material. This method still adopts casting and hot isostatic pressing to prepare target material. The molding method in this method easily causes insufficient density and poor uniformity of target material, and the pressure required for hot isostatic pressing is high, the operation is difficult, and the production cost is high.

[0005] CN 113652662A discloses a getter magnetron target material, including a getter alloy target material and a copper back plate. The raw materials of the getter alloy target material include zirconium, cobalt and rhenium metal powders. The manufacturing process includes: mixing the three metal powders and loading them into a sleeve mold, using a hot isostatic pressing process, sintering and densifying the mixed alloy under high temperature and high pressure to obtain an alloy target semi-finished product, and then cutting and welding the back plate to obtain the getter magnetron target material. This method directly mixes the raw material powders and then performs hot isostatic pressing, which cannot ensure the uniformity of the alloy target material, the density is insufficient, the grain size is uneven, and the getter material with uniform thickness and composition cannot be prepared during magnetron sputtering.

[0006] CN 111647858A discloses a method for preparing an aluminum-scandium alloy target material, which comprises: smelting aluminum raw materials and scandium raw materials in a cold crucible suspension to obtain an aluminum-scandium alloy melt; casting the aluminum-scandium alloy melt onto a mold and cooling it to obtain an aluminum-scandium alloy ingot, placing it in a vacuum crucible furnace to melt it into an aluminum-scandium alloy liquid, atomizing it to obtain an aluminum-scandium alloy powder, sintering it to obtain an aluminum-scandium alloy target blank, and finally machining it to obtain an aluminum-scandium alloy target material. This method atomizes the raw materials after smelting to form a uniform alloy phase, and then hot-presses and sinters it to obtain a dense target material, but the preparation process of targets of different materials may be different and may not be completely applicable.

[0007] In summary, for the preparation process of zirconium-based alloy targets used as getters, a suitable process combination is needed to improve the density and uniformity of the targets and ensure their high purity, which is more conducive to the preparation and application of high-performance getter films. Summary of the invention

[0008] In view of the problems existing in the prior art, the purpose of the present invention is to provide a zirconium-based alloy target material and a preparation method and use thereof. By successively adopting the methods of gas atomization and hot pressing sintering, the raw materials are melted to form a uniform alloy powder, and then hot pressing and sintering are performed to obtain a high-density, high-purity alloy target material with strong structural uniformity. When used for preparing a getter, it is easy to use and has excellent aspiration performance.

[0009] To achieve this object, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides a method for preparing a zirconium-based alloy target, the preparation method comprising the following steps:

[0011] (1) vacuum melting a target material including zirconium in a protective atmosphere, and obtaining a zirconium-based alloy ingot after cooling;

[0012] (2) melting the zirconium-based alloy ingot obtained in step (1) and then atomizing it to obtain a zirconium-based alloy powder;

[0013] (3) The zirconium-based alloy powder obtained in step (2) is hot-pressed and sintered, and then machined to obtain a zirconium-based alloy target.

[0014] In the present invention, for the preparation of alloy target materials, in order to ensure the uniformity of raw materials when forming alloys, it is first necessary to melt and mix the raw materials and then form a solid phase. The present invention first melts the target raw materials to obtain the alloy, then uses a gas atomization method to break it into fine droplets, forms alloy powder after solidification, and then promotes the contact and diffusion of powder particles through hot pressing and sintering, thereby obtaining a high-density alloy target material with strong uniformity of grain structure. When the target material is magnetron sputtered to prepare a getter film, the film has strong uniformity, and by controlling the alloy material, it is ensured that the activation temperature of the getter is low, it is easy to use, and has excellent getter performance; the method is simple to operate, low in cost, and easy to achieve mass production.

[0015] The following are preferred technical solutions of the present invention, but are not intended to be limitations of the technical solutions provided by the present invention. Through the following technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.

[0016] As a preferred technical solution of the present invention, the zirconium-based alloy target material includes a zirconium-vanadium-iron alloy target material.

[0017] Preferably, the mass fraction of zirconium in the target material raw material in step (1) is 60-80wt%, for example, 60wt%, 62wt%, 65wt%, 68wt%, 70wt%, 72wt%, 75wt%, 78wt% or 80wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0018] Preferably, the zirconium element in step (1) includes sponge zirconium or nuclear grade zirconium, and its purity is 2N5 or above, for example 2N5, 2N6, 2N8, 3N, 3N2, 3N5 or 4N, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0019] Preferably, when the zirconium-based alloy selects zirconium-vanadium-iron alloy, the mass fraction of vanadium raw material in the target raw material is 15-30wt%, for example, 15wt%, 16wt%, 18wt%, 20wt%, 22wt%, 25wt%, 27wt% or 30wt%, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are equally applicable; the mass fraction of iron raw material is 5-10wt%, for example, 5wt%, 6wt%, 7wt%, 8wt%, 9wt% or 10wt%, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are equally applicable.

[0020] In the present invention, the selection of the zirconium-vanadium-iron alloy, especially the control of the content of each element, helps to reduce the activation temperature when it is used as a getter; if the zirconium content is too high and the vanadium and iron contents are too low, it is not conducive to the reduction of the activation temperature, while if the zirconium content is too low and the vanadium and iron contents are too high, it will cause a decrease in the getter performance.

[0021] Preferably, the iron raw material includes electrolytic iron having a purity of 3N or above, such as 3N, 3N2, 3N4, 3N5, 3N6, 3N8 or 4N, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0022] Preferably, the vanadium raw material includes vanadium particles having a purity of 3N or above, such as 3N, 3N2, 3N4, 3N5, 3N6, 3N8 or 4N, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] As a preferred technical solution of the present invention, the smelting in step (1) is carried out in a smelting furnace.

[0024] Preferably, the protective gas in step (1) comprises an inert gas, and the inert gas comprises helium, neon, argon, etc.

[0025] Preferably, the temperature of the vacuum melting in step (1) is 1300-1500°C, for example, 1300°C, 1320°C, 1350°C, 1380°C, 1400°C, 1420°C, 1450°C, 1470°C or 1500°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] Preferably, in step (1), the target material is mechanically stirred after being completely melted.

[0027] Preferably, the mechanical stirring time is 3 to 8 minutes, for example, 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes or 8 minutes, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] Preferably, the cooling method in step (1) is furnace cooling, and cooling to room temperature under the condition of continuous introduction of protective gas.

[0029] As a preferred technical solution of the present invention, the zirconium-based alloy ingot in step (2) is placed in an atomizing furnace for heating, melting and gas atomization.

[0030] Preferably, in step (2), the zirconium-based alloy ingot is heated to 1400-1500°C and completely melted, for example, 1400°C, 1420°C, 1440°C, 1450°C, 1460°C, 1480°C or 1500°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0031] Preferably, the atmosphere in the atomization furnace is a protective gas.

[0032] As a preferred technical solution of the present invention, the atomization in step (2) uses a nozzle to spray inert gas onto the alloy melt.

[0033] Preferably, the diameter of the nozzle is 2-4 mm, such as 2 mm, 2.5 mm, 3 mm, 3.5 mm or 4 mm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0034] Preferably, the alloy melt is atomized to form powder, and then the temperature is continuously lowered to room temperature.

[0035] Preferably, in step (2), the zirconium-based alloy powder is sieved and the sieve material is taken to remove the powder with larger particles.

[0036] Preferably, the size of the mesh holes in the sieve used for the screening is 75 to 125 mesh, such as 75 mesh, 80 mesh, 90 mesh, 100 mesh, 110 mesh, 120 mesh or 125 mesh, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] As a preferred technical solution of the present invention, the zirconium-based alloy powder in step (3) is first loaded into a mold and then placed as a whole in a hot pressing sintering furnace.

[0038] Preferably, the mold comprises a graphite mold, a metal plate is arranged between the inner surface of the mold and the zirconium-based alloy powder, and a coating is sprayed on the surface of the metal plate.

[0039] Preferably, the material of the metal plate includes any one of stainless steel, titanium or titanium alloy, and the coating includes boron nitride coating.

[0040] In the present invention, a high temperature resistant metal plate is used and a coating is sprayed, which can effectively isolate the alloy powder from the graphite mold, reduce carburization, and ensure the purity of the alloy target material.

[0041] Preferably, the zirconium-based alloy powder is placed in a mold and then vacuumed.

[0042] As a preferred technical solution of the present invention, the temperature of the hot pressing sintering in step (3) is 950-1200°C, for example, 950°C, 1000°C, 1050°C, 1100°C, 1150°C or 1200°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0043] Preferably, the pressure of the hot pressing sintering in step (3) is 30-40 MPa, for example 30 MPa, 32 MPa, 34 MPa, 35 MPa, 36 MPa, 38 MPa or 40 MPa, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] Preferably, the heat preservation and pressure holding time of the hot pressing sintering in step (3) is 3 to 5 hours, for example 3 hours, 3.25 hours, 3.5 hours, 3.75 hours, 4 hours, 4.25 hours, 4.5 hours, 4.75 hours or 5 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0045] Preferably, after the hot pressing sintering in step (3) is completed, the temperature and pressure are lowered, and the temperature is lowered along with the furnace, and the pressure is lowered by gradient pressure reduction.

[0046] As a preferred technical solution of the present invention, the machining in step (3) includes wire cutting and grinding.

[0047] Preferably, the wire cutting cuts the zirconium-based alloy target blank into a finished product size.

[0048] Preferably, the grinding process uses a grinder to grind the surface of the zirconium-based alloy target blank flat.

[0049] In a second aspect, the present invention provides a zirconium-based alloy target material obtained by the above-mentioned preparation method.

[0050] In a third aspect, the present invention provides a use of the above-mentioned zirconium-based alloy target material, wherein the zirconium-based alloy target material is used for preparing a getter film.

[0051] Compared with the prior art, the present invention has the following beneficial effects:

[0052] (1) The method of the present invention first melts the target material raw material to obtain an alloy, then uses gas atomization to break it into fine droplets, forms alloy powder after solidification, and then promotes the contact and diffusion of powder particles through hot pressing sintering, thereby obtaining a high-density, high-purity alloy target material with strong grain structure uniformity and high purity of the target material;

[0053] (2) The zirconium-based alloy target prepared by the method of the present invention is used to prepare a getter film, and the uniformity of the film is strong. By controlling the alloy material and content, the activation temperature of the getter is ensured to be low, the use is convenient, and the getter performance is excellent;

[0054] (3) The method of the present invention is simple to operate, low in cost, and easy to achieve mass production. DETAILED DESCRIPTION

[0055] In order to better illustrate the present invention and facilitate understanding of the technical solution of the present invention, the present invention is further described in detail below. However, the following embodiments are only simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0056] The specific implementation method of the present invention provides a method for preparing a zirconium-based alloy target, and the preparation method comprises the following steps:

[0057] (1) vacuum melting a target material including zirconium in a protective atmosphere, and obtaining a zirconium-based alloy ingot after cooling;

[0058] (2) melting the zirconium-based alloy ingot obtained in step (1) and then atomizing it to obtain a zirconium-based alloy powder;

[0059] (3) The zirconium-based alloy powder obtained in step (2) is hot-pressed and sintered, and then machined to obtain a zirconium-based alloy target.

[0060] The following are typical but non-limiting embodiments of the present invention:

[0061] Embodiment 1:

[0062] This embodiment provides a method for preparing a zirconium-based alloy target, and the preparation method comprises the following steps:

[0063] (1) adding zirconium sponge with a purity of 2N5, vanadium particles with a purity of 3N, and electrolytic iron with a purity of 3N into a smelting furnace in a ratio of 70wt%, 20wt% and 10wt%, respectively, and performing vacuum smelting in an argon protective atmosphere at a temperature of 1400° C. After the raw materials are completely melted, they are mechanically stirred for 5 minutes, and cooled to room temperature with the furnace under the condition of continuous introduction of protective argon gas to obtain a zirconium-based alloy ingot;

[0064] (2) placing the zirconium-based alloy ingot obtained in step (1) in an atomizing furnace and heating it to 1450° C. to completely melt it, wherein the atmosphere in the atomizing furnace is argon gas, and then spraying argon gas on the alloy melt through a nozzle to atomize it into powder, wherein the diameter of the nozzle is 3 mm, to obtain zirconium-based alloy powder, and sieving the zirconium-based alloy powder through a 100-mesh sieve to take the sieve residue;

[0065] (3) The zirconium-based alloy powder screened in step (2) is first loaded into a graphite mold and then evacuated; a titanium alloy metal plate is arranged between the inner surface of the graphite mold and the zirconium-based alloy powder, the surface of the metal plate is sprayed with boron nitride coating, and then the whole is placed in a hot pressing sintering furnace for hot pressing sintering. The hot pressing sintering temperature is 1100° C., the pressure is 35 MPa, and the heat preservation and pressure holding time is 4 hours. After the hot pressing sintering is completed, the temperature and pressure are reduced, and the cooling method is furnace cooling, and the pressure reduction method is gradient pressure reduction, and then machining is performed. The machining includes wire cutting and grinding. The wire cutting cuts the zirconium-based alloy target blank to the finished product size. The grinding uses a grinder to grind the surface of the zirconium-based alloy target blank to obtain a zirconium-vanadium-iron alloy target.

[0066] In this embodiment, the above method is used to prepare a zirconium-vanadium-iron alloy target, and the density of the target reaches 99.2%. It is used to prepare a getter film, and the activation temperature of the getter film is low and can be used at room temperature, and the getter performance is excellent.

[0067] Embodiment 2:

[0068] This embodiment provides a method for preparing a zirconium-based alloy target, and the preparation method comprises the following steps:

[0069] (1) adding zirconium sponge with a purity of 2N5, vanadium particles with a purity of 3N, and electrolytic iron with a purity of 3N into a smelting furnace in a ratio of 75wt%, 18wt%, and 7wt%, respectively, and performing vacuum smelting in an argon protective atmosphere at a temperature of 1300° C. After the raw materials are completely melted, mechanical stirring is performed for 8 minutes, and the raw materials are cooled to room temperature with the furnace under the condition of continuous introduction of protective argon gas to obtain a zirconium-based alloy ingot;

[0070] (2) placing the zirconium-based alloy ingot obtained in step (1) in an atomizing furnace and heating it to 1400° C. to completely melt it, wherein the atmosphere in the atomizing furnace is argon gas, and then using a nozzle to spray argon gas on the alloy melt to atomize it into powder, wherein the diameter of the nozzle is 2 mm, to obtain a zirconium-based alloy powder, and the zirconium-based alloy powder is sieved through a 120-mesh sieve and the sieve residue is taken;

[0071] (3) The zirconium-based alloy powder screened in step (2) is first loaded into a graphite mold and then evacuated; a titanium metal plate is arranged between the inner surface of the graphite mold and the zirconium-based alloy powder, the surface of the metal plate is sprayed with boron nitride coating, and then the whole is placed in a hot pressing sintering furnace for hot pressing sintering. The hot pressing sintering temperature is 1000° C., the pressure is 40 MPa, and the heat preservation and pressure holding time is 5 hours. After the hot pressing sintering is completed, the temperature and pressure are reduced, and the temperature and pressure are reduced by furnace cooling and gradient pressure reduction. The machining includes wire cutting and grinding. The wire cutting cuts the zirconium-based alloy target blank to the finished product size. The grinding uses a grinder to grind the surface of the zirconium-based alloy target blank to obtain a zirconium-vanadium-iron alloy target.

[0072] In this embodiment, the above method is used to prepare a zirconium-vanadium-iron alloy target, and the density of the target reaches 99.0%. It is used to prepare a getter film, and the activation temperature of the getter film is low, and it can be used at room temperature, and has excellent getter performance.

[0073] Embodiment 3:

[0074] This embodiment provides a method for preparing a zirconium-based alloy target, and the preparation method comprises the following steps:

[0075] (1) adding 3N zirconium sponge, 3N5 vanadium particles and 3N5 electrolytic iron in a proportion of 80 wt%, 15 wt% and 5 wt% by mass into a smelting furnace, and performing vacuum smelting in an argon protective atmosphere at a temperature of 1500° C. After the raw materials are completely melted, they are mechanically stirred for 3 minutes, and cooled to room temperature with the furnace under the condition of continuous introduction of protective argon gas to obtain a zirconium-based alloy ingot;

[0076] (2) placing the zirconium-based alloy ingot obtained in step (1) in an atomizing furnace and heating it to 1500° C. to completely melt it, wherein the atmosphere in the atomizing furnace is argon gas, and then using a nozzle to spray argon gas on the alloy melt to atomize it into powder, wherein the diameter of the nozzle is 4 mm, to obtain a zirconium-based alloy powder, and the zirconium-based alloy powder is sieved through a 90-mesh sieve and the sieve residue is taken;

[0077] (3) The zirconium-based alloy powder screened in step (2) is first loaded into a graphite mold and then evacuated, a stainless steel metal plate is arranged between the inner surface of the graphite mold and the zirconium-based alloy powder, the surface of the metal plate is sprayed with boron nitride coating, and then the whole is placed in a hot pressing sintering furnace for hot pressing sintering, the hot pressing sintering temperature is 1200° C., the pressure is 30 MPa, and the heat preservation and pressure holding time is 3 hours. After the hot pressing sintering is completed, the temperature and pressure are reduced, and the temperature and pressure are reduced by furnace cooling, and the pressure is reduced by gradient pressure reduction, and then machining is performed, and the machining includes wire cutting and grinding. The wire cutting cuts the zirconium-based alloy target blank to the finished product size, and the grinding uses a grinder to grind the surface of the zirconium-based alloy target blank to obtain a zirconium-vanadium-iron alloy target.

[0078] In this embodiment, the above method is used to prepare a zirconium-vanadium-iron alloy target, and the density of the target reaches 98.7%. It is used to prepare a getter film, and the activation temperature of the getter film is low, and it can be used at room temperature, and has excellent getter performance.

[0079] Embodiment 4:

[0080] This embodiment provides a method for preparing a zirconium-based alloy target, and the preparation method comprises the following steps:

[0081] (1) adding nuclear-grade zirconium with a purity of 3N5, vanadium particles with a purity of 4N, and electrolytic iron with a purity of 3N into a smelting furnace in a ratio of 65wt%, 29wt%, and 6wt%, respectively, and performing vacuum smelting in a neon protective atmosphere at a temperature of 1450° C. After the raw materials are completely melted, they are mechanically stirred for 4 minutes, and cooled to room temperature with the furnace under the condition of continuous introduction of neon protective gas to obtain a zirconium-based alloy ingot;

[0082] (2) placing the zirconium-based alloy ingot obtained in step (1) in an atomizing furnace and heating it to 1480° C. to completely melt it, wherein the atmosphere in the atomizing furnace is neon gas, and then spraying neon gas on the alloy melt through a nozzle to atomize it into powder, wherein the diameter of the nozzle is 3.5 mm, to obtain zirconium-based alloy powder, and sieving the zirconium-based alloy powder through a 125-mesh sieve and taking the sieve residue;

[0083] (3) The zirconium-based alloy powder screened in step (2) is first loaded into a graphite mold and then evacuated; a titanium metal plate is arranged between the inner surface of the graphite mold and the zirconium-based alloy powder, the surface of the metal plate is sprayed with boron nitride coating, and then the whole is placed in a hot pressing sintering furnace for hot pressing sintering. The hot pressing sintering temperature is 950° C., the pressure is 40 MPa, and the heat preservation and pressure holding time is 4.5 h. After the hot pressing sintering is completed, the temperature and pressure are reduced, and the temperature and pressure are reduced by furnace cooling and gradient pressure reduction. The machining includes wire cutting and grinding. The wire cutting cuts the zirconium-based alloy target blank to the finished product size. The grinding uses a grinder to grind the surface of the zirconium-based alloy target blank to obtain a zirconium-vanadium-iron alloy target.

[0084] In this embodiment, the above method is used to prepare a zirconium-vanadium-iron alloy target, and the density of the target reaches 98.6%. It is used to prepare a getter film, and the activation temperature of the getter film is low, and it can be used at room temperature, and has excellent getter performance.

[0085] Embodiment 5:

[0086] This embodiment provides a method for preparing a zirconium-based alloy target, and the preparation method comprises the following steps:

[0087] (1) adding 2N8 nuclear grade zirconium, 3N8 vanadium particles and 3N8 electrolytic iron in a proportion of 62wt%, 30wt% and 8wt% by mass into a smelting furnace, and performing vacuum smelting in an argon protective atmosphere at a temperature of 1350° C., mechanically stirring for 6 minutes after the raw materials are completely melted, and cooling to room temperature with the furnace under the condition of continuous introduction of protective argon gas to obtain a zirconium-based alloy ingot;

[0088] (2) placing the zirconium-based alloy ingot obtained in step (1) in an atomizing furnace and heating it to 1430° C. to completely melt it, wherein the atmosphere in the atomizing furnace is argon gas, and then spraying argon gas on the alloy melt through a nozzle to atomize it into powder, wherein the diameter of the nozzle is 2.5 mm, to obtain zirconium-based alloy powder, and sieving the zirconium-based alloy powder through a 75-mesh sieve and taking the sieve residue;

[0089] (3) The zirconium-based alloy powder screened in step (2) is first loaded into a graphite mold and then evacuated; a titanium alloy metal plate is arranged between the inner surface of the graphite mold and the zirconium-based alloy powder, the surface of the metal plate is sprayed with boron nitride coating, and then the whole is placed in a hot pressing sintering furnace for hot pressing sintering. The hot pressing sintering temperature is 1050° C., the pressure is 38 MPa, and the heat preservation and pressure holding time is 3.5 h. After the hot pressing sintering is completed, the temperature and pressure are reduced, and the temperature and pressure are reduced by furnace cooling and gradient pressure reduction. The machining includes wire cutting and grinding. The wire cutting cuts the zirconium-based alloy target blank to the finished product size. The grinding uses a grinder to grind the surface of the zirconium-based alloy target blank to obtain a zirconium-vanadium-iron alloy target.

[0090] In this embodiment, the above method is used to prepare a zirconium-vanadium-iron alloy target, and the density of the target reaches 98.8%. It is used to prepare a getter film, and the activation temperature of the getter film is low, and it can be used at room temperature, and has excellent getter performance.

[0091] Embodiment 6:

[0092] This embodiment provides a method for preparing a zirconium-based alloy target. The preparation method refers to the method in Embodiment 3, except that in step (1), the mass fractions of zirconium, vanadium and iron are 90 wt%, 5 wt% and 5 wt% respectively.

[0093] In this embodiment, since the zirconium content in the target raw material is too high and the vanadium content is too low, the prepared alloy target has a high gettering performance when used for getter film, but the activation temperature is still too high and cannot be used at room temperature.

[0094] Embodiment 7:

[0095] This embodiment provides a method for preparing a zirconium-based alloy target. The preparation method refers to the method in Embodiment 1, except that in step (1), the mass fractions of zirconium, vanadium and iron are 50 wt%, 30 wt% and 20 wt% respectively.

[0096] In this embodiment, since the zirconium content in the target material is too low and the vanadium and iron contents are too high, the getter performance of the prepared alloy target is reduced when used for a getter film.

[0097] Based on the above embodiments, it can be concluded that the method of the present invention first melts the target raw material to obtain an alloy, then breaks it into fine droplets by gas atomization, forms alloy powder after solidification, and then promotes contact and diffusion of powder particles by hot pressing and sintering, thereby obtaining a high-density, high-purity alloy target material with strong uniformity of grain structure and high purity of target material; the zirconium-based alloy target material prepared by the method is used to prepare a getter film with strong uniformity, and by controlling the alloy material and content, it is ensured that the activation temperature of the getter is low, it is easy to use, and has excellent getter performance; the method is simple to operate, low in cost, and easy to achieve mass production.

[0098] The applicant declares that the present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the method of the present invention, addition of auxiliary steps, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a zirconium-based alloy target, characterized in that: The preparation method comprises the following steps: (1) vacuum melting a target material including zirconium in a protective atmosphere, and obtaining a zirconium-based alloy ingot after cooling; (2) melting the zirconium-based alloy ingot obtained in step (1) and then atomizing it to obtain a zirconium-based alloy powder; (3) The zirconium-based alloy powder obtained in step (2) is hot-pressed and sintered, and then machined to obtain a zirconium-based alloy target.

2. The preparation method according to claim 1, characterized in that: The zirconium-based alloy target material includes a zirconium-vanadium-iron alloy target material; Preferably, the mass fraction of zirconium in the target material of step (1) is 60-80wt%; Preferably, the zirconium element in step (1) comprises sponge zirconium or nuclear grade zirconium, and its purity is 2N5 or above; Preferably, when the zirconium-based alloy is zirconium-vanadium-iron alloy, the mass fraction of the vanadium raw material in the target raw material is 15-30wt%, and the mass fraction of the iron raw material is 5-10wt%; Preferably, the iron raw material comprises electrolytic iron, and its purity is 3N or above; Preferably, the vanadium raw material comprises vanadium particles, and the purity of the vanadium particles is above 3N.

3. The preparation method according to claim 1 or 2, characterized in that: The smelting in step (1) is carried out in a smelting furnace; Preferably, the protective gas in step (1) comprises an inert gas; Preferably, the temperature of the vacuum melting in step (1) is 1300-1500° C.; Preferably, in step (1), the target material is mechanically stirred after being completely melted; Preferably, the mechanical stirring time is 3 to 8 minutes; Preferably, the cooling method in step (1) is furnace cooling, and cooling to room temperature under the condition of continuous introduction of protective gas.

4. The preparation method according to any one of claims 1 to 3, characterized in that Step (2) The zirconium-based alloy ingot is placed in an atomizing furnace to heat, melt and atomize; Preferably, in step (2), the zirconium-based alloy ingot is heated to 1400-1500° C. and completely melted; Preferably, the atmosphere in the atomization furnace is a protective gas.

5. The preparation method according to any one of claims 1 to 4, characterized in that: In step (2), the gas atomization adopts a nozzle to spray an inert gas onto the alloy melt; Preferably, the diameter of the nozzle is 2 to 4 mm; Preferably, the alloy melt is atomized to form powder, and then the temperature is continuously lowered to room temperature; Preferably, in step (2), the zirconium-based alloy powder is sieved and the sieve residue is taken; Preferably, the size of the mesh holes in the sieve used for the screening is 75-125 meshes.

6. The preparation method according to any one of claims 1 to 5, characterized in that: Step (3) The zirconium-based alloy powder is first loaded into a mold, and then the whole is placed in a hot pressing sintering furnace; Preferably, the mold comprises a graphite mold, a metal plate is arranged between the inner surface of the mold and the zirconium-based alloy powder, and a coating is sprayed on the surface of the metal plate; Preferably, the material of the metal plate includes any one of stainless steel, titanium or titanium alloy, and the coating includes boron nitride coating; Preferably, the zirconium-based alloy powder is placed in a mold and then vacuumed.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The temperature of the hot pressing sintering in step (3) is 950-1200° C. Preferably, the pressure of the hot pressing sintering in step (3) is 30-40 MPa; Preferably, the heat preservation and pressure holding time of the hot pressing sintering in step (3) is 3 to 5 hours; Preferably, after the hot pressing sintering in step (3) is completed, the temperature and pressure are lowered, and the temperature is lowered along with the furnace, and the pressure is lowered by gradient pressure reduction.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The machining in step (3) includes wire cutting and grinding; Preferably, the wire cutting cuts the zirconium-based alloy target blank into finished product size; Preferably, the grinding process uses a grinder to grind the surface of the zirconium-based alloy target blank flat.

9. The zirconium-based alloy target obtained by the preparation method according to any one of claims 1 to 8.

10. The use of the zirconium-based alloy target material according to claim 9, characterized in that: The zirconium-based alloy target is used for preparing a getter film.

Citation Information

Patent Citations

  • Preparation method of aluminum-scandium alloy target material

    CN111647858A