Corrosion-resistant antibacterial stainless steel material and preparation process thereof
Through magnetron sputtering and electroplating technology, Ni-Fe-P coating is formed on stainless steel materials, and combined with antibacterial coating, the problems of insufficient binding force of the plating and environmental pollution in the existing technology are solved, and corrosion resistance and antibacterial properties are achieved It has both environmental protection.
Patent Information
- Application Number
- CN202411020497.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the preparation of corrosion-resistant and antibacterial stainless steel materials, the binding force of the coating or coating is insufficient, resulting in a degradation of performance and environmental pollution problems, making it difficult to meet the requirements of antibacterial, corrosion resistance and environmental protection at the same time.
Magneto-controlled sputtering technology is used to coat the Ni-Fe metal layer on the surface of stainless steel material, and electroplating is carried out on the basis of the Ni-Fe-P metal layer, combined with spraying antibacterial coatings, and corrosion-resistant antibacterial agents in the antibacterial emulsion and Fluoropolymers improve antibacterial properties and wear resistance, controlling the thickness of the coating and the amount of coating sprayed.
The Ni-Fe metal layer and stainless steel material have a strong interface force, which improves corrosion resistance, hardness and toughness, reduces the residual stress of the coating, obtains a coating with excellent performance, and significantly improves the antibacterial properties and The dirt release performance solves the problems of performance degradation and environmental pollution.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of metal material plating, and specifically discloses a corrosion-resistant and antibacterial stainless steel material and a preparation process thereof. Background Art
[0002] Stainless steel has excellent mechanical properties and good chemical stability, and is widely used in building structures, kitchenware manufacturing, medical equipment manufacturing, automotive industry, etc. Although stainless steel has a certain corrosion resistance, it still needs to be improved, and some industries require stainless steel to have both corrosion resistance and antibacterial properties.
[0003] The existing technology for preparing corrosion-resistant and antibacterial stainless steel mostly adopts plating, coating and other processes, but there are problems such as environmental pollution, performance needs to be improved, and poor bonding between the plating / coating resulting in performance degradation; therefore, it is of great significance to study a corrosion-resistant and antibacterial stainless steel material with good antibacterial properties, good corrosion resistance and less environmental pollution and its preparation process. Summary of the invention
[0004] The object of the present invention is to provide a corrosion-resistant and antibacterial stainless steel material and a preparation process thereof, so as to solve the problems raised in the above-mentioned background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: A preparation process of a corrosion-resistant and antibacterial stainless steel material: comprising the following steps: S1: taking a stainless steel material, cleaning it, and using a magnetron sputtering process to plate a Ni-Fe metal layer on the surface of the stainless steel material to obtain a stainless steel material A; S2: Placing the stainless steel material A in an electroplating solution for electroplating to coat a Ni-Fe-P metal layer to obtain a corrosion-resistant and antibacterial stainless steel material.
[0006] The electroplating solution includes the following raw materials: 0.5-0.8 g / L graphene oxide, 0.2-0.5 g / L dodecylphenol polyoxyethylene ether, 3.5-4 g / L isothiourea propyl sulfuric acid, 180-200 g / L nickel sulfate, 20-25 g / L ferric sulfate, 30-35 g / L phosphorous acid, 25-30 g / L boric acid, and the rest is water.
[0007] More optimally, the thickness of the Ni-Fe metal layer in step S1 is 0.1-0.15 μm; the electroplating process in step S2 is: at a temperature of 45-50° C., a current density of 2-3 A / min, and electroplating for 380-400 seconds.
[0008] More optimally, in step S2, the stainless steel material A is placed in an electroplating solution for electroplating to coat a Ni-Fe-P metal layer; an antibacterial coating is coated on its surface and dried to obtain an antibacterial coating; a corrosion-resistant and antibacterial stainless steel material is obtained; and the spraying amount is 1.8-2 g / m 2 .
[0009] More optimally, step 1: take a corrosion-resistant antibacterial agent, acryloyloxyethyl trimethyl ammonium chloride, styrene, butyl acrylate, acrylic acid, and water, add an emulsifier, stir evenly, and obtain an emulsion; add benzoyl peroxide, stir evenly, react at 80-85°C for 4-5 hours, and filter with a 150-mesh stainless steel filter to obtain an antibacterial emulsion; Step 2: Add the antibacterial emulsion into water and dilute it to obtain an antibacterial coating with a solid content of 10-15wt%.
[0010] More optimally, the antibacterial emulsion comprises the following raw materials, by mass: 40-45 parts of corrosion-resistant antibacterial agent, 20-25 parts of acryloyloxyethyl trimethyl ammonium chloride, 100-110 parts of styrene, 100-110 parts of butyl acrylate, 15-20 parts of acrylic acid, 800-850 parts of water, and 15-23 parts of emulsifier; The emulsifier includes 10-15 parts of Tween 80 and 5-8 parts of hexadecyltrimethylammonium bromide by weight; The amount of benzoyl peroxide added is 1% of the mass of the emulsion; More optimally, the preparation of the corrosion-resistant antibacterial agent includes the following steps: Step 1: adding epigallocatechin gallate, 3-bromo-1-propylene and sodium carbonate to tetrahydrofuran, mixing evenly, reacting at 50-60° C. for 3-5 hours, and removing the solvent to obtain intermediate A; Step 2: Take intermediate A, 2,4-difluorophenyl isocyanate, and dodecyl isocyanate, add a mixed solvent of tetrahydrofuran and benzene, stir evenly, and react at 50-60° C. for 3-4 hours to obtain a corrosion-resistant antibacterial agent.
[0011] More optimally, in step 1, the molar ratio of epigallocatechin gallate, 3-bromo-1-propylene, and sodium carbonate is 1:2:(2-2.1), and the amount of tetrahydrofuran added is 12 times that of epigallocatechin gallate; In step 2, the mass ratio of intermediate A, 2,4-difluorophenyl isocyanate, and dodecyl isocyanate is (6-7): (1.2-1.5): (2-2.2); the mixed solvent of tetrahydrofuran and benzene includes tetrahydrofuran and benzene in a volume ratio of 2:1, and the amount of the mixed solvent added is 12 times the mass of intermediate A.
[0012] More optimally, after spraying the antibacterial coating, the specific drying process is: drying at 100-110°C for 1-2 minutes, and placing at room temperature for 1-1.5 hours to obtain the antibacterial coating.
[0013] More optimally, after spraying the antibacterial coating, the specific drying process is: drying at 110°C for 1 minute and leaving at room temperature for 1.5 hours to obtain the antibacterial coating.
[0014] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: a stainless steel material is firstly obtained, a Ni-Fe metal layer is firstly obtained on the surface of the stainless steel material by magnetron sputtering, and then a Ni-Fe-P metal layer is obtained by electroplating; the Ni-Fe metal layer has a strong interface force with the stainless steel material and has excellent ductility and toughness, and the magnetron sputtering technology used here can obtain a thin, uniform and dense metal layer, which is suitable as a base layer; the Ni-Fe-P metal layer obtained by electroplating contains P element, which greatly improves the corrosion resistance, hardness and wear resistance; at the same time, electroplating after magnetron sputtering can reduce the residual stress of the magnetron sputtering layer, and obtain a coating with excellent performance; The surface of the corrosion-resistant and antibacterial stainless steel material is sprayed with an antibacterial coating, which includes an antibacterial emulsion and water. The antibacterial emulsion is obtained by polymerization of a corrosion-resistant and antibacterial agent, acryloyloxyethyl trimethyl ammonium chloride, styrene, butyl acrylate, and acrylic acid. The corrosion-resistant and antibacterial agent is based on antibacterial catechin gallate, which is modified to contain double bonds that can participate in copolymerization reactions. A certain amount of 2,4-difluorophenyl isocyanate and dodecyl isocyanate are introduced. Fluorine is introduced into 2,4-difluorophenyl isocyanate to form a fluorine-containing polymer. The compound has unique hydrophobicity, chemical stability and biological inertness, and can peel off the bacteria attached to the surface from the surface under the action of low shear force, so it has excellent dirt release performance; dodecyl isocyanate contains long alkyl chains, which play a plasticizing role and improve the performance of the antibacterial coating; the corrosion-resistant antibacterial agent works together with acryloyloxyethyltrimethylammonium chloride to produce an antibacterial coating with good toughness and good antibacterial properties; the amount of corrosion-resistant antibacterial agent added needs to be controlled, too little will lead to a decrease in the antibacterial effect, and too much will lead to greater steric hindrance during the copolymerization reaction. DETAILED DESCRIPTION
[0015] The following is a preferred implementation of the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. For ordinary technicians in this technical field, all other embodiments obtained by ordinary technicians in this field without creative work without departing from the principle of the embodiment of the present invention are within the scope of protection of the present invention.
[0016] The following parts are by mass unless otherwise specified; Example 1: S1: Add epigallocatechin gallate, 3-bromo-1-propylene and sodium carbonate into tetrahydrofuran and mix them evenly. At a speed of 200 r / min and a temperature of 60° C., react for 4 hours, remove the solvent, and obtain intermediate A. The molar ratio of epigallocatechin gallate, 3-bromo-1-propylene and sodium carbonate is 1:2:2.1. Take intermediate A, 2,4-difluorophenyl isocyanate, and dodecyl isocyanate, add a mixed solvent of tetrahydrofuran and benzene, stir evenly, and react at 60° C. for 4 hours to obtain a corrosion-resistant antibacterial agent; the mass ratio of intermediate A, 2,4-difluorophenyl isocyanate, and dodecyl isocyanate is 6.5:1.3:2; Take 42 parts of corrosion-resistant antibacterial agent, 22 parts of acryloyloxyethyl trimethyl ammonium chloride, 100 parts of styrene, 110 parts of butyl acrylate, 18 parts of acrylic acid, 800 parts of water, add 12 parts of Tween 80 and 6 parts of hexadecyl trimethyl ammonium bromide, stir evenly to obtain an emulsion, add 1% of benzoyl peroxide by mass of the emulsion, stir evenly, react at 80°C for 5h, filter with a 150-mesh stainless steel filter to obtain an antibacterial emulsion; dilute with water to a solid content of 10wt% to obtain an antibacterial coating; S2: Take the stainless steel material, ultrasonically clean it in acetone for 20 minutes, rinse it with water, ultrasonically clean it in 3wt% sodium hydroxide for 15 minutes, ultrasonically clean it in 5wt% sulfuric acid for 15 minutes, and rinse it with water; in an external magnetic field of 4T, a sputtering power of 50W, a deposition rate of 0.04nm / s, and a Ni-Fe10at% alloy target, magnetron sputtering is performed to obtain a stainless steel material A with a Ni-Fe metal layer of 0.1μm on the surface; The stainless steel material A is placed in the electroplating solution for plating: the temperature is 50°C, the current density is 3A / min, the electroplating time is 390 seconds, and the Ni-Fe-P metal layer is plated; the antibacterial coating is coated on the surface, and the spraying amount is 2g / m 2 , drying to obtain an antibacterial coating; obtaining a corrosion-resistant and antibacterial stainless steel material; Plating solution: 0.8g / L graphene oxide, 0.25g / L dodecylphenol polyoxyethylene ether, 3.75g / L isothiourea propyl sulfate, 190g / L nickel sulfate, 22g / L ferrous sulfate, 32g / L phosphorous acid, 28g / L boric acid.
[0017] Example 2: S1: Add epigallocatechin gallate, 3-bromo-1-propylene and sodium carbonate into tetrahydrofuran and mix well. At a speed of 200 r / min and a temperature of 50° C., react for 5 h, remove the solvent, and obtain intermediate A. The molar ratio of epigallocatechin gallate, 3-bromo-1-propylene and sodium carbonate is 1:2:2. Take intermediate A, 2,4-difluorophenyl isocyanate, and dodecyl isocyanate, add a mixed solvent of tetrahydrofuran and benzene, stir evenly, and react at 60° C. for 3 hours to obtain a corrosion-resistant antibacterial agent; the mass ratio of intermediate A, 2,4-difluorophenyl isocyanate, and dodecyl isocyanate is 6.5:1.3:2; Take 40 parts of corrosion-resistant antibacterial agent, 25 parts of acryloyloxyethyl trimethyl ammonium chloride, 110 parts of styrene, 110 parts of butyl acrylate, 15 parts of acrylic acid, 800 parts of water, add 10 parts of Tween 80 and 8 parts of hexadecyl trimethyl ammonium bromide, stir evenly to obtain an emulsion, add 1% of benzoyl peroxide by mass of the emulsion, stir evenly, react at 80°C for 5h, filter with a 150-mesh stainless steel filter to obtain an antibacterial emulsion; dilute with water to a solid content of 10wt% to obtain an antibacterial coating; S2: Take stainless steel material, ultrasonically clean it in acetone for 20 minutes, rinse it with water, ultrasonically clean it in 3wt% sodium hydroxide for 15 minutes, and ultrasonically clean it in 5wt% sulfuric acid for 15 minutes, and rinse it with water; in an external magnetic field of 4T, a sputtering power of 50W, a deposition rate of 0.04nm / s, and Ni-Fe10at% as an alloy target, magnetron sputtering is performed to obtain stainless steel material A with a 0.1μm Ni-Fe metal layer on the surface; stainless steel material A is placed in an electroplating solution for coating: at a temperature of 50°C, a current density of 2A / min, electroplating for 400 seconds, and a Ni-Fe-P metal layer is plated; antibacterial coating is coated on its surface with a spraying amount of 2g / m 2 , drying to obtain an antibacterial coating; obtaining a corrosion-resistant and antibacterial stainless steel material; Plating solution: 0.5~0.8g / L graphene oxide, 0.25g / L dodecylphenol polyoxyethylene ether, 3.75g / L isothiourea propyl sulfuric acid, 200g / L nickel sulfate, 25g / L ferrous sulfate, 30g / L phosphorous acid, 30g / L boric acid.
[0018] Example 3: S1: Add epigallocatechin gallate, 3-bromo-1-propylene and sodium carbonate into tetrahydrofuran and mix well. At a speed of 200 r / min and a temperature of 60° C., react for 3 h, remove the solvent, and obtain intermediate A. The molar ratio of epigallocatechin gallate, 3-bromo-1-propylene and sodium carbonate is 1:2:2.1. Take intermediate A, 2,4-difluorophenyl isocyanate, and dodecyl isocyanate, add a mixed solvent of tetrahydrofuran and benzene, stir evenly, and react at 50° C. for 4 hours to obtain a corrosion-resistant antibacterial agent; the mass ratio of intermediate A, 2,4-difluorophenyl isocyanate, and dodecyl isocyanate is 6.5:1.3:2; Take 45 parts of corrosion-resistant antibacterial agent, 20 parts of acryloyloxyethyl trimethyl ammonium chloride, 110 parts of styrene, 100 parts of butyl acrylate, 20 parts of acrylic acid, 800 parts of water, add 15 parts of Tween 80 and 5 parts of hexadecyl trimethyl ammonium bromide, stir evenly to obtain an emulsion, add 1% of benzoyl peroxide by mass of the emulsion, stir evenly, react at 85°C for 5h, filter with a 150-mesh stainless steel filter to obtain an antibacterial emulsion; dilute with water to a solid content of 10wt% to obtain an antibacterial coating; S2: Take stainless steel material, ultrasonically clean it in acetone for 20 minutes, rinse it with water, ultrasonically clean it in 3wt% sodium hydroxide for 15 minutes, and ultrasonically clean it in 5wt% sulfuric acid for 15 minutes, and rinse it with water; in an external magnetic field of 4T, a sputtering power of 50W, a deposition rate of 0.04nm / s, and a Ni-Fe10at% alloy target, magnetron sputtering is performed to obtain a stainless steel material A with a 0.1μm Ni-Fe metal layer on the surface; stainless steel material A is placed in an electroplating solution for coating: at a temperature of 50°C, a current density of 3A / min, electroplating for 380 seconds, and a Ni-Fe-P metal layer is plated; an antibacterial coating is coated on its surface, and the spraying amount is 2g / m 2 , drying to obtain an antibacterial coating; obtaining a corrosion-resistant and antibacterial stainless steel material; Plating solution: 0.5g / L graphene oxide, 0.25g / L dodecylphenol polyoxyethylene ether, 3.75g / L isothiourea propyl sulfate, 180g / L nickel sulfate, 25g / L ferrous sulfate, 35g / L phosphorous acid, 25g / L boric acid.
[0019] Comparative Example 1 (directly plating a Ni-Fe-P metal layer on the surface of a stainless steel material, and the remaining method steps are consistent with Example 1): Take a stainless steel material, ultrasonically clean it in acetone for 20 minutes, rinse it with water, ultrasonically clean it in 3wt% sodium hydroxide for 15 minutes, and ultrasonically clean it in 5wt% sulfuric acid for 15 minutes, rinse it with water, place it in an electroplating solution, and carry out plating: at a temperature of 50°C, a current density of 3A / min, electroplating for 390 seconds, and plating a Ni-Fe-P metal layer; apply an antibacterial coating on its surface, with a spraying amount of 2g / m2, and dry it to obtain an antibacterial coating; obtain a corrosion-resistant and antibacterial stainless steel material.
[0020] Comparative Example 2 (the addition amount of each raw material of the corrosion-resistant antibacterial agent was changed, and the other method steps were consistent with Example 1): S1: Take a stainless steel material, ultrasonically clean it in acetone for 20 minutes, rinse it with water, ultrasonically clean it in 3wt% sodium hydroxide for 15 minutes, and ultrasonically clean it in 5wt% sulfuric acid for 15 minutes, and rinse it with water; in an external magnetic field of 4T, a sputtering power of 50W, a deposition rate of 0.04nm / s, Ni-Fe10at% is used as an alloy target, and magnetron sputtering is performed to obtain a stainless steel material A with a Ni-Fe metal layer of 0.1μm on the surface; S2: stainless steel material A is placed in the electroplating solution for plating: at a temperature of 50°C, a current density of 3A / min, electroplating for 390 seconds, and a Ni-Fe-P metal layer is plated; an antibacterial coating is applied on its surface with a spraying amount of 2g / m 2 , drying to obtain an antibacterial coating; obtaining a corrosion-resistant and antibacterial stainless steel material; Plating solution: 0.8g / L graphene oxide, 0.25g / L dodecylphenol polyoxyethylene ether, 3.75g / L isothiourea propyl sulfate, 190g / L nickel sulfate, 22g / L ferrous sulfate, 32g / L phosphorous acid, 28g / L boric acid; The preparation of the antibacterial coating comprises the following steps: step 1: adding epigallocatechin gallate, 3-bromo-1-propylene and sodium carbonate into tetrahydrofuran and mixing them evenly, reacting them for 4 hours at a speed of 200 r / min and a temperature of 60° C., removing the solvent, and obtaining an intermediate A; the molar ratio of epigallocatechin gallate, 3-bromo-1-propylene and sodium carbonate is 1:2:2.1; Step 2: Take intermediate A, 2,4-difluorophenyl isocyanate, and dodecyl isocyanate, add a mixed solvent of tetrahydrofuran and benzene, stir evenly, and react at 60° C. for 4 hours to obtain a corrosion-resistant antibacterial agent; the mass ratio of intermediate A, 2,4-difluorophenyl isocyanate, and dodecyl isocyanate is 6:2:4; Step 3: Take 42 parts of corrosion-resistant antibacterial agent, 22 parts of acryloyloxyethyl trimethyl ammonium chloride, 100 parts of styrene, 110 parts of butyl acrylate, 18 parts of acrylic acid, 800 parts of water, add 12 parts of Tween 80 and 6 parts of hexadecyl trimethyl ammonium bromide, stir evenly to obtain an emulsion, add 1% of the mass of the emulsion benzoyl peroxide, stir evenly, react at 80°C for 5h, filter with a 150-mesh stainless steel filter to obtain an antibacterial emulsion; dilute with water to a solid content of 10wt% to obtain an antibacterial coating.
[0021] Comparative Example 3 (the amount of each raw material added in the antibacterial emulsion was changed, and the other method steps were consistent with Example 1): S1: Take a stainless steel material, ultrasonically clean it in acetone for 20 minutes, rinse it with water, ultrasonically clean it in 3wt% sodium hydroxide for 15 minutes, and ultrasonically clean it in 5wt% sulfuric acid for 15 minutes, and rinse it with water; in an external magnetic field of 4T, a sputtering power of 50W, a deposition rate of 0.04nm / s, Ni-Fe10at% is used as an alloy target, and magnetron sputtering is performed to obtain a stainless steel material A with a Ni-Fe metal layer of 0.1μm on the surface; S2: placing stainless steel material A in an electroplating solution for plating: at a temperature of 50°C, a current density of 3A / min, electroplating for 390 seconds, plating a Ni-Fe-P metal layer; coating the surface with an antibacterial coating at a spraying amount of 2g / m2, drying, and obtaining an antibacterial coating; obtaining a corrosion-resistant and antibacterial stainless steel material; Plating solution: 0.8g / L graphene oxide, 0.25g / L dodecylphenol polyoxyethylene ether, 3.75g / L isothiourea propyl sulfate, 190g / L nickel sulfate, 22g / L ferrous sulfate, 32g / L phosphorous acid, 28g / L boric acid; The preparation of the antibacterial coating comprises the following steps: step 1: adding epigallocatechin gallate, 3-bromo-1-propylene and sodium carbonate into tetrahydrofuran and mixing them evenly, reacting them for 4 hours at a speed of 200 r / min and a temperature of 60° C., removing the solvent, and obtaining an intermediate A; the molar ratio of epigallocatechin gallate, 3-bromo-1-propylene and sodium carbonate is 1:2:2.1; Step 2: Take intermediate A, 2,4-difluorophenyl isocyanate, and dodecyl isocyanate, add a mixed solvent of tetrahydrofuran and benzene, stir evenly, and react at 60° C. for 4 hours to obtain a corrosion-resistant antibacterial agent; the mass ratio of intermediate A, 2,4-difluorophenyl isocyanate, and dodecyl isocyanate is 6.5:1.3:2; Step 3: Take 32 parts of corrosion-resistant antibacterial agent, 32 parts of acryloyloxyethyl trimethyl ammonium chloride, 100 parts of styrene, 120 parts of butyl acrylate, 8 parts of acrylic acid, 800 parts of water, add 12 parts of Tween 80 and 6 parts of hexadecyl trimethyl ammonium bromide, stir evenly to obtain an emulsion, add 1% of the mass of the emulsion benzoyl peroxide, stir evenly, react at 80°C for 5h, filter with a 150-mesh stainless steel filter to obtain an antibacterial emulsion; dilute with water to a solid content of 10wt% to obtain an antibacterial coating.
[0022] Comparative Example 4 (the amount of each raw material added in the antibacterial emulsion was changed, and the other method steps were consistent with Example 1): S1: Take a stainless steel material, ultrasonically clean it in acetone for 20 minutes, rinse it with water, ultrasonically clean it in 3wt% sodium hydroxide for 15 minutes, and ultrasonically clean it in 5wt% sulfuric acid for 15 minutes, and rinse it with water; in an external magnetic field of 4T, a sputtering power of 50W, a deposition rate of 0.04nm / s, Ni-Fe10at% is used as an alloy target, and magnetron sputtering is performed to obtain a stainless steel material A with a Ni-Fe metal layer of 0.1μm on the surface; S2: placing stainless steel material A in an electroplating solution for plating: at a temperature of 50°C, a current density of 3A / min, electroplating for 390 seconds, plating a Ni-Fe-P metal layer; coating the surface with an antibacterial coating at a spraying amount of 2g / m2, drying, and obtaining an antibacterial coating; obtaining a corrosion-resistant and antibacterial stainless steel material; Plating solution: 0.8g / L graphene oxide, 0.25g / L dodecylphenol polyoxyethylene ether, 3.75g / L isothiourea propyl sulfate, 190g / L nickel sulfate, 22g / L ferrous sulfate, 32g / L phosphorous acid, 28g / L boric acid; The preparation of the antibacterial coating comprises the following steps: step 1: adding epigallocatechin gallate, 3-bromo-1-propylene and sodium carbonate into tetrahydrofuran and mixing them evenly, reacting them for 4 hours at a speed of 200 r / min and a temperature of 60° C., removing the solvent, and obtaining an intermediate A; the molar ratio of epigallocatechin gallate, 3-bromo-1-propylene and sodium carbonate is 1:2:2.1; Step 2: Take intermediate A, 2,4-difluorophenyl isocyanate, and dodecyl isocyanate, add a mixed solvent of tetrahydrofuran and benzene, stir evenly, and react at 60° C. for 4 hours to obtain a corrosion-resistant antibacterial agent; the mass ratio of intermediate A, 2,4-difluorophenyl isocyanate, and dodecyl isocyanate is 6.5:1.3:2; Step 3: Take 52 parts of corrosion-resistant antibacterial agent, 12 parts of acryloyloxyethyl trimethyl ammonium chloride, 100 parts of styrene, 110 parts of butyl acrylate, 18 parts of acrylic acid, 800 parts of water, add 12 parts of Tween 80 and 6 parts of hexadecyl trimethyl ammonium bromide, stir evenly to obtain an emulsion, add 1% of the mass of the emulsion benzoyl peroxide, stir evenly, react at 80°C for 5h, filter with a 150-mesh stainless steel filter to obtain an antibacterial emulsion; dilute with water to a solid content of 10wt% to obtain an antibacterial coating.
[0023] In the above examples, the test methods used are conventional methods unless otherwise specified; the raw materials used are commercially available unless otherwise specified, and the sources of the raw materials are as follows: tetrahydrofuran (CAS: 109-99-9); graphene oxide (Kramer 180110132754); acetone (CAS: 67-64-1); dodecylphenol polyoxyethylene ether (12D-4, Xingtai Xinlanxing Technology Co., Ltd.); isothiourea propyl sulfate (CAS: 21668-81-5); nickel sulfate (CAS: 7786-81-4); ferrous sulfate (CAS: 10028-22-5); phosphorous acid (CAS: 13598-36-2); boric acid (CAS: 10043-35-3); epigallocatechin gallate (B20850, Shanghai Yuanye); 3-Bromo-1-propene (CAS: 106-95-6); sodium carbonate (CAS: 497-19-8); 2,4-difluorophenyl isocyanate (S48727, Shanghai Yuanye); dodecyl isocyanate (CAS: 4202-38-4); benzene (CAS: 71-43-2); acryloyloxyethyl trimethyl ammonium chloride (S26077, Shanghai Yuanye); styrene (CAS: 100-42-5); butyl acrylate (CAS: 141-32-2); acrylic acid (CAS: 79-10-7); Tween 80 (CAS: 9005-65-6); hexadecyl trimethyl ammonium bromide (CAS: 57-09-0); benzoyl peroxide (CAS: 94-36-0); stainless steel material (316 stainless steel plate, thickness 3.0 mm).
[0024] Experiment: Take the corrosion-resistant and antibacterial stainless steel materials including antibacterial coatings prepared in Examples 1 to 3 and Comparative Examples 1 to 4; (1) perform antibacterial testing with reference to HG / T3950-2007; (2) immerse in a FeCl3 aqueous solution with a mass concentration of 20% for 1 h at a temperature of 30°C, and test the corrosion rate, corrosion rate (%) = (weight before corrosion - weight after corrosion) / (weight before corrosion) × 100%; (3) take a 150 mm × 20 mm sample and perform a tensile test with reference to GB / T 228.1; see the table below for specific data;
[0025] Conclusion: In comparative example 1, a Ni-Fe-P metal layer is directly plated on the surface of the stainless steel material, and the performance is reduced due to problems such as coating adhesion and stress; in comparative example 2, the amount of each raw material added of the corrosion-resistant antibacterial agent is changed, and the performance is not as good as that of the embodiment; in comparative example 3 and comparative example 4, the amount of each raw material added of the antibacterial emulsion is changed, which leads to a decrease in performance. It can be seen that the control of the amount of corrosion-resistant antibacterial agent and acryloyloxyethyltrimethylammonium chloride added is of great significance; in summary, the corrosion-resistant and antibacterial stainless steel material including the antibacterial coating prepared by the present invention has good antibacterial and corrosion resistance.
[0026] Finally, it should be noted that the above is only a preferred embodiment of the present invention, but the protection scope of this application is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the spirit and principle of the present invention and within the technical scope disclosed in this application should be included in the protection scope of this application; in the absence of conflict, the embodiments of this application and the features in the embodiments can be combined with each other. Therefore, the protection scope of this application shall be based on the protection scope of the claims.
Claims
1. A preparation process of a corrosion-resistant and antibacterial stainless steel material, characterized by: The following steps are involved: S1: Take a stainless steel material, clean it, and plate a Ni-Fe metal layer on its surface using a magnetron sputtering process to obtain a stainless steel material A; S2: Placing the stainless steel material A in an electroplating solution for electroplating to coat a Ni-Fe-P metal layer to obtain a corrosion-resistant and antibacterial stainless steel material.
2. The preparation process of a corrosion-resistant and antibacterial stainless steel material according to claim 1, characterized in that: The thickness of the Ni-Fe metal layer in step S1 is 0.1-0.15 μm.
3. The preparation process of a corrosion-resistant and antibacterial stainless steel material according to claim 1, characterized in that: The electroplating solution includes the following raw materials: 0.5~0.8g / L graphene oxide, 0.2~0.5g / L dodecylphenol polyoxyethylene ether, 3.5~4g / L isothiourea propyl sulfuric acid, 180~200g / L nickel sulfate, 20~25g / L ferrous sulfate, 30~35g / L phosphorous acid, 25~30g / L boric acid, and the rest is water; The electroplating process is as follows: temperature 45-50° C., current density 2-3 A / min, and electroplating time 380-400 seconds.
4. The preparation process of a corrosion-resistant and antibacterial stainless steel material according to claim 1, characterized in that: In step S2, the stainless steel material A is placed in an electroplating solution for electroplating to coat a Ni-Fe-P metal layer; an antibacterial coating is coated on its surface and dried to obtain an antibacterial coating; and a corrosion-resistant and antibacterial stainless steel material is obtained.
5. The preparation process of a corrosion-resistant and antibacterial stainless steel material according to claim 4 is characterized in that: The preparation of the antibacterial coating comprises the following steps: Take a corrosion-resistant antibacterial agent, acryloyloxyethyl trimethyl ammonium chloride, styrene, butyl acrylate, acrylic acid, and water, add an emulsifier, stir evenly, and obtain an emulsion; add benzoyl peroxide, stir evenly, react at 80-85°C for 4-5 hours, filter, and obtain an antibacterial emulsion; dilute with water to obtain an antibacterial coating with a solid content of 10-15wt%.
6. The preparation process of a corrosion-resistant and antibacterial stainless steel material according to claim 4, characterized in that: The coating amount of the antibacterial coating is 1.8-2 g / m 2 .
7. The preparation process of a corrosion-resistant and antibacterial stainless steel material according to claim 5, characterized in that: The antibacterial emulsion comprises the following raw materials, calculated by weight: 40-45 parts of corrosion-resistant antibacterial agent, 20-25 parts of acryloyloxyethyl trimethyl ammonium chloride, 100-110 parts of styrene, 100-110 parts of butyl acrylate, 15-20 parts of acrylic acid, 800-850 parts of water, and 15-23 parts of emulsifier.
8. The preparation process of the corrosion-resistant and antibacterial stainless steel material according to claim 5, characterized in that: The preparation of the corrosion-resistant antibacterial agent comprises the following steps: Step 1: adding epigallocatechin gallate, 3-bromo-1-propylene and sodium carbonate to tetrahydrofuran in sequence, mixing evenly, reacting at 50-60° C. for 3-5 hours, and removing the solvent to obtain an intermediate A; Step 2: Take intermediate A, 2,4-difluorophenyl isocyanate and dodecyl isocyanate and add them to a mixed solvent of tetrahydrofuran and benzene, stir evenly, and react at 50-60° C. for 3-4 hours to obtain a corrosion-resistant antibacterial agent.
9. The preparation process of the corrosion-resistant and antibacterial stainless steel material according to claim 8, characterized in that: The molar ratio of epigallocatechin gallate, 3-bromo-1-propylene, and sodium carbonate is 1:2:(2~2.1); The mass ratio of intermediate A, 2,4-difluorophenyl isocyanate and dodecyl isocyanate is (6~7):(1.2~1.5):(2~2.2).
10. The corrosion-resistant and antibacterial stainless steel material prepared according to the preparation process of the corrosion-resistant and antibacterial stainless steel material according to any one of claims 1 to 9.
Citation Information
Patent Citations
Stainless steel coating capable of efficiently resisting bacteria and fingerprints and preparation method thereof
CN112552728A
Special stainless steel spring steel wire for antibacterial and corrosion-resistant medical biopsy forceps
CN114539904A
Corrosion-resistant stainless steel band and processing technology thereof
CN115354272A
Processing technology of high-corrosion-resistance stainless steel band for battery shell
CN115369463A
Battery steel shell with surface plated with metal layer and processing technology of battery steel shell
CN115786913A
Cited By
Wear-resistant duplex stainless steel band and processing technology thereof
CN119287465A