Carbon-based catalyst for preparing ethanol through electrocatalytic reduction of CO2 as well as preparation method and application of carbon-based catalyst
By adjusting the metal ratio and calcination conditions, carbon-based catalysts were prepared, solving the problems of complex synthesis, high cost, and low efficiency of existing copper-based catalysts, and achieving the effect of highly efficient electrocatalytic reduction of CO2 to ethanol.
Patent Information
- Application Number
- CN202411041755.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
Existing copper-based catalysts for the electrocatalytic reduction of CO2 to ethanol suffer from problems such as complex synthesis, high cost, and low efficiency. In particular, the synthesis of nanomaterials is complicated, has low production efficiency, and poor selectivity of ethanol products.
A carbon-based catalyst was prepared by adjusting the metal ratio, calcination temperature, and melamine ratio. The specific steps included mixing coal, copper nitrate hexahydrate, and melamine, and calcining them at a certain temperature and time to form a Cu-C3H6N6-C catalyst, thereby enhancing the catalytic activity.
It achieves efficient ethanol production at a lower applied potential, with a Faraday efficiency of 70%, reducing production costs and simplifying the preparation process, making it suitable for commercial production.
Smart Images

Figure CN118957663A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electrochemical catalysis technology, and in particular to a method for electrocatalytic reduction of CO 2 A carbon-based catalyst for producing ethanol and a preparation method and application thereof. Background Art
[0002] The catalysts reported so far for producing ethanol are mainly various modified copper-based catalysts. Polyaniline (PANI) coating is applied to Cu nanoparticles for electrocatalytic reduction of CO 2 The FE of C2+ hydrocarbons obtained by RR can reach 80%, but the FE of ethanol is about 20%. 2 Se nanosheet arrays to regulate Cu sites and CO 2 The interaction between the reaction intermediates in the ER can produce ethanol with high selectivity, and the FE reaches 70.3% at -0.8V vs.RHE. The electrochemical reduction of hollow CuS nanotubes showed that the CuS nanotubes with rich δ+ (0<δ<1) types of Cu 2 S 1-x The catalyst has a 73.3% ethanol Faradaic efficiency at -0.3 V vs. RHE, and the ethanol Faradaic efficiency decreases slightly after 6 hours of reaction. 2 ER, the ethanol Faraday efficiency reached 42% at -0.74V vs.RHE. A certain document prepared a new CuSn-HAB catalyst with Sn...Cu asymmetric double sites by post-synthesis modification of Cu-HAB, and achieved 56% ethanol Faraday efficiency at -0.57V vs.RHE. Using commercial micron-sized copper powder and magnesium powder as raw materials, adding carbon black, a one-step method was used to directly react with H 2 / Ar calcined high-density ordered Cu 3 -Mg site (111) exposed nano Cu 2 Mg intermetallic compounds can achieve -600mA·cm -2 (i.e. -0.84Vvs.RHE) the Faraday efficiency of ethanol is about 76.2%, and after 15 hours the Faraday efficiency of ethanol remains at a relatively stable level. Other literature uses carbon dots rich in functional groups as precursors for catalyst synthesis, introduces F, O, and N atoms by means of the adjustable characteristics of the functional groups in the carbon dots, and synthesizes a series of CuN 2 O 1 The atomic-scale CuFONC catalyst with a Faradaic efficiency of 80.5% at -1.3 V vs. RHE can be used to generate a C 2The selectivity is about 47.8% for ethanol. 2 O as a precursor and hNCNC as a carrier to construct a highly dispersed CuOCu-N 4 Binuclear sites and Cu-N 4 The single-site Cu-based catalyst achieved an ethanol FE of 56.3% at a low applied potential of -0.3 V vs. RHE. In addition, a hydrophobic porous Cu with uniform particle size but continuously adjustable pore size was synthesized by wet chemical method. 2 O ball (P-Cu 2 O), when the pore size is 240nm, the Faradaic efficiency of C2+ products is about 75.3%, but the Faradaic efficiency of ethanol is only about 20%.
[0003] Due to CO 2 The high thermal stability of the molecule leads to electrocatalytic CO 2 The RR reaction to ethanol requires overcoming a high energy barrier and a high potential to be applied. Therefore, the development of catalysts with high catalytic activity is of great research value. 2 The RR reaction is complex and involves many competing reactions, resulting in low Faradaic efficiency and poor selectivity of the ethanol product.
[0004] A large number of modification strategies have been used to improve the electrocatalytic CO 2 The catalytic activity of the reduction reaction to ethanol includes catalyst morphology control, introduction of multi-metal active sites and surface modification. However, commonly used catalyst materials such as MOF, nanotubes and other nanomaterials have a series of problems that make them difficult to commercialize. Including:
[0005] (1) Technical aspects: The synthesis method is complex. The commonly used hydrothermal synthesis, annealing, calcination, doping and other methods are cumbersome and difficult to directly produce the required catalyst. The preparation cycle is long, usually taking several days, and there are many uncontrollable factors in the preparation process, especially nanomaterials are more susceptible to influence.
[0006] (2) Cost: The production cost is high. The materials used to synthesize the catalyst, such as the organic ligands required for the synthesis of MOF, are expensive. At the same time, the synthesis yield of commonly used nanomaterials is not high, and the synthesis process is complicated, which further increases the cost of medicines, water and electricity. The production efficiency is low. The high production costs of time, money, etc. and the low catalyst output all lead to low production efficiency of the catalyst, making it impossible to achieve efficient commercial production.
[0007] (3) Efficiency: Catalysts prepared by different existing technologies are used for electrocatalytic CO 2The Faraday efficiency of RR to ethanol is not high, mostly between 40 and 70%; when the Faraday efficiency of C2+ products is high, the selectivity of ethanol products is also low. In addition, the applied potential required to generate ethanol is high, and the optimal potential is mostly between -0.5 and -0.8 V vs. RHE. Summary of the invention
[0008] In view of the above-mentioned deficiencies in the prior art, the present invention aims to provide a method for electrocatalytic reduction of CO 2 Carbon-based catalyst for ethanol production and its preparation method and application, by adjusting the metal ratio, calcination temperature, calcination time, and the ratio of external nitrogen source melamine in the catalyst preparation process, the optimal preparation conditions are obtained for catalyst production, which is used for electrocatalytic CO 2 RR to produce ethanol to solve the technical, cost and efficiency problems of existing methods.
[0009] In order to achieve the above-mentioned object of the invention, the technical solution adopted by the present invention is:
[0010] Provided is a method for electrocatalytic reduction of CO 2 A method for preparing a carbon-based catalyst for producing ethanol, comprising the following steps:
[0011] Coal, copper nitrate hexahydrate and melamine were mixed to prepare Cu-C 3 H 6 N 6 -C catalyst; wherein the proportion of copper is 1 to 5%, and the proportion of melamine is 1 to 10%; Cu-C 3 H 6 N 6 -C catalyst is calcined at 800-1000°C for 1-7 hours.
[0012] Furthermore, coal, copper nitrate hexahydrate and melamine were mixed and dissolved in 10 mL of N,N-dimethylformamide solution, and stirred at 600 r / min for 3 hours at room temperature to prepare Cu-C 3 H 6 N 6 -C catalyst.
[0013] Furthermore, the proportion of copper is 3% and the proportion of melamine is 5%.
[0014] Furthermore, the calcination temperature is 900°C.
[0015] Furthermore, the calcination time is 5 hours.
[0016] Furthermore, the Cu-C 3 H 6 N 6-C catalyst was placed in a ceramic boat, and the ceramic boat was placed in a quartz tube of a tubular furnace for programmed temperature increase. The temperature increase program was as follows: ① argon was passed through at 30°C, the argon flow rate was 100 mL / min, and the ventilation time was 60 min; ② the temperature was increased from room temperature 30°C to 850°C at 5°C / min over 164 minutes; ③ the temperature was increased from 850°C to 900°C at 1°C / min over 50 minutes; ④ 900°C was maintained for 300 minutes; ⑤ natural cooling to room temperature.
[0017] The beneficial effects of the present invention are:
[0018] (1) Efficiency: Compared with existing electrocatalytic CO 2 Compared with the RR ethanol production technology, the present invention can achieve 70% ethanol Faraday efficiency at a lower applied potential (-0.25V vs. RHE). The present invention can achieve ethanol production at a lower overpotential, which is beneficial to reducing energy consumption and improving the energy conversion efficiency of the reaction.
[0019] (2) Production cost: Generally, a variety of chemical reagents are required, such as isopropanol, dimethyl sulfoxide, acetone, hydrochloric acid, sodium thiosulfate, etc., which increases the basic cost; and there are many synthesis steps, including mixing and stirring, ultrasonic dispersion, suspension heating, high-temperature calcination, etc., and a special sample preparation environment, such as the catalyst must be stored in a glove box filled with pure Ar, which increases the process cost. However, the present invention only uses copper nitrate hexahydrate, melamine and N,N-dimethylformamide, and the reagents used are inexpensive; there are fewer preparation steps, and the process consumes less external costs such as water and electricity, which effectively reduces the production cost of the catalyst. In addition, the present invention directly uses coal that has been commercially produced, which can achieve scale-up production and improve production efficiency.
[0020] (3) Technical aspects: The present invention only requires stirring, adsorption, drying and calcination. The technology used is simple and the production cycle is short. It can be mass-produced to achieve commercial application. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a scanning electron microscope photo of commercial coal after water washing without other processing steps;
[0022] Figure 2 3%Cu-5%C prepared in Example 5 3 H 6 N 6 -SEM photo of the catalyst at 900℃ for 5h;
[0023] Figure 3 X-ray diffraction (XRD) spectra of the original coal, Example 1, and the catalysts prepared in Examples 9-10;
[0024] Figure 4X-ray diffraction (XRD) spectra of the catalysts prepared in Examples 1 to 3;
[0025] Figure 5 X-ray diffraction (XRD) spectra of the catalysts prepared in Example 1 and Examples 4 to 6;
[0026] Figure 6 X-ray diffraction (XRD) spectra of the catalysts prepared in Example 5 and Examples 7-8;
[0027] Figure 7 Schematic diagram of electrochemically active specific surface area of catalysts prepared in Example 1 and Examples 4 to 6;
[0028] Figure 8 3%Cu-5%C prepared in Example 5 3 H 6 N 6 -Schematic diagram of BET specific surface area of C-900℃-5h catalyst;
[0029] Fig. 9 3%Cu-5%C prepared in Example 1 3 H 6 N 6 -Schematic diagram of BET specific surface area of C-900℃-3h catalyst;
[0030] Fig.10 3%Cu-5%C prepared in Example 1 3 H 6 N 6 -C-900℃-3h catalyst electrocatalysis CO 2 Faradaic efficiency diagram of RR generated products and ethanol alone;
[0031] Fig.11 3%Cu-5%C prepared in Example 5 3 H 6 N 6 -C-900℃-5h catalyst electrocatalysis CO 2 Faradaic efficiency diagram of RR generated products and ethanol alone;
[0032] Fig.12 5% C prepared in Comparative Example 1 3 H 6 N 6 -C-900℃-5h catalyst electrocatalysis CO 2 Faradaic efficiency diagram of RR generated products and ethanol alone;
[0033] Fig.13 The 3% Cu-C-900℃-5h catalyst prepared in Comparative Example 2 electrocatalyzed CO 2Faradaic efficiency diagram of RR generated products and ethanol alone;
[0034] Fig.14 3%Cu-5%C prepared in Example 5 3 H 6 N 6 - Schematic diagram of the catalyst stability test results at C-900℃-5h;
[0035] Fig.15 The catalyst prepared in Example 1 and Example 5 electrocatalyzes CO 2 Comparison of RR ethanol production performance with existing literature levels. DETAILED DESCRIPTION
[0036] The specific implementation modes of the present invention are described below so that those skilled in the art can understand the present invention. However, it should be clear that the present invention is not limited to the scope of the specific implementation modes. For those of ordinary skill in the art, as long as various changes are within the spirit and scope of the present invention as defined and determined by the attached claims, these changes are obvious, and all inventions and creations utilizing the concept of the present invention are protected.
[0037] Example 1
[0038] (1) Commercial coal is added to deionized water for washing. After multiple deionized water washings, dust and other impurities on the surface of the coal are washed away, and the coal is placed in an oven at 80°C for drying.
[0039] (2) Weigh a certain amount of dried coal, weigh corresponding amounts of copper nitrate hexahydrate and melamine (in this embodiment, the proportion of copper is 3% and the proportion of melamine is 5%), dissolve them in 10 mL of DMF (N,N-dimethylformamide) solution, and stir and adsorb at room temperature at a speed of 600 r / min for 3 hours to prepare 3% Cu-5% C 3 H 6 N 6 -C catalyst.
[0040] (3) 3%Cu-5%C 3 H 6 N 6 -C catalyst was placed in an oven at 80°C for drying.
[0041] (4) Weigh 300 mg of the dried material and place it in a ceramic boat. Place the ceramic boat in a quartz tube of a tubular furnace (facing the heating resistor) for programmed heating and calcine at 900°C for 3 hours. The heating program is: ① 30°C with argon (100 mL / min) for 60 min, ② 5°C / min from room temperature 30°C to 850°C over 164 min, ③ 1°C / min from 850°C to 900°C over 50 min, ④ 900°C maintained for 180 min, ⑤ naturally cooled to room temperature. 3% Cu-5% C was prepared. 3 H 6 N 6 -C-900℃-3h catalyst.
[0042] Example 2
[0043] In the method steps of Example 2, the same points as those of Example 1 are not described here, and only the differences from Example 1 are described. The difference between Example 2 and Example 1 is that in step (4), the calcination temperature is changed to 800°C for 3 hours to calcine 3% Cu-5% C 3 H 6 N 6 -C. The heating program is: ① 30℃ with argon (100mL / min) for 60min, ② 5℃ / min from room temperature 30℃ to 750℃ over 144min, ③ 1℃ / min from 750℃ to 800℃ over 50min, ④ 800℃ maintained for 180min, ⑤ natural cooling to room temperature. 3%Cu-5%C was prepared. 3 H 6 N 6 -C-800℃-3h catalyst.
[0044] Example 3
[0045] In the method steps of Example 3, the same points as those of Example 1 are not described here, and only the differences from Example 1 are described. The difference between Example 3 and Example 1 is that in step (4), the calcination temperature is changed to 1000°C for 3 hours to calcine 3% Cu-5% C 3 H 6 N 6 -C. The heating program is: ① 30℃ with argon (100mL / min) for 60min, ② 5℃ / min from room temperature 30℃ to 950℃ over 184min, ③ 1℃ / min from 950℃ to 1000℃ over 50min, ④ 1000℃ for 180min, ⑤ natural cooling to room temperature. 3%Cu-5%C was prepared. 3 H 6 N 6 -C-1000℃-3h catalyst.
[0046] Example 4
[0047] In the method steps of Example 4, the same points as those of Example 1 are not described here, and only the differences from Example 1 are described. The difference between Example 4 and Example 1 is that in step (4), the calcination time is changed to 1 hour, and 3% Cu-5% C is calcined at 900°C. 3 H 6 N 6 -C. The heating program is: ① 30℃ with argon (100,L / min) for 60min, ② 5℃ / min from room temperature 30℃ to 850℃ over 164min, ③ 1℃ / min from 850℃ to 900℃ over 50min, ④ 900℃ for 60min, ⑤ natural cooling to room temperature. 3%Cu-5%C was prepared. 3 H 6 N 6 -C-900℃-1h catalyst.
[0048] Example 5
[0049] In the method steps of Example 5, the same points as those of Example 1 are not described here, and only the differences from Example 1 are described. The difference between Example 5 and Example 1 is that in step (4), the calcination time is changed to 5h, and the 3%Cu-5%C is calcined at 900℃. 3 H 6 N 6 -C. The heating program is: ① 30℃ with argon (100mL / min) for 60min, ② 5℃ / min from room temperature 30℃ to 850℃ over 164min, ③ 1℃ / min from 850℃ to 900℃ over 50min, ④ 900℃ for 300min, ⑤ natural cooling to room temperature. 3%Cu-5%C was prepared. 3 H 6 N 6 -C-900℃-5h catalyst.
[0050] Example 6
[0051] In the method steps of Example 6, the same points as those of Example 1 are not described here, and only the differences from Example 1 are described. The difference between Example 6 and Example 1 is that in step (4), the calcination time is changed to 7h, and the 3%Cu-5%C is calcined at 900℃. 3 H 6 N 6-C. The heating program is: ① 30℃ with argon (100mL / min) for 60min, ② 5℃ / min from room temperature 30℃ to 850℃ over 164min, ③ 1℃ / min from 850℃ to 900℃ over 50min, ④ 900℃ for 420min, ⑤ natural cooling to room temperature. 3%Cu-5%C was prepared. 3 H 6 N 6 -C-900℃-7h catalyst.
[0052] Example 7
[0053] In the method steps of Example 7, the same points as those of Example 5 are not described here, and only the differences from Example 5 are described. The difference between Example 7 and Example 5 is that in step (2), the proportion of melamine is changed to 1%, and 3% Cu-1% C 3 H 6 N 6 -C catalyst.
[0054] Example 8
[0055] In the method steps of Example 8, the same points as those of Example 5 are not described here, and only the differences from Example 5 are described. The difference between Example 8 and Example 5 is that in step (2), the proportion of melamine is changed to 10%, and 3% Cu-10% C 3 H 6 N 6 -C catalyst.
[0056] Example 9
[0057] In the method steps of Example 9, the same points as those of Example 1 are not described here, and only the differences from Example 1 are described. The difference between Example 9 and Example 1 is that in step (2), the copper ratio is changed to 1%, and 1% Cu-5% C is prepared. 3 H 6 N 6 -900℃-3h catalyst.
[0058] Example 10
[0059] In the method steps of Example 10, the same points as those of Example 1 are not described here, and only the differences from Example 1 are described. The difference between Example 10 and Example 1 is that in step (2), the copper ratio is changed to 5%, and 5% Cu-5% C is prepared. 3 H 6 N 6 -900℃-3h catalyst.
[0060] Depend on Figure 1-2 It can be seen that the catalyst prepared by the method of the present application retains the structure of the original commercial coal, indicating that the coal structure has not been changed after a series of treatments, and only metallic copper is doped to enhance the electrocatalytic CO 2 Activity of RR in producing ethanol.
[0061] Depend on Figure 3-6 It can be seen that compared with the XRD diffraction peaks of commercial coal, 1%Cu-5%C 3 H 6 N 6 -C-900℃-3h, 5%Cu-5%C 3 H 6 N 6 -C-900℃-3h, 3%Cu-5%C 3 H 6 N 6 -C-800℃-3h, 3%Cu-5%C 3 H 6 N 6 -C-900℃-7h, 3%Cu-10%C 3 H 6 N 6 -C-900℃-5h, 3%Cu-5%C 3 H 6 N 6 -C-900℃-1h red shift occurs, which may be due to the increase in the interplanar spacing of the catalyst or the expansion of the lattice; 3%Cu-5%C 3 H 6 N 6 -C-1000℃-3h, 3%Cu-5%C 3 H 6 N 6 -C-900℃-3h is basically unchanged; while 3%Cu-5%C 3 H 6 N 6 -C-900℃-5h, 3%Cu-1%C 3 H 6 N 6 -C-900℃-5h blue shift occurs, indicating that the lattice spacing between samples becomes smaller or the lattice structure shrinks, which may be beneficial to CO 2 ER. Figure 7 It can be seen that 3%Cu-5%C 3 H 6 N 6 -C-900℃-5h has the largest electrochemically active specific surface area; and Figure 8-9 It can be seen that 3%Cu-5%C 3 H 6 N 6-C-900℃-5h has the largest BET specific surface area. As the specific surface area increases, the available electrocatalytic CO 2 The number of active sites of RR increased, so the catalytic performance of the catalyst was significantly improved. The optimal catalyst preparation conditions were 3% Cu and 5% C. 3 H 6 N 6 , calcination temperature 900℃, calcination time 5h.
[0062] Comparative Example 1
[0063] In the method steps of Comparative Example 1, the same points as those of Example 5 are not described here, and only the differences from Example 5 are described. The difference between Comparative Example 1 and Example 5 is that copper nitrate hexahydrate is not added in step (2) to prepare 5% C 3 H 6 N 6 -C-900℃-5h catalyst.
[0064] Comparative Example 2
[0065] In the method steps of Comparative Example 2, the same points as those of Example 5 are not described here, and only the differences from Example 5 are described. The difference between Comparative Example 2 and Example 5 is that melamine is not added in step (2), and a 3% Cu-C-900°C-5h catalyst is prepared.
[0066] Test example
[0067] Electrocatalytic CO 2 RR performance test: The catalyst loading method was carried out by a catalyst loading method known in the art (not within the scope of protection of the present application), that is, the prepared catalyst was ground into powder using an agate mortar, 5 mg of the catalyst was taken into a 2 mL centrifuge tube, 250 μL of deionized water, 110 μL of acetone and 40 μL of Nafion solution were added to make ink, ultrasonically dispersed for 2 h, and then 150 μL of the ink was coated on a 1×1 cm 2 The carbon paper was clamped on the electrode, and the electrode was placed in an H-type three-electrode electrolytic cell with 10 mL of 0.5 mol / L KHCO on each side. 3 The solution was separated by a proton exchange membrane, and the saturated Ag / AgCl electrode and the platinum electrode were used as the reference electrode and the counter electrode, respectively. At room temperature and pressure, CO was introduced at a flow rate of 20 mL / min. 2 The gas was heated for 20 minutes to make the CO in the solution 2When the gas reaches saturation, CV test is performed, and after stabilization, It test is performed. During the test, the applied voltage range is -0.85V to -1.1V (i.e. -0.2V vs. RHE to -0.45V vs. RHE). After stabilization at constant potential for 20 minutes, the gas product produced is detected by Fuli GC9790II and the liquid product produced is detected by Bruker Avance NEO 400MHz.
[0068] The test results are as follows Figure 10-15 As shown. 3%Cu-5%C prepared in Example 1 3 H 6 N 6 -C-900℃-3h catalyst has a maximum Faraday efficiency of 60.8% for ethanol when the applied potential is -0.25V vs.RHE, which is significantly lower than the applied potential in the existing literature; the 3%Cu-5%C 3 H 6 N 6 -C-900℃-5h, the Faraday efficiency of ethanol was further improved to about 70% when the applied potential was -0.25V vs.RHE. 2 ER, and comparative examples 1 and 2 were tested. It was found that the electrocatalytic CO 2 RR performance is poor. 3 H 6 N 6 -C-900℃-5h catalyst stability was tested and good stability results for 20h were obtained.
[0069] In this application, % represents mass percentage. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention.
[0070] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for preparing a carbon-based catalyst for electrocatalytic reduction of CO2 to ethanol, characterized in that: The following steps are involved: Coal, copper nitrate hexahydrate and melamine are mixed to prepare a Cu-C3H6N6-C catalyst, wherein the proportion of copper is 1-5%, and the proportion of melamine is 1-10%. The Cu-C3H6N6-C catalyst is calcined at 800-1000°C for 1-7 hours.
2. The method for preparing a carbon-based catalyst for electrocatalytic reduction of CO2 to ethanol according to claim 1, characterized in that: Coal, copper nitrate hexahydrate and melamine were mixed, dissolved in N,N-dimethylformamide solution, and stirred and adsorbed at a speed of 600 r / min at room temperature for 3 hours to prepare a Cu-C3H6N6-C catalyst.
3. The method for preparing a carbon-based catalyst for electrocatalytic reduction of CO2 to ethanol according to claim 1, characterized in that: The copper ratio is 3% and the melamine ratio is 5%.
4. The method for preparing a carbon-based catalyst for electrocatalytic reduction of CO2 to ethanol according to claim 1, characterized in that: The calcination temperature is 900°C.
5. The method for preparing a carbon-based catalyst for electrocatalytic reduction of CO2 to ethanol according to claim 1, characterized in that: The calcination time was 5 hours.
6. The method for preparing a carbon-based catalyst for electrocatalytic reduction of CO2 to ethanol according to claim 5, characterized in that: The Cu-C3H6N6-C catalyst was placed in a ceramic boat, and the ceramic boat was placed in a quartz tube of a tubular furnace for programmed temperature rise. The temperature rise program was as follows: ① argon was passed at 30°C, 100 mL / min, for 60 min, ② the temperature was raised from room temperature 30°C to 850°C at 5°C / min over 164 min, ③ the temperature was raised from 850°C to 900°C at 1°C / min over 50 min, ④ 900°C was maintained for 300 min, and ⑤ natural cooling was performed to room temperature.
7. A carbon-based catalyst for electrocatalytic reduction of CO2 to ethanol prepared by the method according to any one of claims 1 to 6.
8. Use of the carbon-based catalyst according to claim 7 in the electrocatalytic reduction of CO2 to produce ethanol.
Citation Information
Cited By
Preparation method and application of electrocatalyst for electroreduction of CO2 into ethanol
CN121110086A