Nitrogen-doped RuO2-TiO2 coating titanium electrode and preparation method thereof
Patent Information
- Application Number
- CN202411016398.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-27
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-27
AI Technical Summary
The electrocatalytic activity and electrode life of existing RuO2-TiO2 coated titanium electrodes are difficult to improve, and the high cost of the precious metal iridium (Ir) limits its application, and the laboratory-scale preparation method is not suitable for practical applications.
By introducing nitrogen-containing precursors in situ into the RuO2-TiO2 coating solution, a nitrogen-doped RuO2-TiO2 coating is formed, and the chlorine-induced activity and life of the electrode are improved by using nitrogen elements and Ru3+, Ti3+ and oxygen vacancies. The surface is used The electrodes are prepared by coating annealing to maintain the easy amplification of the existing electrode preparation process.
The chlorine evolution yield and service life of the electrode was significantly improved. The life of the nitrogen-doped-RuO2-TiO2-coated titanium electrode increased by 50%-150% in the strengthening life experiment, and the chlorine evolution yield increased by 20%-80%, without changing the electrode preparation. process.
Smart Images

Figure CN118957674A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a nitrogen-doped-RuO2-TiO2 coating titanium electrode and a preparation method thereof, belonging to the technical field of inorganic materials. Background Art
[0002] As an anode, RuO2-TiO2 coated titanium electrode can convert chloride ions in water into dissolved free chlorine such as elemental chlorine, hypochlorous acid, hypochlorite, etc. through electrocatalysis. It has the advantages of high mechanical strength, dimensional stability, and corrosion resistance. It is the most widely used chlorine evolution electrode in modern chemical industry, chlor-alkali industry, water treatment and disinfection. The electrocatalytic activity and electrode life of RuO2-TiO2 coated titanium electrode are important indicators for evaluating electrode performance. The chemical valence and occurrence form of Ru, Ti and O in RuO2-TiO2 coating are closely related to the catalytic activity of the electrode. Zhang et al. prepared RuO2 electrocatalyst rich in oxygen vacancies by combining sodium alginate with ruthenium ions, and found that oxygen vacancies help to improve the electrocatalytic oxygen evolution activity of RuO2 [Angew. Chem. Int. Ed. 2021, 60, 18821–18829]. However, the method described in the document prepares RuO2 powder particles and loads them on glassy carbon electrodes for testing, which is only suitable for laboratory-scale characterization analysis and is not suitable for practical applications. In addition, the current method to increase the service life of RuO2-TiO2 coated titanium electrodes is mainly to add precious metal iridium (Ir) to the coating. However, the reserves of Ir in the earth's crust are only one ten-millionth, and the price is very expensive. Therefore, it is urgent to develop new methods to improve the electrocatalytic activity and electrode life of RuO2-TiO2 coated titanium electrodes. Summary of the invention
[0003] The present invention provides a nitrogen-doped modified RuO2-TiO2 coated titanium electrode (nitrogen-doped-RuO2-TiO2 coated titanium electrode) and a preparation method thereof. The prepared electrode has rich Ru 3+ 、Ti 3+ , and oxygen vacancy active sites, the electrode has high chlorine evolution activity and long service life. The preparation of nitrogen-doped-RuO2-TiO2 coated titanium electrode is achieved by in-situ introduction of nitrogen-containing precursors into the RuO2-TiO2 coating solution, that is, in-situ modification of the coating solution. This method does not require changing the existing electrode preparation process and is easy to scale up production.
[0004] The technical solution of the present invention is as follows:
[0005] A nitrogen-doped RuO2-TiO2 coated titanium electrode is prepared by annealing a surface coating method, characterized in that the electrode has a uniform and complete active coating, the active component of the coating is nitrogen-doped RuO2-TiO2; the nitrogen element is uniformly distributed in the active coating, and the nitrogen doping makes the active coating rich in Ru3+ 、Ti 3+ , and oxygen vacancy active sites, so that the electrode has a higher chlorine evolution yield and a longer service life. 2 Under the conditions of enhanced life test at 40℃, the life of nitrogen-doped-RuO2-TiO2 coated titanium electrode is increased by 50%-150% compared with that of RuO2-TiO2 coated titanium electrode. Nitrogen-doped-RuO2-TiO2 coated titanium electrode has the characteristics of high chlorine evolution yield and long life.
[0006] A method for preparing a nitrogen-doped-RuO2-TiO2 coated titanium electrode is as follows:
[0007] (1) Titanium substrate pretreatment
[0008] The titanium substrate is placed in an annealing furnace for annealing to eliminate stress, and after cooling to room temperature, it is sequentially subjected to sandblasting, acetone degreasing cleaning, oxalic acid etching, and deionized water cleaning. The treated titanium substrate is placed in anhydrous ethanol for storage;
[0009] The titanium substrate is a titanium mesh or a titanium sheet; the annealing furnace temperature is set at 400-600°C, and the insulation time is 10-60 minutes; the acid etching is to put the titanium substrate into slightly boiling oxalic acid and boil it for 1-2 hours, and the mass fraction of the oxalic acid solution used for acid etching is 10%-15%.
[0010] (2) Preparation of coating liquid
[0011] A certain amount of nitrogen-containing precursor is added to anhydrous ethanol, stirred and dissolved at 10-60°C, and then a certain amount of tetrabutyl titanate and ruthenium trichloride are added, and a small amount of concentrated hydrochloric acid is added dropwise, and stirred evenly to obtain a coating liquid;
[0012] The nitrogen-containing precursor is ammonium chloride, dicyandiamide, or imidazole, and the mass fraction of the nitrogen-containing precursor in the coating liquid is 0.1wt%-10wt%;
[0013] The molar ratio of tetrabutyl titanate to ruthenium trichloride added to the coating liquid is (7-9):(3-1), and the total concentration of Ti and Ru in the coating liquid is 0.1-0.5 mol / L;
[0014] (3) Electrode coating and calcination
[0015] The coating solution in (2) is applied to the titanium substrate treated in (1) by a brush or a dip coating machine. Each time the coating is applied, the coated electrode is dried under an infrared lamp for 10-15 minutes, and then the electrode is placed in a muffle furnace at 400-600° C. for thermal oxidation in an air atmosphere for 10-15 minutes. Finally, the electrode is taken out and cooled to room temperature before the next coating is applied. This process is repeated 6-15 times.
[0016] The electrode after the last coating is placed in a muffle furnace at 400-600° C. and calcined in an air atmosphere for 1-2 hours, and then naturally cooled to room temperature in the furnace and taken out to obtain a nitrogen-doped-RuO2-TiO2 coated titanium electrode;
[0017] The pulling speed of the immersion and pulling coating machine is 500-1000 μm / s;
[0018] The nitrogen content of the nitrogen-doped-RuO2-TiO2 coated titanium electrode in the coating is 1wt%-15wt%, and the nitrogen is evenly distributed in the coating; doping with nitrogen increases the chlorine evolution active site Ru in the electrode. 3+ 、Ti 3+ , and the number of oxygen vacancies;
[0019] (4) Electrode performance test
[0020] The electrode prepared in (3) was tested for chlorine evolution performance and stability. The chlorine evolution performance test was carried out at 50 mM NaCl, pH 7, 10 mA / cm 2 The stability test was carried out under the conditions of 1M H2SO4, 2A / cm 2 , 40℃;
[0021] Compared with the conventional RuO2-TiO2-coated titanium electrode which is not nitrogen-doped, the chlorine evolution yield of the nitrogen-doped-RuO2-TiO2-coated titanium electrode is increased by 20%-80% and the enhanced service life is increased by 50%-150%.
[0022] The technical features of the present invention are as follows:
[0023] 1. The present invention uses a nitrogen-containing precursor to nitrogen-dope the electrode coating liquid. The nitrogen atoms in the nitrogen-containing precursor react with Ru 3+ Chelation, so that the nitrogen-containing precursor in the coating solution and Ru 3+ A stable and uniform dispersion is formed, thereby obtaining a nitrogen-doped-RuO2-TiO2 coated titanium electrode uniformly doped with N element.
[0024] 2. The selection of nitrogen-containing precursors in the present invention plays an important role in the preparation of electrodes. The nitrogen-containing precursors selected in this patent include but are not limited to ammonium chloride (slightly soluble in ethanol), imidazole (easily soluble in ethanol), and dicyandiamide (easily soluble in ethanol). The above three nitrogen-containing precursors are all reductive. During the thermal oxidation process, their reductive properties promote the formation of low-valent Ti in the TiO2-RuO2 coating. 3+ 、Ru 3+ ; Furthermore, the low-valent Ti in the RuO2-TiO2 lattice 3+ 、Ru 3+ Promoting the generation of oxygen vacancies. TiO2-RuO2 low-valent Ti3+ 、Ru 3+ , and oxygen vacancies significantly improved the chlorine evolution activity and stability of the electrode.
[0025] 3. The mass fraction of the nitrogen-containing precursor in the coating liquid in the present invention is 0.1wt%-10wt%. When the mass fraction is too low, the electrode performance is not significantly improved due to the low N doping amount; when the mass fraction is too high, there are problems such as insufficient dissolution of the nitrogen-containing precursor and excessive chelation with metal ions, which destroys the uniformity of the coating liquid.
[0026] 4. In the present invention, the content of N in the coating is 1wt%-15wt%; the N in the coating is evenly distributed and incorporated into the lattice in the form of O-Ti-N; the incorporation of N stabilizes the oxygen vacancies and Ru in the coating. 3+ 、Ti 3+ , thereby increasing the chlorine evolution activity and life of the electrode; compared with the traditional RuO2-TiO2 coated titanium electrode without nitrogen doping, the nitrogen-doped-RuO2-TiO2 coated titanium electrode has a chlorine evolution output increased by 20%-80% and an enhanced life increased by 50%-150%.
[0027] 5. The pretreatment process of the titanium substrate includes an annealing step to eliminate thermal stress, which helps to slow down the generation of coating cracks caused by thermal stress during the coating brushing-drying-calcining process. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a scanning electron microscope photograph of the nitrogen-doped-RuO2-TiO2 coated titanium electrode in Example 1;
[0029] Figure 2 This is the EDS distribution diagram of the nitrogen-doped-RuO2-TiO2 coated titanium electrode in Example 1;
[0030] Figure 3 The EDS spectrum result of the nitrogen-doped-RuO2-TiO2 coated titanium electrode in Example 2;
[0031] Figure 4 The XPS results of the electrodes in Example 2 and the comparative example: The Ru peak and the Ti peak move toward the low energy direction, indicating that Ru 3+ With Ti 3+ Increased content; O V The (oxygen vacancy) peak area increases, indicating that the oxygen vacancy content increases; the N peak is at 398.6 eV, indicating that N exists in the electrode coating in the form of O-Ti-N;
[0032] Figure 5 is the electrode chlorine evolution yield in Example 3 and the comparative example;
[0033] Figure 6This is an accelerated life experiment of electrodes in Example 3 and the comparative example. DETAILED DESCRIPTION
[0034] The present invention will be described in detail below in conjunction with specific embodiments. The illustrative embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.
[0035] Example 1
[0036] (1) Titanium substrate pretreatment
[0037] The titanium mesh was placed in an annealing furnace at 500°C for 30 minutes to eliminate stress, and then sandblasted and polished, cleaned with acetone for degreasing, and then boiled in slightly boiling oxalic acid (15% mass fraction) for 2 hours, and then cleaned with deionized water. Finally, the treated titanium mesh was placed in anhydrous ethanol for storage;
[0038] (2) Preparation of coating liquid
[0039] 0.32 g of dicyandiamide was added to 100 mL of anhydrous ethanol, and the mixture was stirred at 60°C to dissolve. Then, 11.93 mL of tetrabutyl titanate and 3.11 g of ruthenium trichloride were added, and 3.3 mL of concentrated hydrochloric acid was added dropwise, and the mixture was stirred evenly to obtain a coating liquid.
[0040] (3) Electrode coating and calcination
[0041] The coating liquid in (2) is applied to the titanium mesh treated in (1) with a brush. Each time the coating is applied, the coated electrode is dried under an infrared lamp for 10 minutes, and then the electrode is placed in a muffle furnace at 450°C for thermal oxidation in an air atmosphere for 10 minutes. Finally, the electrode is taken out and cooled to room temperature before the next coating is applied. This is repeated 15 times.
[0042] The electrode after the last coating was placed in a muffle furnace at 450°C and calcined in an air atmosphere for 1 hour. After naturally cooling to room temperature in the furnace, it was taken out to obtain a nitrogen-doped-RuO2-TiO2 coated titanium electrode. The content of nitrogen in the coating was 4.25wt%;
[0043] (4) Electrode performance test
[0044] The electrode prepared in (3) was tested for chlorine evolution performance and stability. The chlorine evolution performance test was carried out at 50 mM NaCl, pH 7, 10 mA / cm 2 The chlorine evolution yield in 30 min was 24.8 mg / L under the conditions of 24.8 mg / L. The chlorine evolution yield in 30 min of the RuO2-TiO2 coated titanium electrode without nitrogen doping prepared under the same conditions was 20.2 mg / L. The chlorine evolution yield of the nitrogen-doped RuO2-TiO2 coated titanium electrode was 22.8% higher than that of the RuO2-TiO2 coated titanium electrode.
[0045] The stability test adopts the enhanced life experiment, in 1M H2SO4, 2A / cm 2 The prepared nitrogen-doped-RuO2-TiO2 coated titanium electrode was cut into 1×1 cm 2 The size of the electrode was used as the anode and the pure titanium sheet was used as the cathode. The lifespan was measured to be 16.5h when the cell voltage rose to 20V; the lifespan of the RuO2-TiO2 coated titanium electrode prepared under the same conditions without nitrogen doping was measured to be 9.5h under this condition; the lifespan of the nitrogen-doped-RuO2-TiO2 coated titanium electrode was increased by 73.7% compared with that of the RuO2-TiO2 coated titanium electrode.
[0046] Example 2
[0047] As described in Example 1, except that:
[0048] In step (2), 0.44 g of imidazole was added to 100 mL of anhydrous ethanol, and the mixture was stirred at 60° C. to dissolve. Then, 11.93 mL of tetrabutyl titanate and 3.11 g of ruthenium trichloride were added, and 3.3 mL of concentrated hydrochloric acid was added dropwise, and the mixture was stirred evenly to obtain a coating liquid.
[0049] In step (3), the coating liquid in (2) is applied to the titanium mesh treated in (1) with a brush. Each time the coating is applied, the coated electrode is dried under an infrared lamp for 10 minutes, and then the electrode is placed in a muffle furnace at 450° C. for thermal oxidation in an air atmosphere for 10 minutes. Finally, the electrode is taken out and cooled to room temperature before the next coating is applied. This process is repeated 15 times.
[0050] The electrode after the last coating was placed in a muffle furnace at 450°C and calcined in an air atmosphere for 1 hour. After naturally cooling to room temperature in the furnace, it was taken out to obtain a nitrogen-doped-RuO2-TiO2 coated titanium electrode. The content of nitrogen in the coating was 3.65wt%;
[0051] In step (4), the electrode prepared in (3) was subjected to a chlorine evolution performance and stability test. The chlorine evolution performance test was carried out at 50 mM NaCl, pH 7, 10 mA / cm 2 The chlorine evolution yield in 30 min was measured to be 25.2 mg / L; the chlorine evolution yield in 30 min of the RuO2-TiO2 coated titanium electrode without nitrogen doping prepared under the same conditions was measured to be 20.2 mg / L under the same conditions; the chlorine evolution yield of the nitrogen-doped-RuO2-TiO2 coated titanium electrode was increased by 24.8% compared with that of the RuO2-TiO2 coated titanium electrode.
[0052] The stability test adopts the enhanced life experiment, in 1M H2SO4, 2A / cm 2The prepared nitrogen-doped-RuO2-TiO2 coated titanium electrode was cut into 1×1 cm 2 The size of the electrode was used as the anode and the pure titanium sheet was used as the cathode. The life span was measured to be 15.2h when the cell voltage rose to 20V; the life span of the RuO2-TiO2 coated titanium electrode prepared under the same conditions without nitrogen doping (measured under this condition was 9.5h; the life span of the nitrogen-doped-RuO2-TiO2 coated titanium electrode was increased by 60% compared with that of the RuO2-TiO2 coated titanium electrode.
[0053] Step (1) is the same as in Example 1.
[0054] Example 3
[0055] As described in Example 1, except that:
[0056] In step (2), 0.27 g of ammonium chloride was added to 100 mL of anhydrous ethanol, and the mixture was stirred at 60° C. to dissolve. Then, 11.93 mL of tetrabutyl titanate and 3.11 g of ruthenium trichloride were added, and 3.3 mL of concentrated hydrochloric acid was added dropwise, and the mixture was stirred evenly to obtain a coating liquid.
[0057] In step (3), the coating liquid in (2) is applied to the titanium mesh treated in (1) with a brush. Each time the coating is applied, the coated electrode is dried under an infrared lamp for 10 minutes, and then the electrode is placed in a muffle furnace at 450° C. for thermal oxidation in an air atmosphere for 10 minutes. Finally, the electrode is taken out and cooled to room temperature before the next coating is applied. This process is repeated 15 times.
[0058] The electrode after the last coating was placed in a muffle furnace at 450°C and calcined in an air atmosphere for 1 hour. After naturally cooling to room temperature in the furnace, it was taken out to obtain a nitrogen-doped-RuO2-TiO2 coated titanium electrode. The content of nitrogen in the coating was 1.45wt%;
[0059] In step (4), the electrode prepared in (3) was subjected to a chlorine evolution performance and stability test. The chlorine evolution performance test was carried out at 50 mM NaCl, pH 7, 10 mA / cm 2 The chlorine evolution yield in 30 min was 35.0 mg / L under the conditions. The chlorine evolution yield in 30 min of the RuO2-TiO2 coated titanium electrode without nitrogen doping prepared under the same conditions was 20.2 mg / L under the conditions. The chlorine evolution yield of the nitrogen-doped RuO2-TiO2 coated titanium electrode increased by 73.3% compared with that of the RuO2-TiO2 coated titanium electrode.
[0060] The stability test adopts the enhanced life experiment, in 1M H2SO4, 2A / cm 2 The prepared nitrogen-doped-RuO2-TiO2 coated titanium electrode was cut into 1×1 cm2 The size of the electrode was used as the anode and the pure titanium sheet was used as the cathode. The life span was measured to be 18.3h when the cell voltage rose to 20V; the life span of the RuO2-TiO2 coated titanium electrode prepared under the same conditions without nitrogen doping was measured to be 9.5h under this condition; the life span of the nitrogen-doped-RuO2-TiO2 coated titanium electrode was increased by 92.6% compared with that of the RuO2-TiO2 coated titanium electrode.
[0061] Step (1) is the same as in Example 1.
[0062] Comparative Example
[0063] As described in Example 1, except that:
[0064] In step (2), 11.93 mL of tetrabutyl titanate and 3.11 g of ruthenium trichloride were added to 100 mL of anhydrous ethanol, and 3.3 mL of concentrated hydrochloric acid was added dropwise, and stirred evenly to obtain a coating liquid;
[0065] In step (3), the coating liquid in (2) is applied to the titanium mesh treated in (1) with a brush. Each time the coating is applied, the coated electrode is dried under an infrared lamp for 10 minutes, and then the electrode is placed in a muffle furnace at 450° C. for thermal oxidation in an air atmosphere for 10 minutes. Finally, the electrode is taken out and cooled to room temperature before the next coating is applied. This process is repeated 15 times.
[0066] The electrode after the last coating was placed in a muffle furnace at 450° C. and calcined in an air atmosphere for 1 hour. After naturally cooling to room temperature in the furnace, the electrode was taken out to obtain a RuO2-TiO2 coated titanium electrode without nitrogen doping.
[0067] In step (4), the RuO2-TiO2 coated titanium electrode prepared in (3) without nitrogen doping was subjected to chlorine evolution performance and stability test. The chlorine evolution performance test was carried out at 50 mM NaCl, pH 7, 10 mA / cm 2 The reaction was carried out under the conditions of , and the chlorine evolution yield in 30 minutes was measured to be 20.2 mg / L.
[0068] The stability test adopts the enhanced life experiment, in 1M H2SO4, 2A / cm 2 The prepared RuO2-TiO2-coated titanium electrode without nitrogen doping was cut into 1×1 cm 2 The size is used as the anode and the pure titanium sheet as the cathode. The life is measured to be 9.5h when the cell voltage rises to 20V.
[0069] Step (1) is the same as in Example 1.
Claims
1. A nitrogen-doped-RuO2-TiO2 coated titanium electrode and a preparation method thereof, comprising the following steps: (1) Titanium substrate pretreatment The titanium substrate is placed in an annealing furnace for annealing to eliminate stress, and after cooling to room temperature, it is sequentially subjected to sandblasting, acetone degreasing cleaning, oxalic acid etching, and deionized water cleaning. The treated titanium substrate is placed in anhydrous ethanol for storage; The titanium substrate is a titanium mesh or a titanium sheet; the annealing furnace temperature is set to 400-600°C, and the holding time is 10-60 minutes; the acid etching is to put the titanium substrate into slightly boiling oxalic acid and boil it for 1-2 hours, and the mass fraction of the oxalic acid solution used for the acid etching is 10%-15%; (2) Preparation of coating liquid A certain amount of nitrogen-containing precursor is added to anhydrous ethanol, stirred and dissolved at 10-60°C, and then a certain amount of tetrabutyl titanate and ruthenium trichloride are added, and a small amount of concentrated hydrochloric acid is added dropwise, and stirred evenly to obtain a coating liquid; The nitrogen-containing precursor is ammonium chloride, dicyandiamide, or imidazole, and the mass fraction of the nitrogen-containing precursor in the coating liquid is 0.1wt%-10wt%; The molar ratio of tetrabutyl titanate to ruthenium trichloride added to the coating liquid is (7-9):(3-1), and the total concentration of Ti and Ru in the coating liquid is 0.1-0.5 mol / L; (3) Electrode coating and calcination The coating solution in (2) is applied to the titanium substrate treated in (1) by a brush or a dip coating machine. Each time the coating is applied, the coated electrode is dried under an infrared lamp for 10-15 minutes, and then the electrode is placed in a muffle furnace at 400-600° C. for thermal oxidation in an air atmosphere for 10-15 minutes. Finally, the electrode is taken out and cooled to room temperature before the next coating is applied. This process is repeated 6-15 times. The electrode after the last coating is placed in a muffle furnace at 400-600° C. and calcined in an air atmosphere for 1-2 hours, and then naturally cooled to room temperature in the furnace and taken out to obtain a nitrogen-doped-RuO2-TiO2 coated titanium electrode; The pulling speed of the immersion and pulling coating machine is 500-1000 μm / s; The nitrogen content of the nitrogen-doped-RuO2-TiO2 coated titanium electrode in the coating is 1wt%-15wt%, and the nitrogen is evenly distributed in the coating. The doping of nitrogen increases the chlorine evolution active site Ru in the electrode. 3+ 、Ti 3+ , and the number of oxygen vacancies. The electrode doped with nitrogen has high chlorine evolution activity and long life. (4) Electrode performance test The electrode prepared in (3) was tested for chlorine evolution performance and stability. The chlorine evolution performance test was carried out at 50 mM NaCl (aq), pH = 7, 10 mA / cm 2 The stability test was carried out under the conditions of 1M H2SO4, 2A / cm 2 , 40℃; Compared with the conventional RuO2-TiO2-coated titanium electrode which is not nitrogen-doped, the chlorine evolution yield of the nitrogen-doped-RuO2-TiO2-coated titanium electrode is increased by 20%-80% and the enhanced service life is increased by 50%-150%.
2. The preparation method according to claim 1, characterized in that In the step (1), the titanium substrate is first placed in an annealing furnace for annealing to eliminate stress. Preferably, the annealing furnace temperature is 500° C. and the holding time is 60 minutes.
3. The preparation method according to claim 1, characterized in that: In the step (2), the type of nitrogen-containing precursor is ammonium chloride, dicyandiamide or imidazole, and the mass fraction of the nitrogen-containing precursor in the coating liquid is 0.1wt%-10wt%; the nitrogen atoms in the nitrogen-containing precursor and Ru 3+ Chelation, so that the nitrogen-containing precursor in the coating solution and Ru 3+ A stable and uniform dispersion is formed, thereby obtaining a nitrogen-doped-RuO2-TiO2 coated titanium electrode uniformly doped with N element.
4. The preparation method according to claim 1, characterized in that: In the step (2), the molar ratio of tetrabutyl titanate to ruthenium trichloride added to the coating liquid is 7:3, 8:2 or 9:1, and the total concentration of Ti and Ru in the coating liquid is 0.1-0.5 mol / L.
5. The preparation method according to claim 1, characterized in that: In the step (3), preferably, after each coating and drying, thermal oxidation is carried out in a muffle furnace at 450-550° C.; and the electrode after the last coating is calcined in a muffle furnace at 450-550° C.
6. The preparation method according to claim 1, characterized in that: In the nitrogen-doped RuO2-TiO2 coated titanium electrode, the content of N in the coating is 1wt%-15wt%; the N element in the coating is doped into the lattice in the form of O-Ti-N; the doping of nitrogen increases the Ru active site in the electrode for chlorine evolution. 3+ 、Ti 3+ , and the number of oxygen vacancies; compared with the traditional RuO2-TiO2 coated titanium electrode without nitrogen doping, the chlorine evolution yield of the nitrogen-doped RuO2-TiO2 coated titanium electrode is increased by 20%-80%, and the enhanced life is increased by 50%-150%.
Citation Information
Patent Citations
Titanium electrode for chlorine generator and preparation method thereof
CN101922016A
Titanium-base TiNx / TiO2-RuO2 nano coating anode
CN104846399A
Preparation method and application of carbon-based anode material for producing chlorine through electrolysis
CN113621979A
Alkali metal-RuO2-TiO2 coating titanium electrode and preparation method thereof
CN114180682A