Large-size single crystal diamond substrate and preparation method thereof
By growing polycrystalline diamond on the Si substrate and forming a composite substrate with Ir diamond, the problem of mismatch between traditional substrate lattice and thermal expansion is solved, the preparation of high-quality large-size single-crystalline diamond is achieved, and the substrate fragmentation is solved The cracking problem has promoted the research on diamond materials.
Patent Information
- Application Number
- CN202411033252.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The lattice constant and thermal expansion coefficient of traditional heteroepitaxy diamond substrates do not match the diamond, which leads to difficulty in making high-quality diamond substrates, especially during the substrate shrinkage process, diamond substrate fragmentation is prone to occur.
By using a self-supported polycrystalline diamond substrate and an Ir diamond composite substrate, polycrystalline diamond composite substrate is formed on the Si substrate and a fixed crystalline iridium film is formed on it, and then on it Single crystal diamond was grown, and the thermal expansion coefficient difference between the Ir film and diamond was peeled off to prepare a substrate with small differences in the lattice constant and thermal expansion coefficient.
It has successfully reduced the difficulty of making high-quality large-size single-crystal diamond substrates, reduced the risk of substrate fragmentation, realized the preparation of high-quality large-size single-crystal diamonds, and promoted the research and application of diamond materials and devices.
Smart Images

Figure CN118957752A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductor devices, and in particular relates to a large-size single-crystal diamond substrate and a preparation method thereof. Background Art
[0002] Diamond has excellent optical, thermal, electrical and mechanical properties. It is an ideal wide bandgap semiconductor material and can be used in optics, medicine, detectors and semiconductors. The preparation of single crystal diamond can be divided into two types: homoepitaxial and heteroepitaxial. Among them, homoepitaxial single crystal diamond is limited by the size of the seed crystal, and it is difficult to obtain a large-sized single crystal diamond substrate. Heteroepitaxial diamond has the advantages of large size and multiple selectivity in substrate selection. Large-sized and high-quality wafer substrates are the prerequisite for the large-scale application of semiconductor materials. Therefore, heteroepitaxial method is the most promising method for preparing large-sized single crystal diamond substrates.
[0003] At present, the traditional heteroepitaxial diamond substrates mainly include silicon (Si), magnesium oxide (MgO), sapphire (Al2O3), yttria-stabilized zirconia (YSZ) and strontium titanate (SrTiO3). There are many problems in growing large-area single-crystal diamond based on these substrates. Two of the main problems are that the lattice constant and thermal expansion coefficient of the substrate and the single-crystal diamond do not match, making it difficult to produce high-quality diamond wafers.
[0004] An effective solution to the problem of lattice constant mismatch is to prepare a metal layer on the substrate as a buffer layer. The lattice constant difference between iridium (Ir) metal and diamond is 7.03%, and it is stable and not easy to decompose, making it an ideal metal element for preparing a metal buffer layer. The thermal expansion coefficient of traditional heteroepitaxial substrates is greater than that of diamond. During the cooling process after the growth of single crystal diamond, the substrate shrinks more and the diamond shrinks less, making it easy for the diamond substrate to break. Therefore, there is an urgent need for a substrate with a small difference in lattice constant and thermal expansion coefficient as a single crystal diamond growth substrate. Summary of the invention
[0005] The embodiment of the present invention provides a large-size single-crystal diamond substrate and a preparation method thereof, aiming to prepare a substrate with small differences in lattice constant and thermal expansion coefficient as a single-crystal diamond growth substrate, thereby reducing the difficulty of manufacturing a high-quality diamond substrate.
[0006] To achieve the above object, the technical solution adopted by the present invention is: to provide a method for preparing a large-size single crystal diamond substrate, the method comprising:
[0007] Preparation of self-supporting polycrystalline diamond substrates;
[0008] Preparation of Ir-coated diamond composite substrate;
[0009] Preparation of single crystal diamond based on the Ir-coated diamond composite substrate.
[0010] The preparation of the self-supporting polycrystalline diamond substrate comprises:
[0011] Polycrystalline diamond is grown after diamond seed crystals are evenly covered on the surface of the Si substrate;
[0012] Polishing of polycrystalline diamond front side;
[0013] A temporary carrier is fixed on the front side of the polished polycrystalline diamond;
[0014] Remove the Si substrate and polish the back side of the polycrystalline diamond;
[0015] The temporary carrier is removed, resulting in a free-standing polycrystalline diamond substrate.
[0016] In conjunction with the first aspect, in an achievable manner, after the surface of the Si substrate is uniformly covered with diamond seed crystals and before polycrystalline diamond is grown, the method includes:
[0017] The cleaned, blown-dried and dried Si substrate is placed in a diamond seed crystal aqueous solution for ultrasonic cleaning for 5-60 minutes, and then soaked for 5-180 minutes after the ultrasonic cleaning. The concentration of the diamond seed crystal aqueous solution is 0.05%-2%, and the size of the diamond seed crystal is 10-2000nm; after the soaking, it is blown-dried again.
[0018] In conjunction with the first aspect, in an achievable manner, a process of growing polycrystalline diamond after uniformly covering the surface of a Si substrate with diamond seed crystals comprises:
[0019] The Si substrate covered with diamond seed crystal is placed in the MPCVD equipment, evacuated to below 5.0E-6mbar, hydrogen is introduced as a carrier gas with a hydrogen flow rate of 300sccm, and then the temperature is raised to 700-900°C, the pressure is controlled between 100-200mbar, a gaseous carbon source is introduced, and the ratio of the gaseous carbon source flow rate to the hydrogen flow rate is maintained at 5%. The growth time is more than 100 hours, and the thickness of the obtained polycrystalline diamond is more than 300μm.
[0020] In combination with the first aspect, in one achievable manner, removing the Si substrate and polishing the back side of the polycrystalline diamond comprises:
[0021] The polycrystalline diamond and Si substrate fixed with a temporary carrier are placed in an acid etching solution, which is a mixture of 50% by volume hydrofluoric acid and 50% by volume nitric acid. After the Si substrate is completely etched clean, the polycrystalline diamond is transferred to the temporary carrier.
[0022] In combination with the first aspect, in one achievable manner, the preparation of the Ir-coated diamond composite substrate includes:
[0023] Depositing a crystal-oriented iridium film on the treated single crystal MgO substrate to obtain an Ir / MgO composite substrate;
[0024] Bonding the front side of the self-supporting polycrystalline diamond substrate to the Ir / MgO composite substrate to form a polycrystalline diamond / fixed crystal orientation iridium film / MgO composite substrate;
[0025] The single crystal MgO substrate is removed to form an Ir-coated diamond composite substrate.
[0026] In combination with the first aspect, in an achievable manner, the preparation of single crystal diamond based on the Ir-coated diamond composite substrate includes:
[0027] The Ir-coated diamond composite substrate is placed in an MPCVD device for heteroepitaxial diamond bias nucleation;
[0028] Growing single crystal diamond on the Ir-coated diamond composite substrate after bias nucleation;
[0029] The polished single crystal diamond and the Ir-coated diamond composite substrate are peeled off to obtain a single crystal diamond substrate.
[0030] In combination with the first aspect, in one achievable manner, heteroepitaxial diamond bias nucleation comprises:
[0031] Place the Ir-coated diamond composite substrate into the MPCVD equipment, heat it to 400-600°C, turn on the bias power supply, the bias range at the substrate is -200V to -100V, the ratio of hydrogen flow to methane flow is 100:5, and the bias nucleation time is 30min.
[0032] In combination with the first aspect, in an achievable manner, growing single crystal diamond on an Ir-coated diamond composite substrate after bias nucleation includes:
[0033] After the bias nucleation is completed, the bias power supply is turned off, the ratio of hydrogen flow rate to methane flow rate is kept unchanged at 100:5, the temperature is raised to 750-900°C, and the growth of single crystal diamond begins.
[0034] In a second aspect, an embodiment of the present invention further provides a large-sized single-crystal diamond substrate, based on a method for preparing the large-sized single-crystal diamond substrate.
[0035] Compared with the prior art, the method for preparing a large-size single-crystal diamond substrate provided by the present invention has the following beneficial effects: first, a self-supporting polycrystalline diamond substrate is prepared, then an iridium metal film with a fixed crystal orientation is transferred to the polycrystalline diamond to form an Ir-coated diamond composite substrate, and finally single-crystal diamond is grown on the composite substrate. The invention is conducive to the preparation of high-quality large-size single-crystal diamond and has important significance for the promotion and research of diamond materials and devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 A schematic diagram of the preparation process of a self-supporting polycrystalline diamond substrate provided in an embodiment of the present invention;
[0037] Figure 2 A schematic diagram of the preparation process of an Ir-coated diamond composite substrate provided in an embodiment of the present invention;
[0038] Figure 3 A schematic diagram of the preparation process of single crystal diamond based on an Ir-coated diamond composite substrate provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0039] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0040] Please also read Figures 1 to 3 Now, the preparation method of the large-size single-crystal diamond substrate provided by the present invention is described. The preparation method of the large-size single-crystal diamond substrate comprises the following steps:
[0041] Step 1: Preparation of self-supporting polycrystalline diamond substrate, see Figure 1 As shown;
[0042] Step 2: Preparation of Ir-coated diamond composite substrate, see Figure 2 As shown;
[0043] Step 3: Preparation of single crystal diamond based on the Ir-coated diamond composite substrate. Figure 3 shown.
[0044] In step 1, the preparation of the self-supporting polycrystalline diamond substrate includes multiple stages, see Figure 1 As shown, the details are as follows:
[0045] The first stage, covering the diamond seed stage, see Figure 1As shown in (1): First, a single crystal Si substrate is selected, and the substrate has a (001) crystal plane. The single crystal Si substrate is ultrasonically cleaned with deionized water and acetone respectively, blown dry with a nitrogen gun, placed in a dustproof device, and dried in an oven; secondly, the cleaned single crystal Si substrate is ultrasonically cleaned in a diamond seed crystal aqueous solution for 5-60 minutes, and then soaked for 5-180 minutes after the ultrasonic cleaning, wherein the concentration of the diamond seed crystal aqueous solution is 0.05%-2%, and the size of the diamond seed crystal is 10-2000nm.
[0046] After the immersion is completed, the single crystal Si substrate is taken out, blown dry again with a nitrogen gun, placed in a dustproof device, and dried in an oven.
[0047] The second stage, the polycrystalline diamond growth stage, see Figure 1 As shown in (2): First, the Si substrate with the diamond seed crystal is placed in the MPCVD equipment and evacuated to below 5.0E-6mbar to prepare for the growth of polycrystalline diamond; secondly, hydrogen is introduced as a carrier gas with a hydrogen flow rate of 300sccm, the microwave power source is turned on, the temperature is raised to 700-900°C, the pressure is controlled between 100-200mbar, and a gaseous carbon source is introduced. The gaseous carbon source can be any one of methane, ethane, ethylene, acetylene and propane. The carbon-hydrogen ratio (C / H) is the ratio of the gaseous carbon source flow rate to the hydrogen flow rate. The C / H ratio is maintained at 5%. The growth time is more than 100 hours, and the thickness of the grown polycrystalline diamond reaches more than 300μm.
[0048] After the growth is completed, the gaseous carbon source is stopped, the cavity pressure is slowly reduced to room temperature in a hydrogen environment, the microwave power is turned off, and the cavity is opened for 30 minutes before taking out the polycrystalline diamond / Si composite material.
[0049] The third stage, the polycrystalline diamond front polishing stage, see Figure 1 As shown in (3): The front side of the polycrystalline diamond is ground and chemically mechanically polished, and the diamond surface roughness (RMS), total thickness deviation (TTV) within the wafer, and wafer warpage (BOW) meet the following standards: Atomic force microscope tests any 10μm×10μm range on the substrate surface, RMS<0.5nm, TTV<10μm, BOW<10μm, and the side connected to the single crystal Si substrate is defined as the back side of the polycrystalline diamond, and the side away from the single crystal Si substrate is the front side of the polycrystalline diamond.
[0050] The fourth stage is the stage of fixing the polycrystalline diamond to the temporary carrier and removing the single crystal Si substrate, see Figure 1 As shown in (4) and (5): the polished polycrystalline diamond / Si composite material is fixed to a temporary carrier, the temporary carrier can be a wafer-level sapphire, and the fixing medium is high-temperature resistant paraffin wax.
[0051] The polycrystalline diamond / Si composite material and a temporary carrier are placed in an acid etching solution, wherein the acid etching solution is a mixture of 50% by volume hydrofluoric acid and 50% by volume nitric acid, and the ratio of hydrofluoric acid to nitric acid is greater than 5; after etching for a period of time and waiting for the single crystal Si substrate to be completely etched, the polycrystalline diamond is transferred to the temporary carrier to form a polycrystalline diamond / temporary carrier composite material, which is then rinsed with deionized water.
[0052] The fifth stage, the polycrystalline diamond backside polishing stage, see Figure 1 As shown in (6): The polycrystalline diamond back surface is ground and chemically mechanically polished, and the diamond surface roughness (RMS), total thickness deviation (TTV) within the wafer, and wafer bow (BOW) meet the following standards: Atomic force microscopy tests any 10μm×10μm range on the substrate surface, RMS<2nm, TTV<10μm, BOW<10μm.
[0053] The sixth stage is the formation of a self-supporting polycrystalline diamond substrate, see Figure 1 As shown in (7): After polishing, the polycrystalline diamond / temporary carrier composite material is placed on a hot plate for heating. After the high temperature resistant paraffin wax melts, the polycrystalline diamond falls off from the temporary carrier and is rinsed with acetone, alcohol and deionized water to obtain a self-supporting polycrystalline diamond substrate.
[0054] Step 2: The preparation of the Ir-coated diamond composite substrate includes multiple stages, see Figure 2 , as follows:
[0055] The first stage is the stage of Ir film growth towards the fixed crystal direction, see Figure 2 As shown in (1) and (2): a single crystal MgO substrate is selected, and the substrate has a (001) crystal plane. The single crystal MgO substrate is ultrasonically cleaned with deionized water and acetone respectively, blown dry with a nitrogen gun, placed in a dustproof device, and dried in an oven; a layer of fixed crystal orientation Ir film is deposited on the treated single crystal MgO substrate by any method of magnetron sputtering, electron beam evaporation, molecular beam epitaxy, and laser pulse deposition to obtain an Ir / MgO composite substrate; the thickness of the fixed crystal orientation Ir film is 50-1000nm; the surface of the fixed crystal orientation Ir film is ultrasonically cleaned with alcohol for 15 minutes, and after cleaning, it is rinsed with deionized water and then blown dry with nitrogen.
[0056] The second stage is the bonding stage between the self-supporting polycrystalline diamond substrate and the Ir / MgO composite substrate, see Figure 2 As shown in (3): the cleaned self-supporting polycrystalline diamond substrate front side is bonded to the Ir / MgO composite substrate to form a polycrystalline diamond / fixed crystal orientation Ir film / MgO composite substrate.
[0057] The third stage is to remove the MgO substrate and form an Ir-coated diamond composite substrate. Figure 2 As shown in (4): the polycrystalline diamond / fixed crystal orientation Ir film / MgO composite substrate is placed in a phosphoric acid etching solution with a phosphoric acid etching solution concentration of 50% by volume; after etching for a period of time, when the single crystal MgO substrate is completely etched away, the fixed crystal orientation Ir film is transferred to the self-supporting polycrystalline diamond to form a fixed crystal orientation Ir film / polycrystalline diamond structure, which is called an Ir-coated diamond composite substrate.
[0058] Step 3: Preparation of single crystal diamond based on the Ir-coated diamond composite substrate, see Figure 3 , including multiple stages, as follows:
[0059] The first stage, BEN stage, see Figure 3 As shown in (1), (2) and (3): biased microwave plasma chemical vapor deposition (hereinafter referred to as MPCVD) equipment is used to perform biased ion bombardment nucleation (BEN) on the Ir-coated diamond composite substrate to prepare diamond nucleation points on the surface of the composite substrate.
[0060] Specifically, the Ir-coated diamond composite substrate is placed in the MPCVD equipment, the temperature is raised to 400-600°C, the bias power supply is turned on, the bias range at the substrate is -200V to -100V, the ratio of hydrogen flow to methane flow is 100:5, and the bias nucleation time is 30min.
[0061] The second stage, the single crystal diamond growth stage, see Figure 3 As shown in (4): After the bias nucleation is completed, the bias power supply is turned off, the ratio of hydrogen flow rate to methane flow rate is kept constant at 100:5, the temperature is raised to 750-900°C, and single crystal diamond begins to grow. The thickness of the single crystal diamond is greater than 300μm, forming a single crystal diamond / fixed crystal orientation Ir film / polycrystalline diamond composite structure material. After the growth is completed, the gaseous carbon source is stopped, the cavity pressure is slowly reduced, and slowly reduced to room temperature in a hydrogen environment, the microwave power supply is turned off, and the cavity is opened for 30 minutes before the composite structure material is taken out.
[0062] The third stage is the single crystal diamond front polishing stage, see Figure 3 As shown in (4): The front surface of the single crystal diamond is ground and chemically mechanically polished, and the diamond surface roughness (RMS), total thickness deviation (TTV) within the wafer, and wafer bow (BOW) meet the following standards: Atomic force microscope tests any 10μm×10μm range on the substrate surface, RMS <1nm, TTV <20μm, BOW <20μm. By definition, the contact surface between the single crystal diamond and the Ir film is the back surface.
[0063] The fourth stage is to peel off the single crystal diamond and the composite substrate to form a single crystal diamond substrate stage, see Figure 3 As shown in (5): the polished single crystal diamond / fixed crystal Ir film / polycrystalline diamond composite structure material is placed in liquid nitrogen, and the difference in thermal expansion coefficient between the Ir film and the diamond is used to cause the single crystal diamond to fall off from the Ir-coated diamond composite substrate, ultimately obtaining a single crystal diamond substrate with a thickness greater than 300 μm.
[0064] The specific examples of the preparation method provided by the present invention are as follows:
[0065] The first step is to combine Figure 1 Understanding the preparation of self-supporting polycrystalline diamond: Select a single crystal Si substrate with a (001) crystal plane, place it in a diamond seed crystal aqueous solution for ultrasonic cleaning for 30 minutes, and soak it for 30 minutes after the ultrasonic cleaning. The concentration of the diamond seed crystal aqueous solution is 0.1%, and the size of the diamond seed crystal is 50nm.
[0066] The single crystal Si substrate with diamond seed crystal was placed in the MPCVD equipment for polycrystalline diamond growth, with a hydrogen flow rate of 300sccm, a growth temperature of 800℃, a growth pressure of 150mbar, a C / H ratio of 5%, a growth time of more than 150 hours, and a polycrystalline diamond thickness of 350μm. After polishing, the front roughness of the polycrystalline diamond was 0.5nm, the back roughness was 1.9nm, and the thickness of the self-supporting polycrystalline diamond was 300μm, the TTV was 8μm, and the BOW was 9μm.
[0067] The second step is to combine Figure 2 Understand the preparation of Ir-coated diamond composite substrate: the selected MgO substrate is the (001) crystal plane, and the laser pulse deposition method is used to grow the fixed crystal orientation Ir film with a thickness of 200nm; the fixed crystal orientation Ir film is transferred to a self-supporting polycrystalline diamond substrate to form an Ir-coated diamond composite substrate; in the single crystal BEN stage, the temperature is 450℃, the bias range is -150V, the ratio of hydrogen flow to methane flow is 100:5, and the bias nucleation time is 30min;
[0068] The third step is to combine Figure 3 Understanding the growth stages of single crystal diamond: the growth temperature is 800°C, the growth pressure is 165mbar, and the ratio of hydrogen flow to methane flow is 100:5. After the single crystal diamond is polished on the front side, the RMS is 0.9nm, the TTV is 16μm, the BOW is 19μm, and the thickness of the final single crystal diamond is 330μm.
[0069] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described or recorded in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.
[0070] Based on the same inventive concept, an embodiment of the present application also provides a large-size single-crystal diamond substrate and a method for preparing the large-size single-crystal diamond substrate.
[0071] The method for preparing a large-size single-crystal diamond substrate provided by the present invention can prepare a single-crystal diamond substrate with a thickness greater than 300 μm. The invention is conducive to preparing high-quality large-size single-crystal diamond and has important significance for the promotion and research of diamond materials and devices.
[0072] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a large-size single crystal diamond substrate, characterized in that: The method comprises: Preparation of self-supporting polycrystalline diamond substrates; Preparation of Ir-coated diamond composite substrate; Preparation of single crystal diamond based on the Ir-coated diamond composite substrate.
2. The method for preparing a large-size single crystal diamond substrate according to claim 1, characterized in that: The preparation of the self-supporting polycrystalline diamond substrate comprises: Polycrystalline diamond is grown after diamond seed crystals are evenly covered on the surface of the Si substrate; Polishing of polycrystalline diamond front side; A temporary carrier is fixed on the front side of the polished polycrystalline diamond; Remove the Si substrate and polish the back side of the polycrystalline diamond; The temporary carrier is removed, resulting in a free-standing polycrystalline diamond substrate.
3. The method for preparing a large-size single crystal diamond substrate according to claim 2, characterized in that: After the Si substrate surface is uniformly covered with diamond seed crystals and before polycrystalline diamond is grown, the following steps are included: The cleaned, blown-dried and dried Si substrate is placed in a diamond seed crystal aqueous solution for ultrasonic cleaning for 5-60 minutes, and then soaked for 5-180 minutes after the ultrasonic cleaning. The concentration of the diamond seed crystal aqueous solution is 0.05%-2%, and the size of the diamond seed crystal is 10-2000nm; after the soaking, it is blown-dried again.
4. The method for preparing a large-size single crystal diamond substrate according to claim 2, characterized in that: The process of growing polycrystalline diamond after uniformly covering the surface of the Si substrate with diamond seed crystals includes: The Si substrate covered with diamond seed crystal is placed in the MPCVD equipment, evacuated to below 5.0E-6mbar, hydrogen is introduced as a carrier gas with a hydrogen flow rate of 300sccm, and then the temperature is raised to 700-900°C, the pressure is controlled between 100-200mbar, a gaseous carbon source is introduced, and the ratio of the gaseous carbon source flow rate to the hydrogen flow rate is maintained at 5%. The growth time is more than 100 hours, and the thickness of the obtained polycrystalline diamond is more than 300μm.
5. The method for preparing a large-size single crystal diamond substrate according to claim 2, characterized in that: Removal of Si substrate and polishing of polycrystalline diamond backside, including: The polycrystalline diamond and Si substrate fixed with a temporary carrier are placed in an acid etching solution, which is a mixture of 50% by volume hydrofluoric acid and 50% by volume nitric acid. After the Si substrate is completely etched clean, the polycrystalline diamond is transferred to the temporary carrier.
6. The method for preparing a large-size single crystal diamond substrate according to claim 1, characterized in that: The preparation of the Ir-coated diamond composite substrate comprises: Depositing a crystal-oriented iridium film on the treated single crystal MgO substrate to obtain an Ir / MgO composite substrate; Bonding the front side of the self-supporting polycrystalline diamond substrate to the Ir / MgO composite substrate to form a polycrystalline diamond / fixed crystal orientation iridium film / MgO composite substrate; The single crystal MgO substrate is removed to form an Ir-coated diamond composite substrate.
7. The method for preparing a large-size single crystal diamond substrate according to claim 6, characterized in that: The preparation of single crystal diamond based on the Ir-coated diamond composite substrate comprises: The Ir-coated diamond composite substrate is placed in an MPCVD device for heteroepitaxial diamond bias nucleation; Growing single crystal diamond on the Ir-coated diamond composite substrate after bias nucleation; The polished single crystal diamond and the Ir-coated diamond composite substrate are peeled off to obtain a single crystal diamond substrate.
8. The method for preparing a large-size single-crystal diamond substrate according to claim 7, characterized in that: Heteroepitaxial diamond bias nucleation, including: Place the Ir-coated diamond composite substrate into the MPCVD equipment, heat it to 400-600°C, turn on the bias power supply, the bias range at the substrate is -200V to -100V, the ratio of hydrogen flow to methane flow is 100:5, and the bias nucleation time is 30min.
9. The method for preparing a large-size single crystal diamond substrate according to claim 7, characterized in that: Growing single crystal diamond on the Ir-coated diamond composite substrate after bias nucleation, comprising: After the bias nucleation is completed, the bias power supply is turned off, the ratio of hydrogen flow rate to methane flow rate is kept unchanged at 100:5, the temperature is raised to 750-900°C, and the growth of single crystal diamond begins.
10. A large-size single-crystal diamond substrate, characterized in that: A method for preparing a large-size single-crystal diamond substrate based on any one of claims 1-9.
Citation Information
Cited By