By gradually reducing the gas flow rate and using helium to replace hydrogen during the production process of zone melted silicon rods, the surface temperature of the silicon rod is controlled, and the problem of stress residue during deposition is solved, and the mechanical properties and product quality of the silicon rods are improved.
Patent Information
- Application Number
- CN202411042858.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
During the production of electronic grade polysilicon for zone melting, plastic stress residues formed during deposition and furnace shutdown lead to breaking of silicon rods, reducing usage efficiency and machining performance, and may lead to cracking and density of silicon rods during annealing. .
By gradually reducing the flow of trichlorosilicon and hydrogen during the deposition process, using high-purity helium to replace hydrogen, adjust the surface temperature of the silicon rod, and assist in cooling with heater, control the temperature gradient of the silicon rod to ensure uniform cooling and reduce stress concentration and cracks form.
Effectively eliminate residual stress inside the silicon rod, improve the mechanical properties and product quality of the silicon rod, reduce the risk of fracture, and ensure the stability and service life of the silicon rod in subsequent machining.
Smart Images

Figure CN118957765A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electronic-grade polysilicon production, and in particular to a method for eliminating residual stress inside a zone melting silicon rod. Background Art
[0002] In the production process of electronic-grade polysilicon for zone melting, a modified Siemens process is adopted. This method mainly uses vapor phase deposition (CVD) technology to chemically react trichlorosilane (SiHCl3) with high-purity hydrogen (H2) at high temperature, thereby depositing high-purity polysilicon on the surface of high-temperature silicon core rods. However, due to the particularity of this production method, it is very easy to form plastic stress residue during deposition and shutdown, which will cause silicon rod breakage in subsequent machining process, greatly reducing the utilization efficiency and machining performance of silicon rods. At the same time, the zone melting crystal pulling equipment will be damaged due to silicon rod breakage during use by downstream manufacturers.
[0003] At present, in order to reduce or eliminate the residual stress in the silicon rod, the industry often anneals the silicon rod again. The traditional treatment method is to continuously adjust the current to cool down the silicon rod. Under the purge of airflow, the temperature drop of the silicon rod surface is significantly faster than that of the inner layer, which makes it difficult to release and eliminate the stress in time. As a result, the silicon rod may be broken due to improper stress release during the annealing process. In addition, during the annealing process, the reduction furnace is in a hydrogen environment, and hydrogen diffuses onto the silicon rod, generating defects, affecting the density of the electronic-grade silicon rod, thereby reducing the quality of the product.
[0004] The information disclosed in this background technology section is only intended to deepen the understanding of the overall background technology of the present invention, and should not be regarded as acknowledging or suggesting in any form that the information constitutes the prior art already known to those skilled in the art. Summary of the invention
[0005] The present invention provides a method for eliminating residual stress inside a zone melt silicon rod, thereby effectively solving the problems pointed out in the background technology.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A method for eliminating residual stress inside a melt zone silicon rod, comprising:
[0008] S10: using trichlorosilane and hydrogen to deposit in a reactor to obtain a silicon rod for zone melting;
[0009] S20: In the first time period, the trichlorosilane inlet flow rate is reduced to 0, and the hydrogen flow rate is slowly reduced to 5% to 20% of the initial flow rate, so that the chlorosilane in the reaction furnace is completely replaced, and the surface temperature of the silicon rod is maintained at T1;
[0010] S30: In the second time period, adjusting the surface temperature of the silicon rod to T2;
[0011] S40: In the third time period, the hydrogen in the reaction furnace is replaced with high-purity helium. After the replacement is complete, the flow rate of the helium is adjusted to be consistent with the final flow rate of the hydrogen, and the temperature is maintained at T2;
[0012] S50: In the fourth time period, a heater is implanted in the reduction furnace and powered on to maintain the surface temperature of the silicon rod at T2;
[0013] S60: In the fifth time period, the current passing through the silicon rod is cut off, the current of the heater is adjusted, and the helium flow rate is adjusted to 1% to 10% of the original flow rate, so as to slowly adjust the surface temperature of the silicon rod to T3.
[0014] Further, in step S20, the first time period takes 30 minutes to 90 minutes, and the temperature T1 is 1000°C to 1050°C.
[0015] Further, in step S30, the second time period takes 30 minutes to 60 minutes, and the temperature T2 is 800°C to 1000°C.
[0016] Further, in step S40, the third time period is maintained for 30 minutes to 60 minutes.
[0017] Furthermore, in step S40, during the helium replacement process, gas replacement efficiency monitoring is added, and the steps include:
[0018] S41: Install high-precision gas flow meters in the helium and hydrogen inlet pipes;
[0019] S42: Connect the gas analyzer to the reaction furnace to detect the concentration changes of hydrogen and helium in real time;
[0020] S43: Setting the permissible range of hydrogen concentration to determine whether it is completely replaced by helium;
[0021] S44: According to the data of the gas analyzer and the gas flow meter, the flow rate of the helium is automatically adjusted through the central control system to optimize the replacement process.
[0022] Further, in step S50, the fourth time period takes 60 minutes to 180 minutes.
[0023] Further, in step S50, when the heaters are provided in a group, they are provided above the center of the chassis; when the heaters are provided in multiple groups, they are provided above the center of the chassis respectively and are evenly arranged between the inner and outer layers.
[0024] Furthermore, in step S50, a temperature feedback control system is also included to automatically adjust the heating power of the heater to maintain a stable temperature, and the steps include:
[0025] S51: using an infrared temperature measuring device to measure the temperature data of the silicon rod surface and the vicinity of the heater;
[0026] S52: using a data acquisition system to transmit the signal of the infrared temperature measuring device to a central control system in real time;
[0027] S53: Connecting the PID controller to the data acquisition system to ensure real-time acquisition of temperature data and output of control signals;
[0028] S54: Setting a temperature setting value of the PID controller to ensure that the heater can maintain the temperature of the silicon rod surface stable at T2;
[0029] S55: Connecting the thyristor regulator to the PID controller, and automatically adjusting the heating power of the heater according to the output signal of the PID controller.
[0030] Further, in step S60, the fifth time period takes 180 minutes to 360 minutes, and the temperature T3 is not higher than 180°C.
[0031] Further, in step S60, the process of dropping from the temperature T2 to the temperature T3 is divided into two stages of cooling. The cooling curve of the first stage is step-shaped. When the temperature drops to the temperature T3, the second stage of cooling begins. The second stage of cooling is a continuous rapid cooling stage.
[0032] The technical solution of the present invention can achieve the following technical effects:
[0033] After the deposition process of zone melting silicon is completed, the trichlorosilane flow rate and hydrogen flow rate are reduced to the specified amount within the specified time, and the surface temperature of the silicon rod is kept constant within a certain range by matching the current in the silicon rod; then the temperature is adjusted to the set value, while keeping the hydrogen flow rate unchanged, in preparation for subsequent furnace annealing; then argon is used to replace the hydrogen in the reduction furnace. At this time, the temperature is still in a larger range to prevent hydrogen from diffusing into the silicon rod and reduce the combination of silicon and hydrogen, which helps to reduce the defects of zone melting silicon and improve product quality. After the replacement is completed, the heater in the furnace is started and the temperature of the silicon rod is maintained for a certain period of time; finally, the silicon rod current is cut off, and the temperature of the silicon rod is continuously reduced to a certain range by controlling the output of the heater, while the argon flow rate remains unchanged. The above method can effectively eliminate the residual stress inside the silicon rod, ensuring that the silicon rod has good mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0035] Figure 1 A schematic flow chart of a method for eliminating residual stress inside a melt zone silicon rod;
[0036] Figure 2 A graph showing the change of material flow rate over time in a method for eliminating residual stress inside a zone melting silicon rod;
[0037] Figure 3 A diagram showing the change of reduction furnace temperature over time in a method for eliminating residual stress inside a zone melting silicon rod;
[0038] Figure 4 It is a graph showing the change of material flow rate over time in Example 1;
[0039] Figure 5 This is a graph showing the temperature of the reduction furnace changing with time in Example 1;
[0040] Figure 6 is a graph showing the temperature of the reduction furnace changing with time in Example 2;
[0041] Figure 7 This is a graph showing the temperature variation over time in the fifth time period in Example 2;
[0042] Figure 8 This is a graph showing the change of the original furnace temperature over time in Example 3. DETAILED DESCRIPTION
[0043] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0044] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0045] like Figures 1 to 3 A method for eliminating residual stress inside a zone melting silicon rod is shown, comprising:
[0046] S10: using trichlorosilane and hydrogen to deposit in a reactor to obtain silicon rods for zone melting; in this step, trichlorosilane (SiHCl3) and hydrogen (H2) are used to perform chemical vapor deposition (CVD) in a reactor to obtain silicon rods for zone melting;
[0047] S20: In the first time period, the trichlorosilane inlet flow rate is reduced to 0, and the hydrogen flow rate is slowly reduced to 5% to 20% of the initial flow rate, so that the chlorosilane in the reactor is completely replaced, and the surface temperature of the silicon rod is maintained at T1; this step adjusts the flow rate of the trichlorosilane logistics to 0, and performs preliminary internal replacement and temperature control;
[0048] S30: In the second time period, the surface temperature of the silicon rod is adjusted to T2; this step adjusts the surface temperature in preparation for subsequent furnace annealing;
[0049] S40: In the third time period, the hydrogen in the reaction furnace is replaced with high-purity helium. After the replacement is complete, the flow rate of the helium is adjusted to be consistent with the final flow rate of the hydrogen, and the temperature is maintained at T2. The purpose of replacing the hydrogen with helium in this step is to create a hydrogen-free environment in the reduction furnace to prevent hydrogen from diffusing onto the silicon rods in subsequent operations, generating defects, and affecting the density and quality of the electronic-grade silicon rods.
[0050] S50: In the fourth time period, a heater is implanted in the reduction furnace and powered on to maintain the surface temperature of the silicon rod at T2; this step adds heater-assisted cooling, controls the cooling process through the heater, adjusts the temperature gradient of the inner and outer layers of the silicon rod, ensures uniform cooling, and prevents stress concentration and crack formation caused by uneven cooling;
[0051] S60: In the fifth time period, the current passing through the silicon rod is cut off, the current of the heater is adjusted, and the helium flow rate is adjusted to 1% to 10% of the original flow rate to slowly adjust the surface temperature of the silicon rod to T3, the current of the heater is cut off, and the helium flow rate is maintained until the specified furnace start temperature is reached, the gas is stopped, and the furnace is started.
[0052] After the deposition process of the zone silicon is completed, the trichlorosilane flow rate and the hydrogen flow rate are reduced to the specified amount within the specified time, and the surface temperature of the silicon rod is kept constant within a certain range by matching the current in the silicon rod; then the temperature is adjusted to the set value, while keeping the hydrogen flow rate unchanged, in preparation for the subsequent furnace annealing; then argon is used to replace the hydrogen in the reduction furnace. At this time, the temperature is still in a larger range to prevent hydrogen from diffusing into the silicon rod and reduce the combination of silicon and hydrogen, which helps to reduce the defects of the zone silicon and improve product quality. After the replacement is completed, the heater in the furnace is started and the temperature of the silicon rod is maintained for a certain period of time; finally, the silicon rod current is cut off, and the temperature of the silicon rod is continuously reduced to a certain range by controlling the output of the heater. The argon flow rate remains unchanged. The above method can effectively eliminate the residual stress inside the silicon rod and ensure that the silicon rod has good mechanical properties.
[0053] After the power supply to the silicon rod is stopped, the present invention heats the surface of the silicon rod through a heater, and the overall cooling process of the silicon rod is controlled externally, which is helpful to adjust the gradient of the inner and outer layers of the silicon rod during the cooling process. Moreover, the silicon core of the silicon rod is in contact with the electrode and the base. After the current is turned off, with the help of the heat conduction effect, the heat of the inner layer of the silicon rod can be discharged through the cooling water of the electrode and the chassis water, so that the cooling speed of the inner layer of the silicon rod is not lower than that of the outer layer of the silicon rod. Therefore, by reasonably controlling the temperature drop speed of the silicon rod surface, the residual stress of the silicon rod can be effectively eliminated, the risk of fracture is reduced, and the silicon rod is guaranteed to have good mechanical properties.
[0054] Through phased and precise gas flow and temperature control, the residual stress inside the silicon rod can be effectively eliminated and the risk of fracture can be reduced. During the cooling process, the temperature gradient between the inner and outer layers of the silicon rod can be reasonably controlled to avoid stress concentration caused by excessive temperature gradient.
[0055] By using helium to replace hydrogen, a hydrogen-free environment is created in the reduction furnace to prevent hydrogen from diffusing onto the silicon rods, which helps reduce defects in the melt zone silicon and improve product quality. The hydrogen-free environment reduces the adsorption of hydrogen on the surface of the silicon rods, reduces surface stress, and improves the mechanical properties of the silicon rods.
[0056] As a preference of the above embodiment, in step S20, the first time period takes 30 minutes to 90 minutes, the temperature T1 is 1000°C to 1050°C, and within the specified time period (30 minutes to 90 minutes), the flow rate of trichlorosilane (TCS) is gradually reduced to 0, and the flow rate of hydrogen is slowly reduced to ensure that the chlorosilane in the reactor is completely replaced. The setting of this time period helps to ensure that all residual chlorosilane is completely removed and reduce the impact of the residue on the silicon rod; maintaining the surface temperature of the silicon rod in the range of 1000°C to 1050°C can make the replacement of chlorosilane more thorough and avoid production problems caused by unstable temperature or incomplete replacement; by gradually reducing the flow rate of chlorosilane within this temperature range, impurities and by-products in the reaction process can be more effectively removed, thereby improving the purity of the silicon rod.
[0057] In this embodiment, in step S30, the second time period takes 30 minutes to 60 minutes, and the temperature T2 is 800°C to 1000°C. Specifically, gradually adjusting the temperature of the silicon rod within the set temperature range (800°C to 1000°C) helps to smoothly transition to the annealing stage and avoid adverse effects of drastic temperature fluctuations on the silicon rod.
[0058] Wherein, in step S40, the third time period is maintained for 30 minutes to 60 minutes. Specifically, maintaining the time period of 30 minutes to 60 minutes is conducive to sufficient mixing and uniform replacement of the gas, ensuring the thoroughness of the replacement process, thereby improving the quality and performance of the silicon rods.
[0059] Since hydrogen diffuses onto the silicon rods in the reduction furnace, it affects the density and quality of the electronic-grade silicon rods. Therefore, it is very important to ensure that helium is completely replaced. Therefore, the following improvements are made:
[0060] As a preference of the above embodiment, in step S40, during the helium replacement process, gas replacement efficiency monitoring is added to ensure complete replacement, and the steps include:
[0061] S41: Install a high-precision gas flow meter (such as a mass flow meter or a volume flow meter) in the inlet pipes of helium and hydrogen; the flow meter monitors the flow of helium and hydrogen in real time to ensure that the gas flow meets the set requirements;
[0062] S42: Connecting a gas analyzer to the reactor to detect concentration changes of hydrogen and helium in real time; using a gas analyzer (such as a gas chromatograph or an infrared gas analyzer) to detect the gas composition in the reactor in real time to ensure that helium has completely replaced hydrogen;
[0063] S43: Set the permissible range of hydrogen concentration to determine whether it is completely replaced by helium; record the trend of the gradual decrease of hydrogen concentration to ensure the thoroughness of the replacement process;
[0064] S44: According to the data from the gas analyzer and gas flow meter, the central control system automatically adjusts the helium flow rate to optimize the replacement process and realize an automatic feedback mechanism. The central control system automatically adjusts the helium flow rate according to the real-time data of helium and hydrogen concentrations to ensure complete replacement.
[0065] By implementing an automatic feedback mechanism, the system can adjust the gas flow rate based on real-time data to ensure that the helium flow rate is maintained at an optimal level during the entire replacement process; by optimizing the replacement process, the internal stress of the silicon rod is effectively controlled, reducing the risk of breakage during subsequent machining and use, and improving the service life and reliability of the silicon rod; the alarm thresholds for gas concentration and flow can also be set to promptly detect and correct abnormalities in the replacement process, ensuring that operators can take prompt measures and reduce operational risks.
[0066] In this embodiment, in step S50, the fourth time period takes 60 minutes to 180 minutes. Specifically, a longer time period (60 minutes to 180 minutes) can ensure that the silicon rod maintains a sufficient heating time at the set temperature T2, so that the temperature of the silicon rod is uniform and stable, which helps to better control the heat treatment process of the silicon rod and ensure that the surface and internal temperatures of the silicon rod are consistent.
[0067] In step S50, when the heaters are provided in a group, they are provided above the center of the chassis; when the heaters are provided in multiple groups, they are respectively provided above the center of the chassis, and are evenly arranged between the inner and outer layers. Specifically, evenly arranged heaters help to reduce the temperature difference between the inner and outer layers of the silicon rod, reduce the internal stress caused by temperature fluctuations, thereby improving the stability of the heating process and the overall quality of the silicon rod.
[0068] As a preferred embodiment of the above, in step S50, a temperature feedback control system is further included to automatically adjust the heating power of the heater to maintain a stable temperature, and the steps include:
[0069] S51: using an infrared temperature measuring device to measure the temperature data of the silicon rod surface and the vicinity of the heater; specifically, the infrared temperature measuring device may be an infrared thermal imager installed outside the reduction furnace equipment, and the temperature is calculated by detecting the infrared radiation on the surface of the object, and the measurement can be performed contactlessly, and is suitable for real-time temperature monitoring in a high temperature environment;
[0070] S52: Use a data acquisition system (DAQ) to transmit the signal of the infrared temperature measuring device to the central control system in real time; ensure that the sampling rate and resolution of the data acquisition system meet the requirements of temperature control;
[0071] S53: Connect the PID controller to the data acquisition system to ensure real-time acquisition of temperature data and output of control signals; the PID controller calculates the control signal according to the data provided by the infrared temperature measuring device, adjusts the heating power to maintain the set temperature, and uses the PID algorithm to achieve automatic temperature adjustment;
[0072] S54: Setting the temperature setting value (T2) of the PID controller to ensure that the heater can maintain the temperature of the silicon rod surface stable at T2; this temperature value is the stable temperature that the silicon rod should maintain, and the PID controller reaches and maintains this setting value by adjusting the heating power;
[0073] S55: Connect the thyristor regulator to the PID controller, and automatically adjust the heating power of the heater according to the output signal of the PID controller. The PID controller outputs a control signal according to the real-time temperature data. The signal is used to adjust the conductivity of the thyristor regulator, thereby controlling the heating power of the heater. This step ensures that the power of the heater can be automatically adjusted to maintain the required temperature.
[0074] The temperature feedback control system can accurately control the temperature of the silicon rod surface by real-time monitoring the temperature of the silicon rod and adjusting the heating power to ensure that it is stable at the set value (T2). Accurate temperature control helps to eliminate residual stress inside the silicon rod and improve product quality. The PID controller can adjust the heating power in real time according to the data of the infrared temperature measuring device to reduce temperature fluctuations. This stability is crucial for eliminating residual stress, because temperature fluctuations may lead to uneven stress release, thereby affecting the mechanical properties of the silicon rod. The system automatically adjusts the heating power, reducing the need for manual intervention, making the operation process more automated and simple, and reducing the workload of operators.
[0075] In this embodiment, in step S60, the fifth time period takes 180 minutes to 360 minutes, and the temperature T3 is not higher than 180°C. Specifically, a long cooling period (180 minutes to 360 minutes) combined with a lower temperature (not higher than 180°C) helps to achieve a slow cooling process. This slow cooling can reduce internal stress concentration or cracks caused by an overly fast cooling rate, thereby ensuring that the internal stress of the silicon rod is effectively released.
[0076] Among them, in step S60, the process of cooling from temperature T2 to temperature T3 is divided into two stages of cooling. The cooling curve of the first stage is step-shaped. When the temperature drops to temperature T3, the second stage of cooling begins. The second stage of cooling is a continuous rapid cooling stage. Specifically, the step-shaped cooling in the first stage helps to gradually release stress during the cooling process, avoid stress mutations caused by sudden temperature drops, and enable the silicon rod to gradually adapt to temperature changes when approaching the target temperature, thereby better releasing internal stress; the step-shaped cooling can reduce the risk of cracks caused by sudden temperature drops, because the temperature changes more gently, which helps to prevent internal stress concentration and material rupture in the silicon rod during the cooling process; after the step-shaped cooling stage, the rapid cooling stage can quickly reduce the temperature of the silicon rod to the final required T3. This rapid cooling can shorten the overall cooling time, improve production efficiency, and ensure that the silicon rod reaches the required terminal temperature; through staged cooling, the temperature changes in each stage can be more carefully managed, and the stability and reliability of the overall cooling process can be improved.
[0077] Embodiment 1, as Figure 4 , Figure 5 As shown:
[0078] (1) using trichlorosilane and hydrogen to deposit in a reactor to obtain a silicon rod for zone melting;
[0079] (2) Within 60 minutes, reduce the trichlorosilane inlet flow rate to 0, slowly reduce the hydrogen flow rate to 20% of the initial flow rate, completely replace the chlorosilane in the reactor, and maintain the silicon rod surface temperature at 1050°C;
[0080] (3) Within 60 minutes, the surface temperature of the silicon rod is adjusted to 1000°C;
[0081] (4) Within 60 minutes, replace the hydrogen in the reactor with high-purity helium. After the replacement is complete, adjust the flow rate of helium to be consistent with the final flow rate of hydrogen and maintain the temperature at 1000°C;
[0082] (5) Within 120 minutes, the heater is implanted and powered on to maintain the surface temperature of the silicon rod at 1000°C. When the heater is arranged in one group, it can be located above the center of the chassis. When multiple groups of heaters are arranged, they can be arranged above the center of the chassis and evenly arranged between the inner and outer layers;
[0083] (6) Within 300 minutes, cut off the current passing through the silicon rod, adjust the current of the heater, and adjust the helium flow rate to 10% of the original flow rate to slowly adjust the silicon rod surface temperature to 150°C. Cut off the current of the heater and maintain the helium flow rate until the specified furnace start temperature is reached. Then stop the gas and start the furnace.
[0084] Embodiment 2, as Figure 6 As shown:
[0085] (1) using trichlorosilane and hydrogen to deposit in a reactor to obtain a silicon rod for zone melting;
[0086] (2) Within 90 minutes, reduce the trichlorosilane inlet flow rate to 0, slowly reduce the hydrogen flow rate to 20% of the initial flow rate, completely replace the chlorosilane in the reactor, and maintain the silicon rod surface temperature at 1000°C;
[0087] (3) Within 60 minutes, the surface temperature of the silicon rod is adjusted to 800°C;
[0088] (4) Within 60 minutes, replace the hydrogen in the reactor with high-purity helium. After the replacement is complete, adjust the flow rate of helium to be consistent with the final flow rate of hydrogen and maintain the temperature at 800°C;
[0089] (5) Within 180 minutes, the heater is implanted and powered on to maintain the surface temperature of the silicon rod at 800°C. When the heater is arranged in one group, it can be located above the center of the chassis. When multiple groups of heaters are arranged, they can be arranged above the center of the chassis and evenly arranged between the inner and outer layers;
[0090] (6) Within 360 minutes, cut off the current passing through the silicon rod, adjust the current of the heater, and adjust the helium flow rate to 10% of the original flow rate to slowly adjust the silicon rod surface temperature to 150°C. Cut off the current of the heater and maintain the helium flow rate until the specified furnace start temperature is reached. Then stop the gas and start the furnace.
[0091] Based on Example 2, a step-by-step cooling method is used in the fifth time period, and the cooling curve is as follows: Figure 7 shown.
[0092] Embodiment 3, as Figure 8 As shown:
[0093] (1) using trichlorosilane and hydrogen to deposit in a reactor to obtain a silicon rod for zone melting;
[0094] (2) Within 90 minutes, reduce the trichlorosilane inlet flow rate to 0, slowly reduce the hydrogen flow rate to 10% of the initial flow rate, completely replace the chlorosilane in the reactor, and maintain the silicon rod surface temperature at 1050°C;
[0095] (3) Within 60 minutes, the surface temperature of the silicon rod is adjusted to 900°C;
[0096] (4) Within 30 minutes, replace the hydrogen in the reactor with high-purity helium. After the replacement is complete, adjust the flow rate of helium to be consistent with the final flow rate of hydrogen and maintain the temperature at 900°C;
[0097] (5) Within 180 minutes, the heater is implanted and powered on to maintain the surface temperature of the silicon rod at 900°C. When the heater is arranged in one group, it can be located above the center of the chassis. When multiple groups of heaters are arranged, they can be arranged above the center of the chassis and evenly arranged between the inner and outer layers;
[0098] (6) Within 300 minutes, cut off the current passing through the silicon rod, adjust the current of the heater, and adjust the helium flow rate to 1% of the original flow rate to slowly adjust the silicon rod surface temperature to 150°C. Cut off the current of the heater and maintain the helium flow rate until the specified furnace start temperature is reached. Then stop the gas and start the furnace.
[0099] 20 rods produced under each working condition were used as samples to cut silicon cores to test their machining performance. The comparative example was silicon rods produced by conventional methods. The experimental results are shown in Table 1 below:
[0100] Table 1 Comparison of yields between comparative examples and embodiments
[0101] Comparative Example Example 1 Example 2 Example 3 Yield / % 80 95 90 95
[0102] It can be seen from Table 1 that the yields of Examples 1 to 3 using the present method are 10% to 15% higher than those of the comparative example. The present invention can prevent stress concentration and crack formation caused by uneven cooling.
[0103] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for eliminating residual stress inside a melting zone silicon rod, characterized in that: include: S10: using trichlorosilane and hydrogen to deposit in a reactor to obtain a silicon rod for zone melting; S20: In the first time period, the trichlorosilane inlet flow rate is reduced to 0, and the hydrogen flow rate is slowly reduced to 5% to 20% of the initial flow rate, so that the chlorosilane in the reactor is completely replaced, and the surface temperature of the silicon rod is maintained at T1; S30: In the second time period, adjusting the surface temperature of the silicon rod to T2; S40: In the third time period, the hydrogen in the reaction furnace is replaced with high-purity helium. After the replacement is complete, the flow rate of the helium is adjusted to be consistent with the final flow rate of the hydrogen, and the temperature is maintained at T2; S50: In the fourth time period, a heater is implanted in the reduction furnace and powered on to maintain the surface temperature of the silicon rod at T2; S60: In the fifth time period, the current passing through the silicon rod is cut off, the current of the heater is adjusted, and the helium flow rate is adjusted to 1% to 10% of the original flow rate to slowly adjust the surface temperature of the silicon rod to T3.
2. The method for eliminating residual stress inside a melt zone silicon rod according to claim 1, characterized in that: In step S20, the first time period is 30 minutes to 90 minutes, and the temperature T1 is 1000°C to 1050°C.
3. The method for eliminating residual stress inside a melt zone silicon rod according to claim 1, characterized in that: In step S30, the second time period takes 30 minutes to 60 minutes, and the temperature T2 is 800°C to 1000°C.
4. The method for eliminating residual stress inside a melt zone silicon rod according to claim 1, characterized in that: In step S40, the third time period is maintained for 30 minutes to 60 minutes.
5. The method for eliminating residual stress inside a melt zone silicon rod according to claim 1, characterized in that: In step S40, during the helium replacement process, gas replacement efficiency monitoring is added, and the steps include: S41: Install high-precision gas flow meters in the helium and hydrogen inlet pipes; S42: Connecting a gas analyzer to the reaction furnace to detect concentration changes of hydrogen and helium in real time; S43: Setting the permissible range of hydrogen concentration to determine whether it is completely replaced by helium; S44: According to the data of the gas analyzer and the gas flow meter, the flow rate of the helium is automatically adjusted through the central control system to optimize the replacement process.
6. The method for eliminating residual stress inside a melt zone silicon rod according to claim 1, characterized in that: In step S50, the fourth time period takes 60 minutes to 180 minutes.
7. The method for eliminating residual stress inside a melt zone silicon rod according to claim 1, characterized in that: In step S50, when the heaters are provided in a group, they are provided above the center of the chassis; when the heaters are provided in multiple groups, they are provided above the center of the chassis respectively and are evenly arranged between the inner and outer layers.
8. The method for eliminating residual stress inside a melt zone silicon rod according to claim 1, characterized in that: In step S50, a temperature feedback control system is also included to automatically adjust the heating power of the heater to maintain a stable temperature. The steps include: S51: using an infrared temperature measuring device to measure temperature data of the silicon rod surface and near the heater; S52: using a data acquisition system to transmit the signal of the infrared temperature measuring device to a central control system in real time; S53: Connecting the PID controller to the data acquisition system to ensure real-time acquisition of temperature data and output of control signals; S54: Setting a temperature setting value of the PID controller to ensure that the heater can maintain the temperature of the silicon rod surface stable at T2; S55: Connecting the thyristor regulator to the PID controller, and automatically adjusting the heating power of the heater according to the output signal of the PID controller.
9. The method for eliminating residual stress inside a melt zone silicon rod according to claim 1, characterized in that: In step S60, the fifth time period takes 180 minutes to 360 minutes, and the temperature T3 is not higher than 180°C.
10. The method for eliminating residual stress inside a melt zone silicon rod according to claim 1, characterized in that: In step S60, the process of cooling from the temperature T2 to the temperature T3 is divided into two stages of cooling. The cooling curve of the first stage is step-shaped. When the temperature drops to the temperature T3, the second stage of cooling begins. The second stage of cooling is a continuous rapid cooling stage.
Citation Information
Cited By
Furnace shutdown method for improving rod falling of electronic-grade polycrystalline silicon reduction furnace
CN121225599A
A method for improving the shutdown of an electronic grade polysilicon reduction furnace
CN121225599B