Silk fibroin microneedle electrode for multi-ion monitoring as well as preparation method and application of silk fibroin microneedle electrode
By preparing silk fibroin microneedle electrodes, the problem that the existing technology cannot monitor the concentration of multiple ions in human sweat in real time is solved, real-time monitoring of multiple ions in sweat is achieved, and good biocompatibility and anti-interference ability is achieved. Suitable for smart wearable devices.
Patent Information
- Application Number
- CN202411014756.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing wearable sensors cannot monitor the concentration of multiple ion in human sweat in real time at the molecular level, and the detection process is complex and inconvenient, making it impossible to achieve real-time display.
Using the preparation method of silk fibroin microneedle electrode, by adding aqueous polyurethane and crosslinking agent to the regenerated silk fibroin solution, pouring it into the PDMS mold and then removing it, performing magnetron sputtering treatment and depositing a metal layer, followed by electrochemical deposition Poly(3,4 ethylenedioxythiophene) polystyrene sulfonate, and finally coated with an ion-selective transmissive membrane, a silk fibroin microneedle electrode for multi-ion monitoring was prepared.
Real-time continuous monitoring of a variety of ions in human sweat is achieved, has good biocompatibility and anti-interference ability, can respond linearly and degrade, and is suitable for smart wearable devices.
Smart Images

Figure CN118961843A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of biomedical sensors, and in particular to a silk fibroin microneedle electrode for multi-ion monitoring, and a preparation method and application thereof. Background Art
[0002] Silk is a natural biomaterial with a wide range of sources and is renewable, meeting the requirements of sustainable development. Regenerated silk fibroin comes from silk, and its good biocompatibility, mechanical stability, sustainability and flexibility have great prospects in the fields of biomedical health, flexible electronic sensing, etc.
[0003] Wearable sensor technology is essential for achieving personalized medicine by continuously monitoring the health status of individuals. Human sweat contains a wealth of physiological information, and sampling it can achieve non-invasive monitoring of human biological signals. Considering the complexity of sweat, multiple screening of target biomarkers is essential, and a mature signal processing system is required to ensure the accuracy of the measurement. Wearable biosensors can achieve real-time and continuous monitoring of human biomarkers. Currently, commercially available wearable sensors can only monitor individual physical activities (such as running) and vital signs (such as heart rate), and cannot observe the user's health status at the molecular level. The detection of human sweat can make this molecular-level observation possible, because sweat contains a wealth of physiological and metabolic information, which can be detected non-invasively. Sweat analysis is currently used in applications such as disease diagnosis and drug testing. The sample collection and analysis processes of these applications are carried out separately, which cannot achieve real-time display of bioinformatics detection in sweat, and requires the use of bulky instruments for numerous laboratory analysis operations.
[0004] Therefore, a method for preparing a silk fibroin microneedle electrode with simple process, good biocompatibility and can be used for multi-ion monitoring is developed, which plays an important role in the continuous and stable monitoring of the concentrations of multiple ions in sweat. Summary of the invention
[0005] The purpose of the present invention is to solve the above problems in the prior art and provide a silk fibroin microneedle electrode for multi-ion monitoring and its preparation method and application. This microneedle electrode has good ion selectivity and good biocompatibility, and has broad application prospects in the fields of smart wearable devices and the like.
[0006] In order to achieve the above object, the present invention adopts the following technical scheme:
[0007] A method for preparing a silk fibroin microneedle electrode for multi-ion monitoring comprises the following steps:
[0008] 1) Adding waterborne polyurethane (WPU) solution and cross-linking agent to the regenerated silk fibroin solution and mixing them evenly, pouring the mixed solution into a PDMS mold containing a needle-shaped micropore array, removing bubbles in the solution, and demolding after drying to obtain regenerated silk fibroin microneedles;
[0009] 2) subjecting the regenerated silk fibroin microneedle to a magnetron sputtering treatment, depositing a metal layer of a certain thickness on the surface of the microneedle, and obtaining a regenerated silk fibroin microneedle electrode;
[0010] 3) electrochemically depositing a layer of poly(3,4-ethylenedioxythiophene) polystyrene sulfonate (PEDOT:PSS) on the surface of the regenerated silk fibroin microneedle electrode;
[0011] 4) dripping the ion selective permeable membrane mixed solution onto the silk fibroin microneedle electrode prepared in step 3), and letting it stand and dry to obtain a silk fibroin microneedle electrode that can be used for multi-ion monitoring.
[0012] In step 1), the cross-linking agent used is an aziridine cross-linking agent.
[0013] In step 2), the metals used for magnetron sputtering are gold (Au), silver (Ag), and platinum (Pt).
[0014] In step 3), the electrochemical deposition method includes a constant current electrochemical method, a constant voltage electrochemical method, and a cyclic voltammetry method.
[0015] In step 4), the ion selective permeable membrane includes a sodium ion selective permeable membrane, a potassium ion selective permeable membrane, and a calcium ion selective permeable membrane.
[0016] A layer of silver / silver chloride (Ag / AgCl) ink is coated on the surface of the regenerated silk fibroin microneedle electrode to obtain a reference electrode.
[0017] An application of a silk fibroin microneedle electrode for multi-ion monitoring is used to detect different ion signals in human sweat. The silk fibroin microneedle electrodes for different ion monitoring are placed on a screen-printed electrode sheet, and after the circuit is connected with conductive silver paste, a signal processing module, a Bluetooth signal transmission module, and a power module are added to form an intelligent wearable silk fibroin microneedle electrode array for multi-ion monitoring.
[0018] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0019] 1. The regenerated silk fibroin of the present invention has good biocompatibility. When used as the base material of the microneedle electrode on the skin, it will not produce adverse reactions and can be degraded after being discarded.
[0020] 2. The silk protein microneedle electrode used for ion monitoring has a linear response signal for detecting ions and has strong anti-interference ability for other interfering ions.
[0021] 3. Integrating silk fibroin microneedle electrodes for different ion monitoring into a smart wearable microneedle electrode array can achieve real-time and continuous monitoring of multiple components in human sweat. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a scanning electron microscope image of the silk fibroin microneedle of Example 1.
[0023] Figure 2 This is an optical photograph of the silk fibroin microneedle electrode used for multi-ion monitoring in Example 2.
[0024] Figure 3 This is a sodium ion signal test diagram of the silk fibroin microneedle electrode (conductive layer silver-plated) used for multi-ion monitoring in Example 1.
[0025] Figure 4 This is a sodium ion signal test diagram of the silk fibroin microneedle electrode (conductive layer gold-plated) used for multi-ion monitoring in Example 4. DETAILED DESCRIPTION
[0026] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention clearer and more understandable, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.
[0027] The present invention provides a method for preparing a silk fibroin microneedle electrode for detecting different ion signals in human sweat, comprising the following steps:
[0028] 1. Add waterborne polyurethane (WPU) solution and cross-linking agent to the regenerated silk fibroin solution and mix well. Pour the mixed solution into the PDMS mold containing the needle-shaped micropore array, evacuate in a vacuum drying oven to remove excess bubbles, dry in an oven and then demold to obtain regenerated silk fibroin microneedles.
[0029] 2. Take out the silk fibroin microneedle from the PDMS mold, use a magnetron sputtering instrument to perform magnetron sputtering on the surface of the silk fibroin microneedle to deposit a metal layer with a thickness of 30 to 50 nm, and obtain a silk fibroin microneedle electrode; the metal is selected from Au, Ag or Pt;
[0030] 3. Electrochemically deposit a layer of poly(3,4-ethylenedioxythiophene) polystyrene sulfonate (PEDOT:PSS) on the surface of the regenerated silk fibroin microneedle electrode; the electrochemical deposition method is selected from constant current electrochemical deposition, constant potential electrochemical deposition or cyclic voltammetry;
[0031] 4. Add the ion selective permeable membrane mixed solution dropwise onto the silk fibroin microneedle electrode prepared in step 3, and let it stand and dry to obtain a silk fibroin microneedle electrode that can be used for multi-ion monitoring; the ion selective permeable membrane is a sodium ion selective permeable membrane, a potassium ion selective permeable membrane, or a calcium ion selective permeable membrane.
[0032] A layer of silver / silver chloride (Ag / AgCl) ink is coated on the surface of the regenerated silk fibroin microneedle electrode to obtain a reference electrode.
[0033] In the present invention, the preparation of the silk protein solution is as follows: 80g of natural silk cocoons, 45g of sodium carbonate and 5L of deionized water are taken, heated to 100°C in an induction cooker, maintained for 20 to 30min, and repeated twice. Then put it into 5L of deionized water and heat it to 100°C again, repeat twice, remove the sericin in the silk, place it in a 65°C oven for drying, and obtain silk fiber. The dried silk fiber is dissolved in a 9.5M lithium bromide solution at 65°C, the added mass ratio of silk fiber to lithium bromide solution is 1:7, and the dissolution time is about 6h. After the silk fiber is completely dissolved in the lithium bromide solution, it is taken out after cooling and placed in a dialysis bag and dialyzed in deionized water for 3 days, and then filtered to obtain a pure silk solution, centrifuged and filtered again, and placed in a 4°C refrigerator for standby use.
[0034] The silk fibroin microneedle electrode for multi-ion monitoring prepared by the above method includes a silk fibroin microneedle, a magnetron sputtering conductive layer, a polymer conductive layer and an ion selective permeable membrane arranged in sequence; the needle tip part of the silk fibroin microneedle is a micron-scale needle structure with a height of 400 to 800 μm, which is achieved by adjusting the size of the mold.
[0035] Example 1
[0036] 1. After the regenerated silk protein solution and WPU (waterborne polyurethane) are mixed evenly, aziridine crosslinking agent is added and crosslinked in an oven at 60-65°C for 10 minutes. The mixed solution is poured into a PDMS microneedle mold with a needle tip height of 500 μm, and the excess bubbles are removed in a vacuum drying oven, and finally placed in a 65°C oven to dry for 8 hours.
[0037] 2. Take out the silk fibroin microneedle from the PDMS mold, and use a magnetron sputtering instrument to perform magnetron sputtering on the surface of the silk fibroin microneedle to deposit a layer of metallic silver (Ag) with a thickness of 30 to 50 nm to obtain a silk fibroin microneedle electrode.
[0038] 3. Coat a layer of silver / silver chloride (Ag / AgCl) ink on the surface of the silk fibroin microneedle electrode and place it in a fume hood to dry overnight to obtain a reference electrode.
[0039] 4. Place the silk fibroin microneedle electrode in a potassium chloride (KCl) solution in which polymer monomers 3,4-ethylenedioxythiophene (EDOT) and polystyrene sulfonate (PSS) are dispersed, and the pH of the solution is adjusted to 1. After setting the parameters by constant current electrochemical deposition method, a layer of poly (3,4-ethylenedioxythiophene): polystyrene sulfonate (PEDOT:PSS) is deposited on the surface of the silk fibroin microneedle electrode.
[0040] 5. Add 20 μL of the sodium ion selective permeable membrane mixed solution prepared by mixing in a fixed ratio onto the silk fibroin microneedle electrode, place it in a fume hood to dry overnight, and obtain a silk fibroin microneedle electrode for sodium ion monitoring.
[0041] Specifically, the preparation of the sodium ion selective permeable membrane mixed solution is as follows: sodium ion carrier X, dioctyl sebacate (DOS), sodium tetraborate (Na-TFPB), and high molecular weight polyvinyl chloride (PVC) are uniformly mixed in a mass ratio of 1:0.55:33:65.45 and dissolved in 660 μL of tetrahydrofuran (THF) to obtain a sodium ion selective permeable membrane mixed solution.
[0042] 6. Using an electrochemical workstation, the silk fibroin microneedle electrode used for sodium ion monitoring is used as the working electrode, and the platinum sheet is used as the counter electrode and the reference electrode obtained in step 3. After connecting the test circuit, the ion concentration signal can be converted into an open circuit voltage, thereby realizing the detection of solutions with different sodium ion concentrations.
[0043] Example 2
[0044] 1. After the regenerated silk protein solution and WPU (waterborne polyurethane) are mixed evenly, aziridine crosslinking agent is added and crosslinked in an oven at 60-65°C for 10 minutes. The mixed solution is poured into a PDMS microneedle mold with a needle tip height of 500 μm, and the excess bubbles are removed in a vacuum drying oven, and finally placed in a 65°C oven to dry for 8 hours.
[0045] 2. Take out the silk fibroin microneedle from the PDMS mold, and use a magnetron sputtering instrument to perform magnetron sputtering on the surface of the silk fibroin microneedle to deposit a layer of metal gold (Au) with a thickness of 30 to 50 nm, thereby obtaining a silk fibroin microneedle electrode.
[0046] 3. Coat a layer of silver / silver chloride (Ag / AgCl) ink on the surface of the silk fibroin microneedle electrode and place it in a fume hood to dry overnight to obtain a reference electrode.
[0047] 4. Place the silk fibroin microneedle electrode in a potassium chloride (KCl) solution in which polymer monomers 3,4-ethylenedioxythiophene (EDOT) and polystyrene sulfonate (PSS) are dispersed, and the pH of the solution is adjusted to 1. After setting the parameters by constant current electrochemical deposition method, a layer of poly (3,4-ethylenedioxythiophene): polystyrene sulfonate (PEDOT:PSS) is deposited on the surface of the silk fibroin microneedle electrode.
[0048] 5. Add 20 μL of the potassium ion selective permeable membrane mixed solution prepared by mixing in a fixed ratio onto the silk fibroin microneedle electrode, place it in a fume hood to dry overnight, and obtain a silk fibroin microneedle electrode for potassium ion monitoring.
[0049] Specifically, the preparation of the potassium ion selective permeable membrane mixed solution is as follows: valinomycin, dioctyl sebacate (DOS), sodium tetraborate (Na-TFPB), and high molecular weight polyvinyl chloride (PVC) are uniformly mixed in a mass ratio of 2:0.5:32.7:64.7 and then dissolved in a cyclohexanone solution to obtain a potassium ion selective permeable membrane mixed solution.
[0050] 6. Using an electrochemical workstation, the silk fibroin microneedle electrode used for potassium ion monitoring is used as the working electrode, and the platinum sheet is used as the counter electrode and the reference electrode obtained in step 3. After connecting the test circuit, the ion concentration signal can be converted into an open circuit voltage, and the detection of solutions with different potassium ion concentrations can be realized.
[0051] Example 3
[0052] 1. After the regenerated silk protein solution and WPU (waterborne polyurethane) are mixed evenly, aziridine crosslinking agent is added and crosslinked in an oven at 60-65°C for 10 minutes. The mixed solution is poured into a PDMS microneedle mold with a needle tip height of 500um, and the excess bubbles are removed in a vacuum drying oven, and finally placed in a 65°C oven to dry for 8 hours.
[0053] 2. Take out the silk fibroin microneedle from the PDMS mold, and use a magnetron sputtering instrument to perform magnetron sputtering on the surface of the silk fibroin microneedle to deposit a layer of metal gold (Au) with a thickness of 30 to 50 nm, thereby obtaining a silk fibroin microneedle electrode.
[0054] 3. Coat a layer of silver / silver chloride (Ag / AgCl) ink on the surface of the silk fibroin microneedle electrode and place it in a fume hood to dry overnight to obtain a reference electrode.
[0055] 4. Place the silk fibroin microneedle electrode in a potassium chloride (KCl) solution in which polymer monomers 3,4-ethylenedioxythiophene (EDOT) and polystyrene sulfonate (PSS) are dispersed, and the pH of the solution is adjusted to 1. After setting the parameters by constant current electrochemical deposition method, a layer of poly (3,4-ethylenedioxythiophene): polystyrene sulfonate (PEDOT:PSS) is deposited on the surface of the silk fibroin microneedle electrode.
[0056] 5. Add 20 μL of the calcium ion selective permeable membrane mixed solution prepared by mixing in a fixed ratio onto the silk fibroin microneedle electrode, place it in a fume hood to dry overnight, and obtain a silk fibroin microneedle electrode for calcium ion monitoring.
[0057] The preparation of the calcium ion selective permeable membrane mixed solution is as follows: calcium ion carrier II, dioctyl sebacate (DOS), sodium tetraborate (Na-TFPB), and high molecular weight polyvinyl chloride (PVC) are mixed evenly in a mass ratio of 1:0.55:33:65.45 and then dissolved in 660uL of tetrahydrofuran (THF) to obtain a calcium ion selective permeable membrane mixed solution.
[0058] 6. Using an electrochemical workstation, the silk fibroin microneedle electrode used for calcium ion monitoring is used as the working electrode, and the platinum sheet is used as the counter electrode and the reference electrode obtained in step 3. After connecting the test circuit, the ion concentration signal can be converted into an open circuit voltage, thereby realizing the detection of solutions with different calcium ion concentrations.
[0059] Example 4
[0060] The difference from Example 1 is that the metal magnetron sputtered in step 2 is gold (Au).
[0061] like Figure 1 It is a scanning electron microscope picture of a silk fibroin microneedle, and the microneedle tip part of the silk fibroin microneedle is very complete.
[0062] Figure 2 This is an optical photograph of a silk fibroin microneedle electrode for multi-ion monitoring. The silk fibroin microneedle electrode array is arranged neatly and regularly.
[0063] like Figure 3 and Figure 4 This is a sodium ion signal test diagram of a silk fibroin microneedle electrode (the conductive layers are silver-plated and gold-plated, respectively) used for multi-ion monitoring. The test results of the silk fibroin microneedle electrode show good linearity within the normal sodium ion concentration range of the human body.
Claims
1. A method for preparing a silk fibroin microneedle electrode for multi-ion monitoring. It is characterized in that The following steps are involved: 1) adding an aqueous polyurethane solution and a cross-linking agent to a regenerated silk fibroin solution and mixing them evenly, pouring the mixed solution into a PDMS mold containing a needle-shaped micropore array, removing bubbles in the solution, and demolding after drying to obtain regenerated silk fibroin microneedles; 2) subjecting the regenerated silk fibroin microneedle to a magnetron sputtering treatment, depositing a metal layer of a certain thickness on the surface of the microneedle, and obtaining a regenerated silk fibroin microneedle electrode; 3) electrochemically depositing a layer of poly(3,4-ethylenedioxythiophene) polystyrene sulfonate on the surface of the regenerated silk fibroin microneedle electrode; 4) dripping the ion selective permeable membrane mixed solution onto the silk fibroin microneedle electrode prepared in step 3), and letting it stand and dry to obtain a silk fibroin microneedle electrode that can be used for multi-ion monitoring.
2. A method for preparing a silk fibroin microneedle electrode for multi-ion monitoring according to claim 1, Features: In step 1), the cross-linking agent used is an aziridine cross-linking agent.
3. A method for preparing a silk fibroin microneedle electrode for multi-ion monitoring according to claim 1, Features: In step 2), the metals used for magnetron sputtering are gold, silver and platinum.
4. A method for preparing a silk fibroin microneedle electrode for multi-ion monitoring according to claim 1, Features: In step 3), the electrochemical deposition method includes a constant current electrochemical method, a constant voltage electrochemical method, and a cyclic voltammetry method.
5. A method for preparing a silk fibroin microneedle electrode for multi-ion monitoring according to claim 1, Features: In step 4), the ion selective permeable membrane includes a sodium ion selective permeable membrane, a potassium ion selective permeable membrane, and a calcium ion selective permeable membrane.
6. A silk fibroin microneedle electrode for multi-ion monitoring, Features: The invention is prepared by the preparation method according to any one of claims 1 to 5.
7. Use of the silk fibroin microneedle electrode for multi-ion monitoring as claimed in claim 6, Features: Used to detect different ion signals in human sweat.
8. The use of a silk fibroin microneedle electrode for multi-ion monitoring as claimed in claim 6, Features: The silk fibroin microneedle electrodes used for monitoring different ions are placed on the screen-printed electrode sheet. After the circuit is connected with conductive silver paste, a signal processing module, a Bluetooth signal transmission module and a power module are added to form an intelligent wearable silk fibroin microneedle electrode array for multi-ion monitoring.
Citation Information
Patent Citations
SFL microcarrier for cell culture as well as preparation method and application of SFL microcarrier
CN106834204A
Silk microneedle electrode and preparation method thereof
CN109171699A
Conductive silk fibroin film as well as preparation method and application thereof
CN113174074A
Wearable microneedle sensor for tissue fluid detection and preparation method thereof
CN114778643A
Preparation method of microneedle array for multi-ion monitoring and wearable monitoring system
CN116269361A