High-flexibility torsion-resistant robot cable copper conductor and preparation method thereof

Through Nihoff Dat pull, multi-head pull, beam twisting, re-twist and 3D graphene modification technology, a copper conductor of high-flexible torsion-resistant robot cable was prepared, which solved the problem of insufficient bending performance of existing conductors and achieved high strength, The improvement of high flexibility and torsion resistance meets the demand for high-performance cables of industrial robots.

CN118969362AActive Publication Date: 2024-11-15JIANGSU XINHAI HIGH-TECH NEW MATERIAL CO LTD

Patent Information

Application Number
CN202411187381.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-15
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

The existing robot cable copper conductors have insufficient bending performance in medium and high frequency torque and bending stress scenarios, resulting in the bending performance of conductor materials ranging from 5 to 8 million times, which cannot meet the demand for high flexibility and torsion resistance of industrial robots, and rely on high imports. Massive copper conductor materials restrict the development of domestic industrial robots.

Method used

High-flexible torsion-resistant robot cable copper conductors are prepared by Nihoff Dallas, Nihoff multi-head pulling, beam twisting, and retwisting processes. The high strength, high flexibility and torsion resistance of the conductor are ensured through surface decomposition and annealing processes, combined with Compatibility of 3D graphene with copper substrate improves conductivity and flexibility.

Benefits of technology

The bending performance of the copper conductor of robot cable has reached more than 12 million times, reducing production costs, improving the overall performance and processing yield of the conductor, meeting the demand for high flexibility and torsion resistance of industrial robots, and reducing the number of imported materials. rely.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005013893480000161
    Figure BDA0005013893480000161
  • Figure BDA0005013893480000171
    Figure BDA0005013893480000171
Patent Text Reader

Abstract

The invention relates to the technical field of flexible cables, in particular to a high-flexibility torsion-resistant robot cable copper conductor and a preparation method thereof. The high-flexibility torsion-resistant robot cable copper conductor is prepared by performing Nihoff large pulling, Nihoff multi-head pulling, bunch stranding and compound stranding on a copper rod. Wiredrawing annealing and stranding equipment is adopted for fine machining, the phenomena of wire breakage, oxidation and the like are avoided in the wiredrawing annealing process, the stranded outer diameter of the prepared robot cable copper conductor is smaller than or equal to 3.3 mm, the direct-current resistance is smaller than or equal to 3.3 ohm / km, and the robot cable copper conductor has the advantages of being high in strength, high in flexibility, good in torsion resistance and high in safety.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flexible cables, and in particular to a highly flexible and torsion-resistant robot cable copper conductor and a preparation method thereof. Background Art

[0002] With the rapid development of science and technology and the continuous upgrading of the industrial production market, industrial robots have gradually broken away from the constraints of traditional single-purpose robots and developed in a more complex and multifunctional direction. In this context, the replacement of manpower by machines has become an irreversible trend, heralding the arrival of the era of industrial robots.

[0003] my country's industrial robot market is developing rapidly, accounting for about one-third of the global market share, and is the world's largest industrial robot application market. At present, the demand for intelligent transformation and upgrading of my country's manufacturing is becoming increasingly prominent, and the market demand for industrial robots remains strong. According to statistics, my country's industrial robot sales in 2018 reached US$6.23 billion, and it is predicted that sales in 2024 will exceed US$19 billion.

[0004] As an important part of robots, the market demand for wires and cables has shown explosive growth. As a carrier and important component of power transmission and control capabilities, robot cables are particularly important for the normal operation of robots. It plays a role similar to the human central nervous system. Once any link goes wrong, the entire system will not work properly.

[0005] As industrial robot technology matures, the application of industrial robots has begun to spread rapidly. Robot cables not only need to have excellent electrical conductivity and mechanical properties, but also must have unique high flexibility and torsion resistance to meet the needs of different environments and application scenarios. With the rapid growth of the robotics industry, the use environment is becoming more and more harsh, and the requirements for robot cables are also getting higher and higher. High flexibility and torsion resistance are the most concerned aspects of robot cable use.

[0006] Robot cables must have good advantages such as high flexibility and torsion resistance. This requires not only that the outer layer of the cable has good electrical insulation, flexibility, and impact resistance, but also that the robot cable core conductor has good conductivity, mechanical properties, and high flexibility and torsion resistance. At present, the bending performance of the copper conductor material of the robot cable whisker suitable for installation in medium and high frequency torque and bending stress scenarios is required to be more than 8 million times. With the development of industrial robots, the bending performance requirements for the copper conductor material of the robot cable whisker will become higher and higher. The bending performance of the copper conductor material of the domestic robot cable whisker is generally between 5 and 8 million. High-quality copper conductor materials still rely on imports, which restricts the development of my country's industrial robots. To this end, the inventor provides a high-flexibility and torsion-resistant robot cable copper conductor and a preparation method thereof. Summary of the invention

[0007] In order to solve the difficulties existing in the prior art, the inventor provides a highly flexible and torsion-resistant robot cable copper conductor and a preparation method thereof. The robot cable copper conductor has a twisted outer diameter of ≤3.3mm, a DC resistance of ≤3.3Ω / km, and a bending performance of ≥12 million times.

[0008] The invention provides a highly flexible and torsion-resistant robot cable copper conductor, which is realized by the following technical solutions:

[0009] A highly flexible and torsion-resistant robot cable copper conductor is prepared by a copper rod through Niehoff pulling, Niehoff multi-head pulling, bundle twisting, and multiple twisting; the highly flexible and torsion-resistant robot cable copper conductor has a twisted outer diameter of ≤3.3mm and a DC resistance of ≤3.3Ω / km.

[0010] The present invention adopts wire drawing annealing and twisting equipment for fine processing. No wire breakage, oxidation and the like occur during the wire drawing annealing process. The prepared robot cable copper conductor has a twisted outer diameter of ≤3.3mm and a DC resistance of ≤3.3Ω / km. It has the advantages of high strength, high flexibility, good torsion resistance and high safety.

[0011] The present invention provides a method for preparing a highly flexible and torsion-resistant robot cable copper conductor, which is achieved by the following scheme:

[0012] A method for preparing a highly flexible and torsion-resistant robot cable copper conductor comprises the following steps:

[0013] Step 1: Perform surface impurity removal treatment on the raw material copper rod to remove oil stains and oxides on the raw material copper rod;

[0014] Step 2: input the copper rod that has been subjected to the impurity removal treatment in step 1 into a Niehof double-head drawing machine for Niehof drawing treatment, and process the copper rod that has been subjected to the Niehof drawing treatment into a busbar with a diameter of 1.82 mm to 1.84 mm;

[0015] Step 3, inputting the busbar with a diameter of 1.82 mm to 1.84 mm in step 2 into a Nihoff multi-head wire drawing machine for Nihoff multi-head drawing, and processing the busbar after Nihoff multi-head drawing into a copper wire with a diameter of 0.200 to 0.202 mm;

[0016] Step 4, inputting a number of copper wires with a diameter of 0.200-0.202 mm obtained in step 3 into a high-speed stranding machine for bundle stranding, and obtaining a copper wire bundle with a diameter of 1.25±0.02 mm after the bundle stranding process;

[0017] Step 5: Input the copper wire bundle with a diameter of 1.25±0.02mm obtained in step 4 into a high-speed stranding machine for re-twisting to obtain a high-flexibility and torsion-resistant robot cable copper conductor with a diameter of 3.2±0.02mm and a DC resistance of ≤3.3Ω / km.

[0018] The preparation method provided by the present invention has low operational difficulty, is easy to implement industrialized manufacturing, and reduces overall production costs.

[0019] Preferably, the diameter of the raw material copper rod described in step one is 8±0.05 mm; the raw material copper rod is made of pure copper or copper alloy.

[0020] Preferably, the raw material copper rod is a copper alloy, and the copper alloy copper rod is extruded or integrally cast from a copper rod; the copper alloy includes 3D graphene and copper, and the content of the 3D graphene is 0.5-2wt%; the surface of the 3D graphene is doped with at least one of nano-copper clusters, nano-silver clusters, single-atom copper, and single-atom silver; the 3D graphene has 3-4 layers, a thickness of 1.3-1.4nm, a size of 0.5-8 microns, and a conductivity of >3000S / m.

[0021] By adopting the above technical solution, the copper conductor processing performance, thermal conductivity and flexibility of the prepared robot cable can be improved.

[0022] Preferably, the 3D graphene content is 1.0-1.5wt%; the surface of the 3D graphene is doped with single-atom copper and single-atom silver; the mass ratio of the single-atom copper to the single-atom silver is (2-4):1; the mass ratio of the total doping mass of the single-atom copper and the single-atom silver to the 3D graphene is 1:(20-50).

[0023] In the present invention, 3D graphene with surface modified by single-atom copper and single-atom silver is used to make the 3D graphene have good compatibility with the copper substrate, so that the 3D graphene can be evenly dispersed inside the copper substrate through a traditional melt casting process, which can not only effectively improve the conductivity of the prepared robot cable copper conductor, but also improve the ductility, flexibility, processing lubrication performance and surface cleanliness of the robot cable copper conductor, thereby improving the overall processing yield of the robot cable copper conductor.

[0024] Preferably, in the step 2, the copper rod that has undergone impurity removal treatment in the step 1 is input into a Niehoff double-head drawing machine for Niehoff drawing treatment: drawing liquid temperature: 35-45°C, annealing coefficient: 7.5-8.5, coolant temperature: 35-45°C, equipment speed: 25-28m / S, and the copper rod that has undergone Niehoff drawing treatment is processed into a busbar with a diameter of 1.82mm-1.84mm.

[0025] Preferably, in the step three, the busbar with a diameter of 1.82 mm to 1.84 mm in the step two is input into a Nihof multi-head wire drawing machine for Nihof multi-head drawing treatment: wire drawing liquid temperature: 35 to 45°C, wire drawing oil concentration: 4% to 9%, annealing liquid temperature: 35 to 45°C, annealing liquid concentration: 0.5% to 1.0%, annealing coefficient: 8.0 to 9.2, line speed: 24 to 28 m / s, and the busbar treated with Nihof multi-head drawing is processed into a copper wire with a diameter of 0.200 to 0.202 mm.

[0026] Preferably, in the step four, several copper wires with a diameter of 0.200-0.202 mm in step three are input into a high-speed stranding machine for bundle twisting processing: wire pay-off tension: 15±2N, wire take-up tension: 35±5%, rotation speed: 3200±200TPM, wire branching structure: 3+1, mold: 1.25±0.02mm, and after bundle twisting processing, a copper wire bundle with a diameter of 1.25±0.02mm is obtained.

[0027] Preferably, in the step five, the copper wire bundle with a diameter of 1.25±0.02mm obtained in the step four is input into a high-speed stranding machine for re-twisting processing: pay-off tension: 35±2N, take-up tension: 100±5N, rotation speed: 1600±200TPM, branching structure: 1+6, mold: 3.2±0.02mm, so as to obtain a high-flexibility and torsion-resistant robot cable copper conductor with a diameter of 3.2±0.02mm and a DC resistance of ≤3.3Ω / km.

[0028] By studying the influence of annealing coefficient on the elongation of the wire, the annealing coefficient is adjusted online in real time according to the change of the wire elongation, so as to control the change of temperature difference, make the elongation of the wire within a certain range, and achieve uniform softness of different batches of wires, thereby ensuring that the prepared robot cable copper conductor has the advantages of high strength, high flexibility, good torsion resistance and high safety.

[0029] Preferably, the method for preparing the highly flexible and torsion-resistant robot cable copper conductor comprises the following steps:

[0030] Step 1: Perform surface impurity removal treatment on a copper rod with a diameter of 8±0.05 mm to remove oil stains and oxides from the copper rod;

[0031] Step 2: The copper rod treated with impurities in step 1 is input into a Niehof double-head drawing machine for Niehof drawing: drawing liquid temperature: 40°C, annealing coefficient: 8.5, coolant temperature: 45°C, equipment speed: 26m / S, and the copper rod treated with Niehof drawing is processed into a busbar with a diameter of 1.82mm to 1.84mm;

[0032] Step 3, input the busbar with a diameter of 1.82 mm to 1.84 mm in step 2 into a Nihoff multi-head wire drawing machine for Nihoff multi-head drawing treatment: wire drawing liquid temperature: 40°C, wire drawing oil concentration: 8%, annealing liquid temperature: 40°C, annealing liquid concentration: 0.8%, annealing coefficient: 9.0, line speed: 28 m / s, and the busbar treated by Nihoff multi-head drawing is processed into a copper wire with a diameter of 0.200 to 0.202 mm;

[0033] Step 4, inputting several copper wires with a diameter of 0.200-0.202 mm in step 3 into a high-speed stranding machine for bundle stranding: setting the wire tension to 15N, setting the wire tension to 35%, setting the speed to 3000 TPM, the wire splitting structure to 3+1, and the die to 1.25±0.02 mm, and obtaining a copper wire bundle with a diameter of 1.25±0.02 mm after the bundle stranding process;

[0034] Step 5. Input the copper wire bundle with a diameter of 1.25±0.02mm obtained in step 4 into a high-speed stranding machine for re-twisting: pay-off tension: 35N, take-up tension: 100N, rotation speed: 1500TPM, branching structure: 1+6, mold: 3.2±0.02mm, and you can get a high-flexibility and torsion-resistant robot cable copper conductor with a diameter of 3.2±0.02mm and a DC resistance of ≤3.3Ω / km.

[0035] Through experimental research, a preparation method for industrially producing high-quality cable copper conductors was obtained. This not only ensures that the robot cable copper conductors have the advantages of high strength, high flexibility, good torsion resistance and high safety, but also reduces energy consumption and improves the processing yield of robot cable copper conductors, which is beneficial to optimize the cost of robot cable copper conductors and enhance core competitiveness.

[0036] In summary, the present invention has the following advantages:

[0037] 1. The present invention adopts wire drawing annealing and twisting equipment for fine processing. No wire breakage, oxidation and the like occur during the wire drawing annealing process, which can effectively improve the torsional flexibility of the copper conductor of the robot cable and ensure the overall conductive performance and safe use.

[0038] 2. Through the study of the influence of annealing coefficient on the elongation of the wire, the annealing coefficient is adjusted online in real time according to the change of the wire elongation, so as to control the change of temperature difference, make the elongation of the wire within a certain range, and achieve uniform softness of different batches of wires, thereby ensuring that the copper conductor of the robot cable has the advantages of high strength, high flexibility, good torsion resistance and high safety.

[0039] 3. Due to the special usage of the robot, torsional movement will occur, so there are special requirements for the softness of the conductor and the smoothness of the surface. To ensure the softness of the cable, it is necessary to first use several annealed soft copper wires to synthesize the strands, and then use the double twisting method to twist the core to ensure the torsional flexibility and conductivity of the robot cable copper conductor.

[0040] 4. The preparation method provided by the present invention has low operational difficulty, is easy to implement industrialized manufacturing, and reduces production costs.

[0041] 5. In the present invention, by using 3D graphene with surface modified by single-atom copper + silver, the 3D graphene has good compatibility with the copper substrate, so that the 3D graphene can be evenly dispersed inside the copper substrate through the traditional melt casting process, which can not only effectively improve the conductivity of the prepared robot cable copper conductor, but also improve the ductility, flexibility, processing lubrication performance and surface cleanliness of the robot cable copper conductor, thereby improving the overall processing yield of the robot cable copper conductor. DETAILED DESCRIPTION

[0042] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples and comparative examples.

[0043] A high-flexibility and torsion-resistant robot cable copper conductor is prepared from a copper rod through Niehoff large-stretching, Niehoff multi-stretching, bundle twisting, and multiple twisting. The prepared high-flexibility and torsion-resistant robot cable copper conductor has a twisted outer diameter of ≤3.3mm and a DC resistance of ≤3.3Ω / km.

[0044] A method for preparing a highly flexible and torsion-resistant robot cable copper conductor comprises the following steps:

[0045] Step 1: Perform surface impurity removal treatment on the raw material copper rod to remove oil stains and oxides on the raw material copper rod;

[0046] Preferably, the raw material copper rod described in step 1 has a diameter of 8±0.05 mm; the raw material copper rod is made of pure copper or copper alloy; further preferably, the raw material copper rod is a copper alloy, and the copper rod made of copper alloy is extruded or integrally cast from a copper rod; the copper alloy includes 3D graphene and copper, and the 3D graphene content is 0.5-2wt%; the surface of the 3D graphene is doped with at least one of nano-copper clusters, nano-silver clusters, single-atom copper, and single-atom silver; the number of layers of the 3D graphene is 3-4, the thickness is 1.3-1.4nm, the size is 0.5-8 microns, and the conductivity is>3000S / m;

[0047] Preferably, in step 2, the copper rod subjected to the impurity removal treatment in step 1 is input into a Niehof double-head drawing machine for Niehof drawing treatment, and the copper rod subjected to the Niehof drawing treatment is processed into a busbar with a diameter of 1.82 mm to 1.84 mm;

[0048] Step 2: Input the copper rod treated with impurities in step 1 into a Niehof double-head drawing machine for Niehof drawing: wire drawing liquid temperature: 35-45°C, annealing coefficient: 7.5-8.5, coolant temperature: 35-45°C, equipment speed: 25-28m / S, and process the copper rod treated with Niehof drawing into a busbar with a diameter of 1.82mm-1.84mm;

[0049] Step 3, inputting the busbar with a diameter of 1.82 mm to 1.84 mm in step 2 into a Nihoff multi-head wire drawing machine for Nihoff multi-head drawing, and processing the busbar after Nihoff multi-head drawing into a copper wire with a diameter of 0.200 to 0.202 mm;

[0050] Preferably, in step three, the busbar with a diameter of 1.82 mm to 1.84 mm in step two is input into a Niehof multi-head wire drawing machine for Niehof multi-head drawing treatment: wire drawing liquid temperature: 35 to 45 ° C, wire drawing oil concentration: 4% to 9%, annealing liquid temperature: 35 to 45 ° C, annealing liquid concentration: 0.5% to 1.0%, annealing coefficient: 8.0 to 9.2, line speed: 24 to 28 m / s, and the busbar treated by Niehof multi-head drawing is processed into a copper wire with a diameter of 0.200 to 0.202 mm;

[0051] Step 4, inputting a number of copper wires with a diameter of 0.200-0.202 mm obtained in step 3 into a high-speed stranding machine for bundle stranding, and obtaining a copper wire bundle with a diameter of 1.25±0.02 mm after the bundle stranding process;

[0052] Preferably, in step 4, the copper wires with a diameter of 0.200-0.202 mm in step 3 are input into a high-speed stranding machine for bundle stranding: pay-off tension: 15±2N, take-up tension: 35±5%, rotation speed: 3200±200TPM, wire splitting structure: 3+1, mold: 1.25±0.02mm, and a copper wire bundle with a diameter of 1.25±0.02mm is obtained after bundle stranding;

[0053] Step 5: Input the copper wire bundle with a diameter of 1.25±0.02mm obtained in step 4 into a high-speed stranding machine for re-twisting to obtain a high-flexibility and torsion-resistant robot cable copper conductor with a diameter of 3.2±0.02mm and a DC resistance of ≤3.3Ω / km.

[0054] Preferably, in step five, the copper wire bundle with a diameter of 1.25±0.02mm obtained in step four is input into a high-speed stranding machine for re-twisting: pay-off tension: 35±2N, take-up tension: 100±5N, rotation speed: 1600±200TPM, branching structure: 1+6, mold: 3.2±0.02mm, so as to obtain a high-flexibility and torsion-resistant robot cable copper conductor with a diameter of 3.2±0.02mm and a DC resistance of ≤3.3Ω / km.

[0055] Preferably, the 3D graphene content is 1.0-1.5wt%; the surface of the 3D graphene is doped with single-atom copper and single-atom silver; the mass ratio of the single-atom copper and the single-atom silver is (2-4):1; the mass ratio of the total doping mass of the single-atom copper and the single-atom silver to the 3D graphene is 1:(20-50).

[0056] Through experimental research, a preparation method for industrialized high-quality production of cable copper conductors was obtained, as follows:

[0057] Step 1: Perform surface impurity removal treatment on a copper rod with a diameter of 8±0.05 mm to remove oil stains and oxides from the copper rod;

[0058] Step 2: The copper rod treated with impurities in step 1 is input into a Niehof double-head drawing machine for Niehof drawing: drawing liquid temperature: 40°C, annealing coefficient: 8.5, coolant temperature: 45°C, equipment speed: 26m / S, and the copper rod treated with Niehof drawing is processed into a busbar with a diameter of 1.82mm to 1.84mm;

[0059] Step 3, input the busbar with a diameter of 1.82 mm to 1.84 mm in step 2 into a Nihoff multi-head wire drawing machine for Nihoff multi-head drawing treatment: wire drawing liquid temperature: 40°C, wire drawing oil concentration: 8%, annealing liquid temperature: 40°C, annealing liquid concentration: 0.8%, annealing coefficient: 9.0, line speed: 28 m / s, and the busbar treated by Nihoff multi-head drawing is processed into a copper wire with a diameter of 0.200 to 0.202 mm;

[0060] Step 4, inputting several copper wires with a diameter of 0.200-0.202 mm in step 3 into a high-speed stranding machine for bundle stranding: setting the wire tension to 15N, setting the wire tension to 35%, setting the speed to 3000 TPM, the wire splitting structure to 3+1, and the die to 1.25±0.02 mm, and obtaining a copper wire bundle with a diameter of 1.25±0.02 mm after the bundle stranding process;

[0061] Step 5. Input the copper wire bundle with a diameter of 1.25±0.02mm obtained in step 4 into a high-speed stranding machine for re-twisting: pay-off tension: 35N, take-up tension: 100N, rotation speed: 1500TPM, branching structure: 1+6, mold: 3.2±0.02mm, and you can get a high-flexibility and torsion-resistant robot cable copper conductor with a diameter of 3.2±0.02mm and a DC resistance of ≤3.3Ω / km.

[0062] The above preparation method can not only ensure that the copper conductor of the robot cable has the advantages of high strength, high flexibility, good torsion resistance and high safety, but also reduce energy consumption and improve the processing yield rate of the copper conductor of the robot cable, which is beneficial to optimize the cost of the copper conductor of the robot cable and enhance core competitiveness.

[0063] Embodiment 1: A method for preparing a highly flexible and torsion-resistant robot cable copper conductor comprises the following steps:

[0064] Step 1: Perform surface impurity removal treatment on a pure copper rod with a diameter of 8±0.05 mm: first, use 2000 mesh corundum to perform surface sandblasting to remove oxides on the surface of the pure copper rod, then rinse it twice with an ethanol aqueous solution (ethanol / deionized water volume ratio = 1:2), then rinse it twice with an acetone aqueous solution (acetone / deionized water volume ratio = 1:9), and finally rinse it three times with deionized water, and dry it to complete the pure copper rod with impurity removal treatment;

[0065] Step 2: Input the pure copper rod with a diameter of 8±0.05 mm that has been treated with impurities in step 1 into the MSM86 Niehof double-head drawing machine for Niehof drawing: wire drawing liquid (JY-9077F fully synthetic copper wire drawing liquid, concentration 5%, pH value: 8.5±0.5) temperature: 40°C, annealing coefficient: 8.5, coolant temperature: 45°C, equipment speed: 26m / S, and the copper rod treated with Niehof drawing is processed into a busbar with a diameter of 1.82mm-1.84mm;

[0066] Step 3, input the busbar with a diameter of 1.82 mm to 1.84 mm in step 2 into the MMH series Niehof multi-head wire drawing machine for Niehof multi-head drawing treatment: wire drawing liquid temperature: 40°C, wire drawing oil concentration in JY-9077F fully synthetic copper wire drawing liquid: 8%, annealing liquid (copper wire annealing liquid C500MT) temperature: 40°C, copper wire annealing liquid C500MT concentration: 0.8%, annealing coefficient: 9.0, line speed: 28 m / s, the busbar processed by Niehof multi-head drawing is processed into a copper wire with a diameter of 0.200 to 0.202 mm;

[0067] Step 4: Input several copper wires with a diameter of 0.200-0.202 mm in step 3 into the FC-650B Fuchuan high-speed stranding machine for bundle stranding: set the wire tension to 15N, set the wire tension to 35%, set the speed to 3000 TPM, wire splitting structure to 3+1, and die to 1.25±0.02 mm. After the bundle stranding process, a copper wire bundle with a diameter of 1.25±0.02 mm is obtained;

[0068] Step five, input the copper wire bundle with a diameter of 1.25±0.02mm obtained in step four into another FC-650B Fuchuan high-speed stranding machine for re-twisting: pay-off tension: 35N, take-up tension: 100N, rotation speed: 1500TPM, branching structure: 1+6, mold: 3.2±0.02mm, and you can get a high-flexibility and torsion-resistant robot cable copper conductor with a diameter of 3.2±0.02mm and a DC resistance of ≤3.3Ω / km. The center of the obtained high-flexibility and torsion-resistant robot cable copper conductor is circular, and the rest are bow-shaped.

[0069] The difference between Example 2 and Example 1 is that: in step 2, the pure copper rod with a diameter of 8±0.05 mm that has been treated with impurities in step 1 is input into the MSM86 Niehof double-head drawing machine for Niehof drawing treatment: drawing liquid temperature: 35°C, annealing coefficient: 7.5, coolant temperature: 35°C, equipment speed: 25m / S, and the copper rod treated with Niehof drawing is processed into a busbar with a diameter of 1.82mm-1.84mm;

[0070] Step three, input the busbar with a diameter of 1.82mm to 1.84mm in step two into the MMH series Nihof multi-head wire drawing machine for Nihof multi-head drawing treatment: wire drawing liquid temperature: 35°C, wire drawing oil concentration: 4%, annealing liquid temperature: 35°C, annealing liquid concentration: 0.5%, annealing coefficient: 8.0, line speed: 24m / s. The busbar treated with Nihof multi-head drawing is processed into copper wire with a diameter of 0.200 to 0.202mm.

[0071] The difference between Example 3 and Example 1 is that: Step 2, the pure copper rod with a diameter of 8±0.05 mm that has been treated with impurities in Step 1 is input into the MSM86 Niehof double-head drawing machine for Niehof drawing treatment: drawing liquid temperature: 45°C, annealing coefficient: 8.5, coolant temperature: 45°C, equipment speed: 28m / S, and the copper rod treated with Niehof drawing is processed into a busbar with a diameter of 1.82mm-1.84mm;

[0072] Step three, input the busbar with a diameter of 1.82mm to 1.84mm in step two into the MMH series Nihof multi-head wire drawing machine for Nihof multi-head drawing treatment: wire drawing liquid temperature: 45°C, wire drawing oil concentration: 9%, annealing liquid temperature: 45°C, annealing liquid concentration: 1%, annealing coefficient: 9.2, line speed: 28m / s. The busbar treated with Nihof multi-head drawing is processed into copper wire with a diameter of 0.200 to 0.202mm.

[0073] The difference between Example 4 and Example 1 is that: Step 2, the pure copper rod with a diameter of 8±0.05 mm that has been treated with impurities in Step 1 is input into the MSM86 Niehof double-head drawing machine for Niehof drawing treatment: drawing liquid temperature: 35°C, annealing coefficient: 7.5, coolant temperature: 35°C, equipment speed: 25m / S, and the copper rod treated with Niehof drawing is processed into a busbar with a diameter of 1.82mm-1.84mm;

[0074] Step three, input the busbar with a diameter of 1.82mm to 1.84mm in step two into the MMH series Nihof multi-head wire drawing machine for Nihof multi-head drawing treatment: wire drawing liquid temperature: 40°C, wire drawing oil concentration: 8%, annealing liquid temperature: 40°C, annealing liquid concentration: 0.8%, annealing coefficient: 9.0, line speed: 28m / s. The busbar treated with Nihof multi-head drawing is processed into copper wire with a diameter of 0.200 to 0.202mm.

[0075] The difference between Example 5 and Example 1 is that: in step 2, the pure copper rod with a diameter of 8±0.05 mm that has been treated with impurities in step 1 is input into the MSM86 Niehof double-head drawing machine for Niehof drawing treatment: drawing liquid temperature: 35°C, annealing coefficient: 7.5, coolant temperature: 35°C, equipment speed: 25m / S, and the copper rod treated with Niehof drawing is processed into a busbar with a diameter of 1.82mm-1.84mm;

[0076] Step three, input the busbar with a diameter of 1.82mm to 1.84mm in step two into the MMH series Nihof multi-head wire drawing machine for Nihof multi-head drawing treatment: wire drawing liquid temperature: 45°C, wire drawing oil concentration: 9%, annealing liquid temperature: 45°C, annealing liquid concentration: 1%, annealing coefficient: 9.2, line speed: 28m / s. The busbar treated with Nihof multi-head drawing is processed into copper wire with a diameter of 0.200 to 0.202mm.

[0077] The difference between Example 6 and Example 1 is that: Step 2, the pure copper rod with a diameter of 8±0.05 mm that has been treated with impurities in Step 1 is input into the MSM86 Niehof double-head drawing machine for Niehof drawing treatment: drawing liquid temperature: 40°C, annealing coefficient: 8.5, coolant temperature: 45°C, equipment speed: 26m / S, and the copper rod treated with Niehof drawing is processed into a busbar with a diameter of 1.82mm-1.84mm;

[0078] Step three, input the busbar with a diameter of 1.82mm to 1.84mm in step two into the MMH series Nihof multi-head wire drawing machine for Nihof multi-head drawing treatment: wire drawing liquid temperature: 45°C, wire drawing oil concentration: 9%, annealing liquid temperature: 45°C, annealing liquid concentration: 1%, annealing coefficient: 9.2, line speed: 28m / s. The busbar treated with Nihof multi-head drawing is processed into copper wire with a diameter of 0.200 to 0.202mm.

[0079] The difference between Example 7 and Example 1 is that: Step 2, the pure copper rod with a diameter of 8±0.05 mm that has been treated with impurities in Step 1 is input into the MSM86 Niehof double-head drawing machine for Niehof drawing treatment: drawing liquid temperature: 40°C, annealing coefficient: 8.5, coolant temperature: 45°C, equipment speed: 26m / S, and the copper rod treated with Niehof drawing is processed into a busbar with a diameter of 1.82mm-1.84mm;

[0080] Step three, input the busbar with a diameter of 1.82mm to 1.84mm in step two into the MMH series Nihof multi-head wire drawing machine for Nihof multi-head drawing treatment: wire drawing liquid temperature: 35°C, wire drawing oil concentration: 4%, annealing liquid temperature: 35°C, annealing liquid concentration: 0.5%, annealing coefficient: 8.0, line speed: 24m / s. The busbar treated with Nihof multi-head drawing is processed into copper wire with a diameter of 0.200 to 0.202mm.

[0081] The difference between Example 8 and Example 1 is that: Step 2, the pure copper rod with a diameter of 8±0.05 mm that has been treated with impurities in Step 1 is input into the MSM86 Niehof double-head drawing machine for Niehof drawing treatment: drawing liquid temperature: 40°C, annealing coefficient: 8.5, coolant temperature: 35°C, equipment speed: 25m / S, and the copper rod treated with Niehof drawing is processed into a busbar with a diameter of 1.82mm-1.84mm;

[0082] Step three, input the busbar with a diameter of 1.82mm to 1.84mm in step two into the MMH series Nihof multi-head wire drawing machine for Nihof multi-head drawing treatment: wire drawing liquid temperature: 45°C, wire drawing oil concentration: 6%, annealing liquid temperature: 40°C, annealing liquid concentration: 0.8%, annealing coefficient: 9.0, line speed: 25m / s. The busbar treated with Nihof multi-head drawing is processed into copper wire with a diameter of 0.200 to 0.202mm.

[0083] The difference between Example 9 and Example 1 is that: in step 4, a number of copper wires with a diameter of 0.200 to 0.202 mm in step 3 are input into the FC-650B Fuchuan high-speed stranding machine for bundle stranding: the wire setting tension is 15N, the wire setting tension is 30%, the set speed is 3400 TPM, the wire splitting structure is 3+1, and the mold is 1.25±0.02 mm. After the bundle stranding process, a copper wire bundle with a diameter of 1.25±0.02 mm is obtained;

[0084] Step 5. Input the copper wire bundle with a diameter of 1.25±0.02mm obtained in step 4 into another FC-650B Fuchuan high-speed stranding machine for re-twisting: pay-off tension: 35N, take-up tension: 95N, rotation speed: 1700TPM, branching structure: 1+6, mold: 3.2±0.02mm, and you can get a high-flexibility and torsion-resistant robot cable copper conductor with a diameter of 3.2±0.02mm and a DC resistance of ≤3.3Ω / km.

[0085] The difference between Example 10 and Example 1 is that: in step 4, a number of copper wires with a diameter of 0.200 to 0.202 mm in step 3 are input into the FC-650B Fuchuan high-speed stranding machine for bundle stranding: the wire setting tension is 15N, the wire setting tension is 40%, the set speed is 3200 TPM, the wire splitting structure is 3+1, and the mold is 1.25±0.02 mm. After the bundle stranding process, a copper wire bundle with a diameter of 1.25±0.02 mm is obtained;

[0086] Step 5. Input the copper wire bundle with a diameter of 1.25±0.02mm obtained in step 4 into another FC-650B Fuchuan high-speed stranding machine for re-twisting: pay-off tension: 35N, take-up tension: 105N, rotation speed: 1600TPM, branching structure: 1+6, mold: 3.2±0.02mm, and you can get a high-flexibility and torsion-resistant robot cable copper conductor with a diameter of 3.2±0.02mm and a DC resistance of ≤3.3Ω / km.

[0087] The difference between Example 11 and Example 1 is that the raw material copper rod is made of copper alloy. The copper alloy is made of 3D graphene doped with nano copper clusters on the surface and electrolytic copper melted and cast into one, and the 3D graphene doped with nano copper clusters on the surface has a content of 0.5%. The 3D graphene doped with nano copper clusters on the surface is prepared by conventional sol-gel method (customized by Xi'an Qiyue Biotechnology Co., Ltd.), and the size of the nano copper clusters is 20-25nm. The 3D graphene raw material is purchased from TN3DRGO, Chengdu Organic Chemistry Co., Ltd., Chinese Academy of Sciences, with 3-4 layers, 1.3-1.4nm thickness, 6-8 microns in size, and conductivity>3000S / m. The 3D graphene raw material is input into a planetary ball mill for ball milling and refinement treatment, with a ball milling speed of 240rpm. After ball milling for 1h, a 3D graphene carrier material with an average size of 0.5-2 microns is obtained, and the obtained 3D graphene carrier material is produced on its surface by sol-gel method with a size of 20-25nm nano copper clusters.

[0088] The difference between Example 12 and Example 11 is that the copper alloy is prepared by using 3D graphene with nano-copper clusters doped on the surface and electrolytic copper, and the content of 3D graphene with nano-copper clusters doped on the surface is 1%.

[0089] The difference between Example 13 and Example 11 is that the copper alloy is prepared by using 3D graphene with nano-copper clusters doped on the surface and electrolytic copper, and the content of 3D graphene with nano-copper clusters doped on the surface is 1.5%.

[0090] The difference between Example 14 and Example 11 is that the copper alloy is prepared by using 3D graphene with nano-copper clusters doped on the surface and electrolytic copper, and the content of 3D graphene with nano-copper clusters doped on the surface is 2.0%.

[0091] The difference between Example 15 and Example 11 is that the raw material copper rod is made of copper alloy. The copper alloy is prepared by 3D graphene (customized by Beijing Graphene Technology Research Institute Co., Ltd.) doped with single-atom copper on the surface and electrolytic copper, and the content of 3D graphene doped with single-atom copper on the surface is 0.5%. The mass of single-atom copper doped in 3D graphene doped with single-atom copper is 2.02wt%. The 3D graphene raw material is purchased from TN3DRGO of Chengdu Organic Chemistry Co., Ltd., Chinese Academy of Sciences, with 3-4 layers, 1.3-1.4nm thickness, 6-8 microns in size, and conductivity>3000S / m. The 3D graphene raw material is input into a planetary ball mill for ball milling and refining treatment, with a ball milling speed of 240rpm. After ball milling for 1h, a 3D graphene carrier material with an average size of 0.5-2 microns is obtained, and the obtained 3D graphene carrier material is loaded with single-atom copper on its surface by the existing preparation method of metal single-atom doped graphene.

[0092] The preparation method of 3D graphene doped with single-atom copper on the surface is as follows:

[0093] Step 1, weighing 200 mg of a 3D graphene carrier material with an average size of 0.5-2 microns and dispersing it in 200 mL of deionized water to obtain a graphene dispersion, weighing 1.2 g of KOH and dissolving it in 200 mL of deionized water to obtain a KOH solution, adding the KOH solution dropwise to the graphene dispersion, stirring and drying at 80° C. to obtain a graphene / KOH dry powder;

[0094] Step 2: weigh 1.72 g of CuCl2 into a crucible, and place 1.4 g of graphene / KOH dry powder in the crucible; place the crucible containing CuCl2 and the crucible containing graphene / KOH dry powder in the upstream and downstream areas of the tubular furnace, respectively, and seal the tubular furnace; introduce Ar gas into the tubular furnace, and under the Ar atmosphere, increase the temperature of the upstream zone of the tubular furnace from room temperature to 550°C at a heating rate of 10°C / min, and keep it at 550°C for 1 hour, and at the same time, increase the temperature of the downstream zone of the tubular furnace from room temperature to 550°C at a heating rate of 10°C / min, and keep it at 550°C for 1 hour, to obtain a metal single-atom copper-doped 3D graphene precursor;

[0095] Step three, the metal single atom copper doped 3D graphene precursor is added to 100 mL of dilute hydrochloric acid with a concentration of 1 mL / L, stirred, vacuum filtered, washed and dried to obtain 3D graphene with single atomic copper doped on the surface, and the obtained metal single atom doped graphene sample is structurally characterized. The atoms exist in the form of copper single atoms on the graphene surface, and inductively coupled plasma emission spectroscopy analysis shows that the copper single atom doping amount is about 2.02 wt%.

[0096] The difference between Example 16 and Example 15 is that the copper alloy is prepared by using 3D graphene with single-atom copper doped on the surface and electrolytic copper, and the content of 3D graphene with single-atom copper doped on the surface is 1.0%.

[0097] The difference between Example 17 and Example 15 is that the copper alloy is prepared by using 3D graphene with single-atom copper doped on the surface and electrolytic copper, and the content of 3D graphene with single-atom copper doped on the surface is 1.5%.

[0098] The difference between Example 18 and Example 15 is that the copper alloy is prepared by using 3D graphene with single-atom copper doped on the surface and electrolytic copper, and the content of 3D graphene with single-atom copper doped on the surface is 2.0%.

[0099] The difference between Example 19 and Example 15 is that the copper alloy is prepared by using 3D graphene doped with single-atom copper on the surface, 3D graphene doped with single-atom silver on the surface, and electrolytic copper.

[0100] The content of 3D graphene doped with single-atom copper on the surface is 1.0%, and the content of 3D graphene doped with single-atom silver on the surface is 0.5%. The mass of single-atom copper doped in the 3D graphene doped with single-atom copper is 2.02wt%. The mass of single-atom silver doped in the 3D graphene doped with single-atom silver on the surface is 0.97wt%.

[0101] The preparation method of 3D graphene doped with single-atom copper on the surface is as follows:

[0102] Step 1, weighing 200 mg of a 3D graphene carrier material with an average size of 0.5-2 microns and dispersing it in 200 mL of deionized water to obtain a graphene dispersion, weighing 1.2 g of KOH and dissolving it in 200 mL of deionized water to obtain a KOH solution, adding the KOH solution dropwise to the graphene dispersion, stirring and drying at 80° C. to obtain a graphene / KOH dry powder;

[0103] Step 2: weigh 1.12 g of AgNO3 into a crucible, and place 1.4 g of graphene / KOH dry powder in the crucible; place the crucible containing AgNO3 and the crucible containing graphene / KOH dry powder in the upstream and downstream areas of the tubular furnace, respectively, and seal the tubular furnace; introduce Ar gas into the tubular furnace, and under the Ar atmosphere, increase the temperature of the upstream temperature zone of the tubular furnace from room temperature to 480°C at a heating rate of 10°C / min, and keep it at 480°C for 1h, and at the same time, increase the temperature of the downstream temperature zone of the tubular furnace from room temperature to 480°C at a heating rate of 10°C / min, and keep it at 480°C for 1h, to obtain a metal single-atom copper-doped 3D graphene precursor;

[0104] Step three, the metal single atom copper doped 3D graphene precursor is added to 100 mL of dilute hydrochloric acid with a concentration of 1 mL / L, stirred, vacuum filtered, washed and dried to obtain 3D graphene with single atomic copper doped on the surface, and the obtained metal single atom doped graphene sample is structurally characterized. The atoms exist in the form of copper single atoms on the graphene surface, and inductively coupled plasma emission spectroscopy analysis shows that the copper single atom doping amount is about 0.97wt%.

[0105] The difference between Example 20 and Example 19 is that the copper alloy is prepared by using 3D graphene doped with single-atom copper on the surface, 3D graphene doped with single-atom silver on the surface and electrolytic copper. The content of 3D graphene doped with single-atom copper on the surface is 0.8%, and the content of 3D graphene doped with single-atom silver on the surface is 0.2%. The mass of single-atom copper doped in the 3D graphene doped with single-atom copper is 4.95wt%. The mass of single-atom silver doped in the 3D graphene doped with single-atom silver on the surface is 1.98wt%.

[0106] The difference between Comparative Example 1 and Example 11 is that the raw material copper rod is made of copper alloy. The copper alloy is prepared by using 3D graphene doped with nano copper clusters on the surface and electrolytic copper, and the content of 3D graphene doped with nano copper clusters on the surface is 0.2%.

[0107] The difference between Comparative Example 2 and Example 11 is that the raw material copper rod is made of copper alloy. The copper alloy is prepared by using 3D graphene doped with nano copper clusters on the surface and electrolytic copper, and the content of 3D graphene doped with nano copper clusters on the surface is 2.5%.

[0108] The difference between Comparative Example 3 and Example 11 is that the raw material copper rod is made of copper alloy. The copper alloy is made of 3D graphene not doped with nano copper clusters on the surface and electrolytic copper, and the content of 3D graphene not doped with nano copper clusters on the surface is 0.2%.

[0109] The difference between Comparative Example 4 and Example 15 is that the raw material copper rod is made of copper alloy. The copper alloy is prepared by using 3D graphene doped with single-atom copper on the surface and electrolytic copper, and the content of 3D graphene doped with single-atom copper on the surface is 0.1%.

[0110] The difference between Comparative Example 5 and Example 15 is that the raw material copper rod is made of copper alloy. The copper alloy is prepared by using 3D graphene doped with single-atom copper on the surface and electrolytic copper, and the content of 3D graphene doped with single-atom copper on the surface is 2.5%.

[0111] The difference between Comparative Example 6 and Example 15 is that the raw material copper rod is made of copper alloy. The copper alloy is prepared by using 3D graphene doped with single-atom copper on the surface and electrolytic copper, and the content of 3D graphene doped with single-atom copper on the surface is 0.5%. The mass of single-atom copper doped in 3D graphene doped with single-atom copper on the surface is 0.21wt%.

[0112] Performance test: Bending performance test of robot cable copper conductor: The robot cable (PVC Hanhua Ningbo HG-700 injection molding grade as cable sheath, thickness 0.80±0.05mm) prepared from robot cable copper conductors in Examples 1-20 and Comparative Examples 1-6 was tested for bending performance using the Verkuni robot cable bending tester WK5015D-5SET in accordance with the standards of the China Robot Industry Alliance, CRIA 0003.2-2016 "Industrial Robot Special Cable Part 2: Test Methods", and PFG 2577 / 08.16. Test parameters: bending speed 50 times / min, bending radius 40mm, test stroke 1200mm, bending reference number (standard value, 10,000 times) 8 million times.

[0113] Table 1: Test parameter table of robot cables in Examples 1-20 and Comparative Examples 1-6

[0114]

[0115]

[0116] It can be seen from Example 1 and Examples 2-9 and Table 1 that, through the study of the influence of the annealing coefficient on the elongation of the wire, the annealing coefficient is adjusted online in real time according to the change in the elongation of the wire, so as to control the change in the temperature difference, so that the elongation of the wire is within a certain range, and the softness of different batches of wires is uniform, thereby ensuring that the prepared robot cable copper conductor has the advantages of high strength, high flexibility, good torsion resistance and high safety.

[0117] It can be seen from Examples 11-14 and Comparative Examples 1-3 combined with Table 1 that the robot cable copper conductor prepared from copper rod raw materials made of 3D graphene doped with nano-copper clusters on the surface and electrolytic copper has relatively good high flexibility and torsion resistance, and the doping amount of 3D graphene doped with nano-copper clusters on the surface is preferably controlled to 0.5-2.0wt%.

[0118] It can be seen from Examples 15-20 and Comparative Examples 4-6 combined with Table 1 that the robot cable copper conductor made of copper rod raw materials made from 3D graphene doped with single-atom copper and / or silver on the surface and electrolytic copper has relatively better flexibility and torsion resistance, and the doping amount of 3D graphene doped with single-atom copper and / or silver on the surface is preferably controlled to 0.5-2.0wt%.

[0119] Performance testing: The copper alloy materials in Examples 11-20 and Comparative Examples 1-6 were tested for volume resistivity and tensile strength. The tensile strength test was conducted in accordance with the room temperature tensile test method for copper and copper alloy materials GB / T34505-2017. The volume resistivity test was conducted in accordance with GB / T 3048.2-2007 "Electrical performance test methods for wires and cables Part 2: Resistivity test of metallic materials".

[0120] Table 2: Test parameters of copper alloy materials used for robot cable copper conductors in Examples 1-20 and Comparative Examples 1-6

[0121] Tensile strength MPa Volume resistivity Ω·m Control group 200-300 <![CDATA[1.70~1.80×10 -8 ]]> Embodiment 11 330.6 <![CDATA[1.56×10 -8 ]]> Example 12 344.4 <![CDATA[1.49×10 -8 ]]> Example 13 351.0 <![CDATA[1.45×10 -8 ]]> Embodiment 14 353.9 <![CDATA[1.42×10 -8 <!-- 12 -->]]> Embodiment 15 342.1 <![CDATA[1.48×10 -8 ]]> Example 16 352.5 <![CDATA[1.41×10 -8 ]]> Embodiment 17 358.2 <![CDATA[1.38×10 -8 ]]> Embodiment 18 362.7 <![CDATA[1.35×10 -8 ]]> Embodiment 19 360.2 <![CDATA[1.36×10 -8 ]]> Embodiment 20 354.7 <![CDATA[1.39×10 -8 ]]> Comparative Example 1 305.2 <![CDATA[1.64×10 -8 ]]> Comparative Example 2 355.1 <![CDATA[1.40×10 -8 ]]> Comparative Example 3 237.8 <![CDATA[1.85×10 -8 ]]> Comparative Example 4 331.5 <![CDATA[1.59×10 -8 ]]> Comparative Example 5 363.8 <![CDATA[1.33×10 -8 ]]> Comparative Example 6 317.4 <![CDATA[1.62×10 -8 ]]>

[0122] Combining Examples 11-20 and Comparative Examples 1-6 with Table 1-2, it can be seen that the robot cable copper conductor in the present invention has better electrical conductivity and mechanical strength, and can improve the overall high flexibility and torsion resistance of the robot cable. The robot cable copper conductor prepared by 3D graphene doped with single-atom copper and / or silver on the surface has better electrical conductivity and mechanical strength.

[0123] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed. However, as long as they are within the scope of the claims of the present invention, they are protected by the patent law.

Claims

1. A highly flexible and torsion-resistant robot cable copper conductor, characterized in that: The copper conductor of the highly flexible and torsion-resistant robot cable is prepared from a copper rod through Niehoff pulling, Niehoff multi-head pulling, bundle twisting, and multiple twisting; the twisted outer diameter of the copper conductor of the highly flexible and torsion-resistant robot cable is ≤3.3mm, and the DC resistance is ≤3.3Ω / km.

2. A method for preparing the highly flexible and torsion-resistant robot cable copper conductor according to claim 1, characterized in that: The following steps are involved: Step 1: Perform surface impurity removal treatment on the raw material copper rod to remove oil stains and oxides on the raw material copper rod; Step 2: input the copper rod that has been subjected to the impurity removal treatment in step 1 into a Niehof double-head drawing machine for Niehof drawing treatment, and process the copper rod that has been subjected to the Niehof drawing treatment into a busbar with a diameter of 1.82 mm to 1.84 mm; Step 3, inputting the busbar with a diameter of 1.82 mm to 1.84 mm in step 2 into a Nihoff multi-head wire drawing machine for Nihoff multi-head drawing, and processing the busbar after Nihoff multi-head drawing into a copper wire with a diameter of 0.200 to 0.202 mm; Step 4, inputting a number of copper wires with a diameter of 0.200-0.202 mm obtained in step 3 into a high-speed stranding machine for bundle stranding, and obtaining a copper wire bundle with a diameter of 1.25±0.02 mm after the bundle stranding process; Step 5: Input the copper wire bundle with a diameter of 1.25±0.02mm obtained in step 4 into a high-speed stranding machine for re-twisting to obtain a high-flexibility and torsion-resistant robot cable copper conductor with a diameter of 3.2±0.02mm and a DC resistance of ≤3.3Ω / km.

3. The high-flexibility and torsion-resistant robot cable copper conductor according to claim 2 is characterized in that: The diameter of the raw material copper rod described in step 1 is 8±0.05 mm; the raw material copper rod is made of pure copper or copper alloy.

4. The method for preparing a highly flexible and torsion-resistant robot cable copper conductor according to claim 2, characterized in that: In the step 2, the copper rod that has been treated with impurities in step 1 is input into a Niehof double-head drawing machine for Niehof drawing treatment: drawing liquid temperature: 35-45°C, annealing coefficient: 7.5-8.5, coolant temperature: 35-45°C, equipment speed: 25-28m / S, and the copper rod that has been treated with Niehof drawing is processed into a busbar with a diameter of 1.82mm-1.84mm.

5. The method for preparing a highly flexible and torsion-resistant robot cable copper conductor according to claim 2, characterized in that: In the step three, the busbar with a diameter of 1.82 mm to 1.84 mm in the step two is input into a Nihof multi-head wire drawing machine for Nihof multi-head drawing treatment: wire drawing liquid temperature: 35 to 45°C, wire drawing oil concentration: 4% to 9%, annealing liquid temperature: 35 to 45°C, annealing liquid concentration: 0.5% to 1.0%, annealing coefficient: 8.0 to 9.2, line speed: 24 to 28 m / s, and the busbar treated with Nihof multi-head drawing is processed into a copper wire with a diameter of 0.200 to 0.202 mm.

6. The method for preparing a highly flexible and torsion-resistant robot cable copper conductor according to claim 2, characterized in that: In the step four, several copper wires with a diameter of 0.200-0.202 mm in step three are input into a high-speed stranding machine for bundle twisting: pay-off tension: 15±2N, take-up tension: 35±5%, rotation speed: 3200±200 TPM, wire branching structure: 3+1, mold: 1.25±0.02 mm, and after bundle twisting, a copper wire bundle with a diameter of 1.25±0.02 mm is obtained.

7. The method for preparing a highly flexible and torsion-resistant robot cable copper conductor according to claim 2, characterized in that: In the step five, the copper wire bundle with a diameter of 1.25±0.02mm obtained in the step four is input into a high-speed stranding machine for re-twisting: pay-off tension: 35±2N, take-up tension: 100±5N, rotation speed: 1600±200TPM, branching structure: 1+6, mold: 3.2±0.02mm, so as to obtain a high-flexibility and torsion-resistant robot cable copper conductor with a diameter of 3.2±0.02mm and a DC resistance of ≤3.3Ω / km.

8. The method for preparing a highly flexible and torsion-resistant robot cable copper conductor according to claim 7, characterized in that: In the step 1, a copper rod having a diameter of 8±0.05 mm is subjected to surface impurity removal treatment to remove oil stains and oxides on the copper rod; Step 2: The copper rod treated with impurities in step 1 is input into a Niehof double-head drawing machine for Niehof drawing: drawing liquid temperature: 40°C, annealing coefficient: 8.5, coolant temperature: 45°C, equipment speed: 26m / S, and the copper rod treated with Niehof drawing is processed into a busbar with a diameter of 1.82mm to 1.84mm; Step 3, input the busbar with a diameter of 1.82 mm to 1.84 mm in step 2 into a Nihoff multi-head wire drawing machine for Nihoff multi-head drawing treatment: wire drawing liquid temperature: 40°C, wire drawing oil concentration: 8%, annealing liquid temperature: 40°C, annealing liquid concentration: 0.8%, annealing coefficient: 9.0, line speed: 28 m / s, and the busbar treated by Nihoff multi-head drawing is processed into a copper wire with a diameter of 0.200 to 0.202 mm; Step 4, inputting several copper wires with a diameter of 0.200-0.202 mm in step 3 into a high-speed stranding machine for bundle stranding: setting the wire tension to 15N, setting the wire tension to 35%, setting the speed to 3000 TPM, the wire splitting structure to 3+1, and the die to 1.25±0.02 mm, and obtaining a copper wire bundle with a diameter of 1.25±0.02 mm after the bundle stranding process; Step 5. Input the copper wire bundle with a diameter of 1.25±0.02mm obtained in step 4 into a high-speed stranding machine for re-twisting: pay-off tension: 35N, take-up tension: 100N, rotation speed: 1500TPM, branching structure: 1+6, mold: 3.2±0.02mm, and you can get a high-flexibility and torsion-resistant robot cable copper conductor with a diameter of 3.2±0.02mm and a DC resistance of ≤3.3Ω / km.

9. The method for preparing a highly flexible and torsion-resistant robot cable copper conductor according to claim 2 or 8, characterized in that: The raw material copper rod is a copper alloy, and the copper alloy copper rod is formed by extrusion or integral casting of a copper rod; the copper alloy includes 3D graphene and copper, and the content of the 3D graphene is 0.5-2wt%; the surface of the 3D graphene is doped with at least one of nano-copper clusters, nano-silver clusters, single-atom copper, and single-atom silver; the number of layers of the 3D graphene is 3-4, the thickness is 1.3-1.4nm, the size is 0.5-8 microns, and the conductivity is >3000S / m.

10. The method for preparing a highly flexible and torsion-resistant robot cable copper conductor according to claim 9, characterized in that: The 3D graphene content is 1.0-1.5wt%; the surface of the 3D graphene is doped with single-atom copper and single-atom silver; the mass ratio of the single-atom copper to the single-atom silver is (2-4):1; the mass ratio of the total doping mass of the single-atom copper and the single-atom silver to the 3D graphene is 1:(20-50).

Citation Information

Patent Citations

  • Processing method of power cable

    CN110233002A

  • Nickel-plated stranded copper conductor used for automobile and manufacturing method thereof

    CN110675970A

  • Copper wire drawing process

    CN110935742A

  • Flexible cable for 10MW offshore wind generating set and preparation method of flexible cable

    CN114068061A

  • Heat-resistant high-voltage cable copper conductor for new energy automobile

    CN221149703U

Cited By

  • Preparation process of ultrafine copper conductor for new energy automobile

    CN120280222A

  • Preparation process of ultra-fine copper conductor for new energy vehicles

    CN120280222B