Cristobalite gate oxide dielectric layer and preparation method and application thereof
By generating a cubic quartz layer on the 4H-SiC surface, the problems of low oxidation rate and many interface defects in amorphous silicon dioxide in silicon carbide devices are solved, and the dielectric performance and reliability of the device are improved.
Patent Information
- Application Number
- CN202411114799.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, the gate oxygen dielectric layer of amorphous silicon dioxide as a silicon carbide device has problems such as low oxidation rate, many interface defects and insufficient barrier height, resulting in limited device performance and reliability.
By performing specific oxidation and annealing processes on the 4H-SiC surface, a fully covered crescent quartz layer is generated, and the high dielectric properties and strict lattice arrangement of crescent quartz can be used to solve interface defects and improve device performance.
The neat arrangement of the interface atoms between the crescent quartz gate oxygen dielectric layer and the SiC is achieved, reducing vacancy defects, improving the barrier height and dielectric performance of the MOS dielectric layer, and enhancing the reliability and temperature and pressure resistance of the device.
Smart Images

Figure CN118969604A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a cristobalite gate oxide dielectric layer and a preparation method and application thereof. Background Art
[0002] Amorphous silicon dioxide (SiO2) has long been the preferred material for the gate oxide dielectric layer of silicon carbide (SiC) devices. However, with the increasing performance requirements of microelectronic devices, amorphous SiO2 has gradually exposed its inherent disadvantages, including: low oxidation rate, resulting in a thicker interface layer between SiO2 and SiC; the disordered structure of amorphous SiO2 easily causes interface defects with the substrate, which in turn affects device performance; the barrier height of the metal-oxide-semiconductor (MOS) structure is low, resulting in an increase in MOS leakage current, further affecting the reliability of the MOS gate.
[0003] To solve the above problems, a lot of research has been devoted to finding high dielectric constant gate materials such as hafnium dioxide (HfO2) and aluminum oxide (Al2O3) to replace SiO2. Although these new materials show advantages in some aspects, their preparation process is complicated and the preparation cost is high. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In order to solve at least one of the above-mentioned technical problems of the gate oxide dielectric layer in the prior art, an embodiment of the present invention provides a cristobalite gate oxide dielectric layer and a preparation method and application thereof, wherein a fully covered cristobalite layer is generated by performing a specific oxidation and annealing process on the surface of 4H-SiC, and the process method is simple and does not introduce other elements; and the atoms at the interface between the prepared cristobalite gate oxide dielectric layer and SiC are neatly arranged, and there are fewer vacancy defects and interface states; cristobalite is introduced into the gate oxide dielectric layer of 4H-SiC, and the high dielectric properties and strict lattice arrangement of cristobalite are used to solve the influence of interface defects on device performance.
[0006] (II) Technical solution
[0007] In view of the above technical problems, embodiments of the present invention provide a cristobalite gate oxide dielectric layer and a preparation method and application thereof.
[0008] According to a first aspect of the present invention, a method for preparing a quartz gate oxide dielectric layer is provided, comprising the following steps: preparing a 4H silicon carbide sample to be oxidized; heating and oxidizing the surface of the 4H silicon carbide sample to be oxidized to generate an initial quartz oxide layer; and annealing the initial quartz oxide layer to obtain oxidized 4H silicon carbide, wherein the oxidized 4H silicon carbide includes or is entirely a quartz gate oxide dielectric layer.
[0009] In some exemplary embodiments, heating and oxidizing the surface of a 4H silicon carbide sample to be oxidized includes: placing the 4H silicon carbide sample to be oxidized in a crucible; placing the crucible containing the 4H silicon carbide sample to be oxidized in a tube furnace; and heating and oxidizing the 4H silicon carbide sample to be oxidized according to a first process parameter.
[0010] In some exemplary embodiments, the first process parameters include: adjusting and maintaining the cavity vacuum degree in the tube furnace to a preset vacuum degree; raising the temperature of the tube furnace to 120°C±5°C at a heating rate of 2°C / min±0.5°C / min; continuing to increase the temperature at a heating rate of 10°C / min±0.5°C / min until the temperature in the tube furnace cavity reaches 1400°C±5°C; keeping warm at 1400°C±5°C for 15min±2min, wherein during the insulation process, oxygen is introduced into the tube furnace cavity at a flow rate of 500sccm±10sccm while maintaining the vacuum degree in the tube furnace cavity at no more than 75Torr; and after the insulation is completed, stopping the introduction of oxygen.
[0011] In some exemplary embodiments, annealing the initial quartz oxide layer includes annealing the initial quartz oxide layer according to second process parameters, wherein the second process parameters include: lowering the temperature in the tube furnace chamber to 1200°C±5°C; keeping warm at 1200°C±5°C for 10h±0.1h, wherein the vacuum degree in the tube furnace chamber is maintained at no more than 75Torr during the insulation process; and naturally cooling from the annealing temperature to room temperature after the insulation is completed to remove the oxidized 4H silicon carbide, wherein the vacuum degree in the tube furnace chamber is maintained at no more than 75Torr during the natural cooling process.
[0012] In some exemplary embodiments, no amorphous silicon dioxide is present on the surface of the oxidized 4H silicon carbide.
[0013] In some exemplary embodiments, the method further includes: optimizing the position for interface defect shielding, wherein the optimizing the position for interface defect shielding includes performing selective etching by utilizing the difference in etching rates between quartz and amorphous silicon dioxide in hydrofluoric acid; after the etching is completed, retaining the quartz gate oxide dielectric layer at defect-free positions to remove silicon carbide interface and surface defects.
[0014] According to a second aspect of the present invention, a method for preparing a quartz gate oxide dielectric layer is provided, comprising the following steps: preparing a 4H silicon carbide sample to be oxidized; oxidizing at 1200°C±5°C for 15min±2min to obtain an initial amorphous oxide layer; and annealing at 1400°C±5°C for 15min±2min to obtain a quartz gate oxide dielectric layer.
[0015] According to a third aspect of the present invention, a cristobalite gate oxide dielectric layer is provided. The cristobalite gate oxide dielectric layer is prepared by any of the above methods.
[0016] According to a fourth aspect of the present invention, there is provided an application of three cristobalite gate oxide dielectric layers prepared by the above method, which can be applied to MOS structures.
[0017] In some exemplary embodiments, the preparation method of the MOS structure includes: evaporating a layer of metal nickel on the back side of the oxidized 4H silicon carbide; annealing at 950°C for 90 seconds to obtain a back electrode; and using an electrode template to evaporate a metal nickel layer and a metal aluminum layer in sequence on the front side of the oxidized 4H silicon carbide to obtain a front electrode.
[0018] (III) Beneficial effects
[0019] It can be seen from the above technical solutions that the cristobalite gate oxide dielectric layer and the preparation method and application thereof provided in the embodiments of the present invention have at least the following beneficial effects:
[0020] (1) A specific oxidation and annealing process is performed on the 4H-SiC surface to generate a full-coverage or selective-coverage quartz layer. This process is simple and does not introduce other elements.
[0021] (2) The atoms at the interface between the prepared quartz gate oxide dielectric layer and SiC are neatly arranged, with fewer vacancy defects and interface states.
[0022] (3) Cristobalite replaces amorphous silicon dioxide as the gate oxide dielectric layer of the device. The high dielectric properties of cristobalite are used to compensate for the negative impact of defects on the MOS voltage withstand process, further improving the barrier height and dielectric properties of the MOS dielectric layer, improving the reliability of the device, and giving full play to the temperature and voltage resistance advantages of wide bandgap semiconductor devices.
[0023] (4) By utilizing the circular growth characteristics of cristobalite, cristobalite in a specific area is prepared, thereby obtaining a new structure that can eliminate and shield defects. The entire preparation process ensures both the integrity of the structure and the excellent electrical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The above contents and other objects, features and advantages of the present invention will become more apparent through the following description of the embodiments of the present invention with reference to the accompanying drawings, in which:
[0025] Figure 1 A schematic diagram of a process for preparing a quartz layer on 4H silicon carbide according to an embodiment of the present invention is shown;
[0026] Figure 2 A schematic diagram of a process for preparing a 4H silicon carbide sample to be oxidized according to an embodiment of the present invention is shown;
[0027] Figure 3A schematic diagram of a process for heating and oxidizing a sample to be oxidized of 4H silicon carbide according to an embodiment of the present invention is shown;
[0028] Figure 4 A schematic diagram of a temperature-time curve of a method for preparing a cristobalite gate oxide dielectric layer according to an embodiment of the present invention is schematically shown;
[0029] Figure 5 Schematically shows the emergence and growth process of the cristobalite phase according to an embodiment of the present invention;
[0030] Figure 6 The flowchart of the method for preparing the first cristobalite gate oxide dielectric layer according to the embodiment of the present invention is schematically shown;
[0031] Figure 7 Schematically showing an optical microscope image of quartz on the surface of 4H-SiC after oxidation according to an embodiment of the present invention;
[0032] Figure 8 Schematically showing an optical microscope image of cristobalite on the surface of 4H-SiC according to an embodiment of the present invention after being etched by HF aqueous solution for 6 minutes;
[0033] Fig. 9 The Raman spectrum of the oxidized 4H-SiC surface according to an embodiment of the present invention is schematically shown;
[0034] Fig.10 A schematic diagram of a process of preparing a second cristobalite gate oxide dielectric layer according to an embodiment of the present invention is shown;
[0035] Fig.11 A schematic diagram of a process of preparing a MOS structure according to an embodiment of the present invention is shown;
[0036] Fig.12 A schematic diagram of a MOS structure based on 4H-SiC according to an embodiment of the present invention is shown; and
[0037] Fig.13 The schematic diagram of the MOS structure based on 4H-SiC with different positional relationships between defects and cristobalite phase according to an embodiment of the present invention is shown schematically, wherein: Fig.13 (a) schematically shows a cross-sectional view of a MOS based on defective 4H-SiC in the prior art, in which amorphous silicon dioxide is used as a dielectric layer; Fig.13 (b) schematically shows a cross-sectional view of a MOS based on a fully covered quartz dielectric layer of a first quartz gate oxide dielectric layer according to an embodiment of the present invention; Fig.13(c) schematically shows a cross-sectional view of a MOS in a specific area using a quartz dielectric layer without defects in the second quartz gate oxide dielectric layer according to an embodiment of the present invention; and Fig.13 (d) schematically shows a cross-sectional view of a MOS in which the overall dielectric constant and defect withstand voltage capability are improved by using cristobalite to shield defects in the third cristobalite gate oxide dielectric layer according to an embodiment of the present invention. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in combination with specific embodiments and with reference to the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] Figure 1 The figure schematically shows a flow chart of a method for preparing a quartz layer on 4H silicon carbide according to an embodiment of the present invention.
[0040] like Figure 1 As shown, a method for preparing a quartz layer on 4H silicon carbide according to an embodiment of the present invention includes steps S110-S130.
[0041] In step S110 , a 4H silicon carbide sample to be oxidized is prepared.
[0042] In some exemplary embodiments, step S110 includes steps S111-S113, see Figure 2 .
[0043] In step S111 , a 4H silicon carbide surface is selected as the oxidation surface.
[0044] In step S112, the oxidized surface is cleaned to remove pollutants on the oxidized surface. Optionally, cleaning the oxidized surface includes cleaning the oxidized surface using a standard chemical process (RCA).
[0045] In step S113, nitrogen is used to blow dry the cleaned 4H silicon carbide to ensure that the surface is clean and free of residue.
[0046] In step S120, the surface of the 4H silicon carbide sample to be oxidized is heated and oxidized to generate an initial cristobalite oxide layer.
[0047] In some exemplary embodiments, step S120 includes steps S121-S123, see Figure 3 .
[0048] In step S121, a 4H silicon carbide sample to be oxidized is placed in a crucible.
[0049] In step S122, a crucible containing a 4H silicon carbide sample to be oxidized is placed in a tube furnace.
[0050] In step S123, the 4H silicon carbide sample to be oxidized is heated and oxidized according to the first process parameters.
[0051] In some exemplary embodiments, the first process parameters include: adjusting and maintaining the cavity vacuum degree in the tube furnace to a preset vacuum degree; raising the temperature of the tube furnace to 120°C±5°C at a heating rate of 2°C / min±0.5°C / min; continuing to increase the temperature at a heating rate of 10°C / min±0.5°C / min until the temperature in the tube furnace cavity reaches 1400°C±5°C; keeping warm at 1400°C±5°C for 15min±2min, wherein during the insulation process, oxygen is introduced into the tube furnace cavity at a flow rate of 500sccm±10sccm while maintaining the vacuum degree in the tube furnace cavity at no more than 75Torr; and after the insulation is completed, stopping the introduction of oxygen.
[0052] For example, a clean surface 4H-SiC sample is placed in a covered alumina crucible, and then the crucible is pushed into a corundum tube furnace heated by a silicon molybdenum rod. Start the vacuum pumping speed system, adjust and maintain the vacuum degree of the cavity in the tube furnace at 7.5Torr±0.5Torr to ensure the stability of the oxidation environment. Start the heating system of the tube furnace, first carry out the preheating stage, and heat from room temperature (20℃) to 120℃ at a heating rate of 2℃ / min. Then, adjust the heating rate to 10℃ / min, and continue heating until the cavity temperature in the tube furnace reaches 1400℃. When the temperature reaches the preset value of 1400℃, open the air inlet, pass oxygen, and keep it at this temperature for 15 minutes to fully oxidize the 4H-SiC sample. During this period, control the oxygen flow rate to 500sccm, and ensure that the vacuum degree in the cavity does not exceed 75Torr. After the oxidation is completed, close the air inlet. The rapid oxidation was carried out at 1400°C for 15 minutes, using the sublimation of silicon atoms at high temperatures to trigger the gas phase oxidation reaction. During this process, cristobalite crystals grew on the sample surface by gas phase nucleation.
[0053] In step S130, the initial cristobalite oxide layer is annealed to obtain oxidized 4H silicon carbide, wherein the oxidized 4H silicon carbide includes a cristobalite gate oxide dielectric layer.
[0054] In some exemplary embodiments, annealing the initial quartz oxide layer includes annealing the initial quartz oxide layer according to second process parameters, wherein the second process parameters include: lowering the temperature in the tube furnace chamber to 1200°C±5°C; keeping warm at 1200°C±5°C for 10h±0.1h, wherein the vacuum degree in the tube furnace chamber is maintained at no more than 75Torr during the insulation process; and naturally cooling from the annealing temperature to room temperature after the insulation is completed to remove the oxidized 4H silicon carbide, wherein the vacuum degree in the tube furnace chamber is maintained at no more than 75Torr during the natural cooling process.
[0055] For example, after the oxidation is completed, the cooling process begins, and when the temperature drops to 1200°C, the annealing stage is entered. The high-temperature annealing treatment is performed in a vacuum environment for 10 hours, while maintaining the vacuum degree within 7.5 Torr to ensure the stability of the oxide layer and optimize the performance of the oxide layer. By annealing at 1200°C for 10 hours, the lateral crystallization of cristobalite is promoted, thereby eliminating amorphous SiO2 and ensuring that cristobalite dominates the oxide layer, and finally a cristobalite gate oxide dielectric layer is obtained. The temperature-time curve of the method for preparing the cristobalite gate oxide dielectric layer according to an embodiment of the present invention can be found in Figure 4 ; and the appearance and growth process of the cristobalite phase refer to Figure 5 .
[0056] Figure 6 The flowchart of the first method for preparing a cristobalite gate oxide dielectric layer according to an embodiment of the present invention is schematically shown.
[0057] like Figure 6 As shown, according to the first method for preparing a quartz gate oxide dielectric layer of an embodiment of the present invention, Figure 1 The method shown further includes step S140.
[0058] In step S140 , position optimization is performed for interface defect shielding.
[0059] In the embodiment of the present invention, the position optimization for interface defect shielding includes selectively etching by utilizing the difference in etching rates between cristobalite and amorphous silicon dioxide in hydrofluoric acid; and after the etching is completed, retaining the cristobalite gate oxide dielectric layer at the defect-free position to remove silicon carbide interface and surface defects. For example, the cristobalite gate oxide dielectric layer is selectively etched by using a 20% volume fraction hydrofluoric acid aqueous solution to obtain a second cristobalite gate oxide dielectric layer.
[0060] Optionally, in order to eliminate the influence of a weak oxidation reaction that may occur on the back side, the front side of the sample is first protected, and then a 20% volume fraction hydrofluoric acid aqueous solution is used to remove the oxide layer on the back side to ensure that the back side is clean and free of oxide residues.
[0061] In the embodiment of the present invention, a fully covered cristobalite layer is directly prepared by an oxidation annealing process. At this time, there is no amorphous silicon dioxide on the SiC surface. Since there are few oxygen vacancies in cristobalite and the interface state is low, cristobalite, which has a strict lattice arrangement and high dielectric properties, is used to replace the amorphous silicon dioxide that cannot shield the SiC surface and interface defects.
[0062] The existence of the full cristobalite oxide layer obtained according to the embodiment of the present invention was verified by optical microscopy, Raman spectroscopy and HF etching method. Figure 7 ,Depend on Figure 7 It can be seen that there are round quartz phases in the prepared quartz oxide layer, but due to the transparent nature of silicon oxide, it is difficult to identify whether the quartz phase has completely replaced the amorphous silicon dioxide. The HF aqueous solution etching method was adopted, and the quartz grain boundaries were exposed by immersing in a 20% volume fraction HF aqueous solution for 6 minutes. The optical microscope image of quartz on the surface of 4H-SiC after 6 minutes of HF aqueous solution etching can be found in Figure 8 ,Depend on Figure 8 It can be seen that the amorphous areas in the oxide layer have been completely replaced by cristobalite, forming a polycrystalline cristobalite layer. The Raman spectrum of the oxidized 4H silicon carbide surface can be found at Fig. 9 ,exist Fig. 9 In the Raman spectrum, only the Raman peaks of cristobalite phase and 4H-SiC substrate were found, confirming the existence of cristobalite.
[0063] The cristobalite gate oxide dielectric layer according to the embodiment of the present invention can be applied to the MOS structure. The cristobalite prepared according to the embodiment of the present invention has a tightly packed crystal structure and good periodicity. According to the calculation of density functional theory, it shows a significant advantage over amorphous and other polycrystalline materials in terms of band gap. In addition, the interface between crystalline silicon dioxide and the substrate usually has fewer interface states, which is crucial for the MOS structure. Good interface quality can significantly reduce leakage current and improve device reliability. Therefore, the cristobalite layer according to the embodiment of the present invention can exhibit excellent electrical properties as a dielectric layer.
[0064] Fig.10 The flowchart of the second method for preparing a cristobalite gate oxide dielectric layer according to an embodiment of the present invention is schematically shown.
[0065] like Fig.10 As shown, the second method for preparing a cristobalite gate oxide dielectric layer according to an embodiment of the present invention includes steps S210-S230.
[0066] In step S210, a 4H silicon carbide sample to be oxidized is prepared.
[0067] In step S220, oxidation is performed at 1200°C±5°C for 15min±2min to obtain an initial amorphous oxide layer.
[0068] In step S230, annealing is performed at 1400°C±5°C for 15min±2min to obtain a cristobalite gate oxide dielectric layer.
[0069] In the embodiment of the present invention, the oxidation temperature is lower than the annealing temperature. After a layer of amorphous silicon dioxide is grown by oxidation, high temperature annealing is used to induce cristobalite nucleation growth at the defect, so that the defect position that is easy to break down under high pressure is surrounded by cristobalite with high dielectric properties, and a localized cristobalite shielding layer is formed near the defect.
[0070] Fig.11 The flowchart of the method for preparing the MOS structure according to the embodiment of the present invention is schematically shown.
[0071] like Fig.11 As shown, the method for preparing a MOS structure according to an embodiment of the present invention includes steps S310 - S330 .
[0072] In step S310, a layer of metal nickel is evaporated on the back side of the oxidized 4H silicon carbide.
[0073] In step S320 , an annealing process is performed at 950° C. for 90 seconds to obtain a back electrode.
[0074] In step S330, a metal nickel layer and a metal aluminum layer are sequentially evaporated on the front side of the oxidized 4H silicon carbide using an electrode template to obtain a front electrode.
[0075] For example, a 100nm thick layer of nickel (Ni) is evaporated on the back of the oxidized 4H silicon carbide sample, followed by a rapid thermal annealing treatment at 950°C for 90 seconds to form an ohmic contact of the back electrode. A circular metal electrode template with a diameter of 1mm is used on the front of the sample to evaporate 10nm of Ni and 200nm of aluminum (Al) in sequence to complete the preparation of the MOS structure. Fig.12 .
[0076] Furthermore, by utilizing the positional relationship between defects and the cristobalite phase, the oxide layer structure of the MOS based on 4H-SiC can be further improved to avoid the negative impact caused by defects. Fig.13 (a) is a MOS structure of the prior art. It can be seen that the defects in the 4H-SiC surface are exposed in the gate oxide layer, forming a large number of interface states and breakdown points, which makes the performance and reliability of the gate oxide low. In view of this, the present invention is designed as follows Fig.13The three new MOS gate oxide structures (b), (c) and (d) utilize the strict lattice arrangement and high dielectric properties of quartz to shield the surface and interface defects of silicon carbide, thereby improving gate oxide performance and reliability. Fig.13 (b) in the figure: a fully covered quartz layer is directly prepared by oxidation annealing process. At this time, there is no amorphous silicon dioxide on the surface of silicon carbide. Since there are few oxygen vacancies and low interface states in quartz, better gate oxide performance can be achieved. Fig.13 (c) in the figure: Further position optimization for interface defect shielding. The difference in etching rate between cristobalite and amorphous silicon dioxide in HF acid is used to perform selective etching. Only cristobalite without defect positions is retained, and MOS electrodes are prepared on this basis to achieve excellent interface and MOS gate oxide performance. Fig.13 (d) in the figure: After growing a layer of amorphous silicon dioxide by oxidation, high temperature annealing is used to induce quartz nucleation growth at the defect site, forming a localized quartz shielding layer near the defect. The high dielectric properties of quartz are used to compensate for the negative impact of defects on the MOS withstand voltage process, thereby improving gate oxide performance and reliability.
[0077] The above specific embodiments further illustrate the purpose, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a cristobalite gate oxide dielectric layer, characterized in that: The following steps are involved: Prepare 4H silicon carbide samples to be oxidized; Heating and oxidizing the surface of the 4H silicon carbide sample to be oxidized to generate an initial cristobalite oxide layer; and Annealing the initial quartz oxide layer to obtain oxidized 4H silicon carbide, Wherein, the oxidized 4H silicon carbide includes or is entirely a cristobalite gate oxide dielectric layer.
2. The method for preparing a cristobalite gate oxide dielectric layer according to claim 1, characterized in that: Heating and oxidizing the surface of the 4H silicon carbide sample to be oxidized comprises: Putting the 4H silicon carbide sample to be oxidized into a crucible; placing the crucible containing the 4H silicon carbide sample to be oxidized into a tube furnace; and The 4H silicon carbide sample to be oxidized is heated and oxidized according to the first process parameters.
3. The method for preparing a cristobalite gate oxide dielectric layer according to claim 2, characterized in that: The first process parameters include: Adjusting and maintaining the vacuum degree of the cavity in the tube furnace to a preset vacuum degree; Raise the temperature of the tube furnace to 120°C ± 5°C at a heating rate of 2°C / min ± 0.5°C / min; Continue heating at a heating rate of 10°C / min±0.5°C / min until the temperature in the tube furnace chamber reaches 1400°C±5°C; Keeping the temperature at 1400° C.±5° C. for 15 min±2 min, wherein during the keeping temperature process, oxygen is introduced into the tube furnace chamber at a flow rate of 500 sccm±10 sccm, while maintaining the vacuum degree in the tube furnace chamber at no more than 75 Torr; and After the insulation is completed, stop introducing oxygen.
4. The method for preparing a cristobalite gate oxide dielectric layer according to claim 3, characterized in that: The annealing of the initial quartz oxide layer comprises annealing the initial quartz oxide layer according to a second process parameter, Wherein, the second process parameters include: Lowering the temperature in the tube furnace chamber to 1200°C ±5°C; Keeping the temperature at 1200°C ± 5°C for 10 h ± 0.1 h, wherein the vacuum degree in the tube furnace chamber is maintained at no more than 75 Torr during the keeping process; After the heat preservation is completed, the annealing temperature is naturally cooled to room temperature to take out the oxidized 4H silicon carbide, wherein the vacuum degree in the tube furnace chamber is maintained at no more than 75 Torr during the natural cooling process.
5. The method for preparing a cristobalite gate oxide dielectric layer according to claim 1, characterized in that: There is no amorphous silicon dioxide on the surface of oxidized 4H silicon carbide.
6. The method for preparing a cristobalite gate oxide dielectric layer according to claim 1, characterized in that: Also includes: Position optimization for interface defect shielding, The position optimization for interface defect shielding includes performing selective etching by utilizing the difference in etching rates between cristobalite and amorphous silicon dioxide in hydrofluoric acid; After the etching is completed, the quartz gate oxide dielectric layer is retained at defect-free locations to remove silicon carbide interface and surface defects.
7. A method for preparing a cristobalite gate oxide dielectric layer, characterized in that: The following steps are included: Prepare 4H silicon carbide samples to be oxidized; Oxidation at 1200°C ± 5°C for 15 min ± 2 min to obtain an initial amorphous oxide layer; and Annealing is performed at 1400°C ±5°C for 15min±2min to obtain a quartz gate oxide dielectric layer.
8. A cristobalite gate oxide dielectric layer, characterized in that: The cristobalite gate oxide dielectric layer is prepared by the method according to any one of claims 1 to 7.
9. An application of a cristobalite gate oxide dielectric layer prepared by the method according to any one of claims 1 to 7, characterized in that: Applied to MOS structure.
10. The use of the cristobalite gate oxide dielectric layer according to claim 9, characterized in that: The method for preparing the MOS structure comprises: Vapor-plating a layer of metallic nickel on the back side of the oxidized 4H silicon carbide; Annealing at 950° C. for 90 seconds to obtain a back electrode; and An electrode template is used to sequentially evaporate and plate a metal nickel layer and a metal aluminum layer on the front side of the oxidized 4H silicon carbide to obtain a front electrode.