Metal oxide semiconductor and preparation method and application thereof
By doping tungsten oxide and silicon oxide in metal oxide semiconductors, the problems of high carrier concentration and sensitivity of acid etching liquid caused by oxygen vacancies are solved, and the high carrier mobility and chemical stability are improved. , improves the performance and stability of semiconductor devices.
Patent Information
- Application Number
- CN202410900510.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-15
AI Technical Summary
The presence of oxygen vacancies in the existing metal oxide semiconductor systems leads to high carrier concentration and deterioration of performance. The back-channel etching structure is sensitive to acidic etching liquid, which easily damages the semiconductor layer and affects device performance.
Doping tungsten oxide and silicon oxide in metal oxide semiconductors, adjusting their sputtering power through the sputtering process to form a composite oxide semiconductor, improving carrier mobility and chemical stability, and enhancing resistance to acidic etching liquid .
It effectively reduces the carrier concentration, improves the carrier mobility and chemical stability, enhances the resistance of semiconductors in acid etching liquid, and improves device performance and stability.
Smart Images

Figure HDA0004930343580000011 
Figure HDA0004930343580000012 
Figure HDA0004930343580000021
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor manufacturing, and in particular to a metal oxide semiconductor and a preparation method and application thereof. Background Art
[0002] In the existing metal oxide semiconductor system, the 5s orbital of Sn ion is the main electron transport channel. However, due to the low bond breaking energy after Sn ion and O ion bond formation, there are a large number of oxygen vacancy defects in the simple SnO2 film. Oxygen vacancies are the main reason for the high carrier concentration and deterioration of performance of metal oxide thin film transistors. Secondly, the back channel etching structure uses low-cost wet etching technology to pattern the source / drain electrodes. During the electrode patterning process, most oxide semiconductor materials are sensitive to acidic etching solutions, which can easily cause damage to the surface of the semiconductor layer (i.e., the back channel of the device), resulting in deterioration of device performance. At the same time, in order to ensure the performance uniformity of semiconductor devices, the metal oxide semiconductor film needs to maintain an amorphous film structure.
[0003] Therefore, it is imperative to develop a semiconductor with high carrier mobility and high chemical stability. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention proposes a metal oxide semiconductor, which effectively suppresses the oxygen vacancy concentration in the film by doping a small amount of tungsten oxide or silicon oxide into the main metal oxide, and at the same time, can increase the electron orbit overlap area to improve the semiconductor carrier mobility. The oxide semiconductor has strong acid resistance and has a high etching selectivity with the etching metal.
[0005] A second aspect of the present invention provides a method for preparing a metal oxide semiconductor.
[0006] According to a third aspect of the present invention, a thin film transistor is provided.
[0007] A fourth aspect of the present invention provides an application of a thin film transistor in a display panel or a detector.
[0008] According to a metal oxide semiconductor of the first aspect of the present invention, the components of the metal oxide semiconductor include, in molar ratio, Sn:W:Si of 0.70-1.0:0.01-0.06:0.1-0.30.
[0009] The embodiments according to the first aspect of the present invention have at least the following beneficial effects:
[0010] The composite metal oxide semiconductor provided by the present invention is a composite oxide semiconductor based on tin oxide. A small amount of doping with tungsten oxide and silicon oxide can suppress the carrier concentration and improve the chemical stability at a lower doping amount, so that the semiconductor can have a higher mobility and improve the chemical stability of the semiconductor in an acidic etching solution. When SnO2 is undoped, the mobility is 5cm 2 ·V -1 ·S -1 After doping with a small amount of atomic ratio of tungsten and silicon, the carrier concentration can be greatly reduced, and it is beneficial to increase the overlap of Sn ion 5s orbitals and improve the mobility of the material. Compared with the traditional pure SnO 2 material, the migration rate is only 5cm 2 / vs, a new type of tungsten ion and silicon ion doped metal oxide semiconductor, the device mobility can reach 12cm 2 / vs; that is, within the above doping range, tungsten oxide and silicon oxide can be used to show the suppression of their carrier concentration and the chemical stability to the acidic etching solution, while at the same time, the metal oxide semiconductor can maintain a better mobility.
[0011] The metal oxide semiconductor provided by the present invention can effectively reduce the carrier concentration in the film at a relatively low doping concentration. Compared with traditional oxide semiconductors, the mobility of the device is basically not affected after the etching process.
[0012] According to some embodiments of the present invention, in terms of molar ratio, the sum of the molar numbers of Sn:W and Si is not less than 2.
[0013] n(Sn):n(W+Si) is not less than 2, which can achieve suppression of carrier concentration and improvement of chemical stability at a lower doping amount, and can make the semiconductor have a higher mobility while improving the chemical stability of the semiconductor in the acidic etching solution.
[0014] According to the second aspect of the present invention, a method for preparing a metal oxide semiconductor comprises the following steps: adjusting the sputtering power of tungsten oxide and silicon oxide for doping under a fixed sputtering power of tin dioxide, and obtaining the metal oxide semiconductor by magnetron sputtering.
[0015] The present invention utilizes the influence of sputtering power on sputtering rate, fixes the sputtering power of the main tin dioxide and adjusts the sputtering power of the other two oxides for doping, and obtains a composite metal oxide semiconductor, wherein the sputtering power of the other two oxides is less than the sputtering power of the main tin oxide.
[0016] In the present invention, the sputtering power of the main tin dioxide is fixed and the sputtering power of the other two oxides is adjusted to perform doping, thereby obtaining several composite oxide films with different sputtering powers. Hall carrier concentration and carrier mobility tests are performed on several composite oxide films with different sputtering powers, and machine learning is performed to predict the sputtering power of different oxides with the best carrier mobility and carrier concentration. Verification and feedback guidance are provided to screen out the best sputtering power under the best carrier mobility and carrier concentration of the composite oxide semiconductor.
[0017] According to some embodiments of the present invention, during the sputtering deposition process, the power source includes at least one of radio frequency (RF) sputtering, direct current (DC) sputtering, and alternating current (AC) sputtering.
[0018] According to some embodiments of the present invention, the sputtering gas pressure is 0.1 Pa-10 Pa.
[0019] According to some embodiments of the present invention, the sputtering gas pressure is 0.2Pa-0.7Pa.
[0020] When the sputtering pressure is too low, stable glow sputtering cannot be maintained; when the sputtering pressure is too high, the scattering of the sputtered particles during the deposition process on the substrate increases significantly, the energy loss increases, the kinetic energy decreases after reaching the substrate, and the film defects formed increase, which seriously affects the performance of the device.
[0021] According to some embodiments of the present invention, during the sputtering deposition process, the oxygen partial pressure is 0-1Pa.
[0022] According to some embodiments of the present invention, during the sputtering deposition process, the oxygen partial pressure is 0.001-0.5 Pa.
[0023] According to some embodiments of the present invention, during the sputtering deposition process, the oxygen partial pressure is 0.01-0.1 Pa.
[0024] According to some embodiments of the present invention, during the sputtering deposition process, the oxygen flow rate ratio is preferably 0.
[0025] According to some embodiments of the present invention, during the sputtering deposition process, the substrate temperature is 0-40°C.
[0026] According to a third aspect of the present invention, a thin film transistor comprises an active layer, and the active layer is prepared from the metal oxide semiconductor.
[0027] According to some embodiments of the present invention, the thickness of the active layer is 3-20 nm.
[0028] According to some embodiments of the present invention, the thickness of the active layer is 3-10 nm.
[0029] According to some embodiments of the present invention, the thickness of the active layer is 3-5 nm.
[0030] According to some embodiments of the present invention, the carrier concentration of the metal oxide semiconductor film forming the active layer is less than 5×10 19 cm -3 .
[0031] According to some embodiments of the present invention, the thin film transistor switching ratio is greater than 10 6 .
[0032] According to some embodiments of the present invention, the saturation mobility of the thin film transistor is greater than 7 cm 2 ·V -1 ·S -1 .
[0033] According to some embodiments of the present invention, the preparation method includes at least one of a physical vapor deposition process, a chemical vapor deposition process, an atomic layer deposition process, a laser deposition process and a solution method.
[0034] According to some embodiments of the present invention, the sputtering gas pressure in the magnetron sputtering process is 0.1-0.6Pa.
[0035] According to some embodiments of the present invention, the substrate temperature in the magnetron sputtering process is 0-300°C.
[0036] According to some embodiments of the present invention, the volume percentage of oxygen in the sputtering atmosphere in the magnetron sputtering process is 0%.
[0037] Under the above sputtering conditions, an active layer with uniform texture, good adhesion and good film quality can be deposited.
[0038] According to some embodiments of the present invention, when the preparation method is a physical vapor deposition process, a single target sputtering or co-sputtering method is adopted.
[0039] The deposition rate of sputtered films is generally faster due to the participation of high-energy plasma; the film does not have enough time to relax during the deposition process, which will cause a certain proportion of dislocation and stress to remain in the film. This requires subsequent heating and annealing treatment to continue to achieve the required relative steady state and improve the performance of the film.
[0040] According to some embodiments of the present invention, the patterning process of the active layer film is carried out by photolithography combined with wet etching, and the etching solution used in the wet etching includes: a mixture of phosphoric acid, nitric acid and glacial acetic acid, a commercial oxalic acid-based etching solution, a dilute hydrochloric acid etching solution, and etching solutions such as hydrofluoric acid.
[0041] According to some embodiments of the present invention, when the preparation method is a physical vapor deposition process, a single target sputtering method is adopted.
[0042] Single-target sputtering can provide more repeatable and stable films, and the microstructure of the film is easier to control; unlike co-sputtered films, the sputtered particles will be disturbed by more factors during the recombination process.
[0043] According to some embodiments of the present invention, the annealing process is provided after the active layer is deposited.
[0044] On the one hand, annealing after the active layer is deposited can effectively improve the in-situ defects in the active layer and enhance the ability of the active layer to resist possible damage in subsequent processes.
[0045] In addition, in the implementation of the present invention, the treatment method may not only be heat treatment, but may also include plasma treatment of the interface (such as the gate insulation layer / semiconductor interface). The above treatment process can effectively improve the performance of the device and enhance the stability of the device.
[0046] According to some embodiments of the present invention, the thin film transistor further includes a substrate, a gate, a gate insulating layer, and a source and drain electrode.
[0047] According to some embodiments of the present invention, the thin film transistor further includes a planarization layer, a reflective electrode and a pixel definition layer.
[0048] According to some embodiments of the present invention, the substrate includes at least one of a rigid alkali glass, an alkali-free glass, a quartz glass and a silicon substrate, polyimide (PI), polyethylene naphthalate (PEN), polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polystyrene (PS), polysulfone ether (PES) and a metal foil.
[0049] The substrate in the present invention is not particularly limited, and any substrate known in the art can be used, such as hard alkali glass, alkali-free glass, quartz glass, silicon substrate, etc.; it can also be flexible polyimide (PI), polyethylene naphthalate (PEN), polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polystyrene (PS), polysulfone ether (PES) or metal foil, etc.
[0050] According to some embodiments of the present invention, the gate comprises at least one of a transparent conductive oxide, graphene, a metal-oxide semiconductor stack and a metal-metal stack.
[0051] According to some embodiments of the present invention, the transparent conductive oxide includes at least one of ITO, AZO, GZO, IZO, ITZO and FTO.
[0052] According to some embodiments of the present invention, the metal-oxide semiconductor stack includes at least one of ITO / Ag / ITO and IZO / Ag / IZO.
[0053] According to some embodiments of the present invention, the metal-metal stack includes at least one of Mo / Al / Mo and Ti / Al / Ti.
[0054] The gate material in the present invention is not particularly limited, and it can be arbitrarily selected from materials known in the art, such as transparent conductive oxides (ITO, AZO, GZO, IZO, ITZO, FTO, etc.), graphene, metals (Mo, Al, Cu, Ag, Ti, Au, Ta, Cr, Ni, etc.) and their alloys, and composite conductive films formed by metals and oxides (ITO / Ag / ITO, IZO / Ag / IZO, etc.), and metals and metal stacks (Mo / Al / Mo, Ti / Al / Ti, etc.).
[0055] According to some embodiments of the present invention, the method for preparing the gate includes at least one of sputtering, electroplating and thermal evaporation.
[0056] The specific structure of the gate electrode used in the present invention depends on the technical parameters to be achieved. For example, if a transparent electrode is required in a transparent display, a single layer of ITO or ITO / Ag / ITO can be used as the gate electrode. In addition, if a high temperature process is required in the application of special fields, the gate electrode can be a metal alloy film that can withstand high temperatures.
[0057] According to some embodiments of the present invention, the gate is prepared by thermal evaporation.
[0058] According to some embodiments of the present invention, the gate includes a gate insulating layer, and the insulating layer includes at least one of silicon oxide, silicon nitride, aluminum oxide, tantalum oxide, hafnium oxide, yttrium oxide and a polymer organic film layer.
[0059] The gate insulating layer may be formed by stacking a plurality of insulating films, which can form better insulating properties on the one hand, and improve the interface properties between the active layer and the gate insulating layer on the other hand.
[0060] The composition of the gate insulating layer film in the present invention may not be consistent with the theoretical stoichiometric ratio. In addition, the gate insulating layer may be formed by stacking multiple insulating films, which can form better insulation properties on the one hand and improve the interface properties between the active layer and the gate insulating layer on the other hand.
[0061] According to some embodiments of the present invention, the method for preparing the gate insulating layer includes at least one of physical vapor deposition, chemical vapor deposition, atomic layer deposition, laser deposition, anodization and a solution method.
[0062] The composition of the gate insulating layer film in the present invention may not be consistent with the theoretical stoichiometric ratio. In addition, the gate insulating layer may be formed by stacking multiple insulating films, which can form better insulation properties on the one hand and improve the interface properties between the active layer and the gate insulating layer on the other hand. The film prepared by the thermal evaporation method has good adhesion to the substrate, excellent uniformity, and can be prepared on a large area.
[0063] According to some embodiments of the present invention, the thin film transistor adopts a back channel etching structure.
[0064] In the present invention, in the preparation of the device of the back channel etching structure, the source and drain electrodes and the active layer need to have a suitable etching selectivity, otherwise the device cannot be prepared. The preferred etching solution is the Mo etching solution, mainly because the metal oxide semiconductor material of the present invention can effectively resist the etching of the wet hydrogen peroxide-based etching solution, and it has a very high etching selectivity with metals (such as molybdenum, molybdenum alloy, molybdenum / copper, titanium / copper, etc.), and the metal oxide semiconductor layer is basically not affected by the etching solution, and the prepared device has excellent performance and good stability.
[0065] It should be noted that the components of these insulating films may not be consistent with the theoretical stoichiometric ratio. In addition, the gate insulating layer may be formed by stacking multiple insulating films, which can form better insulating properties on the one hand and improve the interface properties of the active layer and the passivation layer on the other hand. Moreover, the passivation layer can be prepared in various ways, such as physical vapor deposition, chemical vapor deposition, atomic layer deposition, laser deposition or solution method.
[0066] The patterning process of the source-drain electrode film in the present invention is performed by photolithography combined with wet or dry etching. The etching solution used in wet etching includes: a mixture of phosphoric acid, nitric acid and glacial acetic acid or a mixture based on hydrogen peroxide. For dry etching, a plasma etching process can be selected, and the etching gas includes a chlorine-based or fluorine-based gas.
[0067] A fourth aspect of the present invention provides an application of a thin film transistor in a display panel or a detector.
[0068] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be obvious from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0069] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0070] Figure 1 The Hall electrical performance diagram of the tin dioxide film of Example 1;
[0071] Figure 2 The Hall electrical performance diagram of the composite oxide film of Example 1;
[0072] Figure 3 The etching rates and etching selectivities of the composite oxide film of Example 1 and metal aluminum and metal molybdenum in an acidic etching solution;
[0073] Figure 4 is a schematic diagram of the structure of a thin film transistor according to Example 2;
[0074] Figure 5 is the output characteristic curve of Example 2;
[0075] Figure 6 This is a transfer characteristic curve diagram of Example 2. DETAILED DESCRIPTION
[0076] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0077] Example 1
[0078] This embodiment provides a metal oxide semiconductor and a method for preparing the same, specifically:
[0079] A group of metal oxide semiconductor materials, wherein tungsten oxide and silicon oxide are doped into tin oxide (SnO2) to form tin silicon tungsten oxide (SnSiWO) oxide semiconductor materials, wherein the atomic ratio of Sn, W and Si in the tin silicon tungsten oxide is Sn:W:Si=0.75:0.05:0.20;
[0080] This group of tungsten oxide and silicon oxide doped tin oxide thin films uses three ceramic targets of tungsten oxide (WO3) and tin oxide (SnO2) doped with silicon oxide (SiO2), adopts a co-sputtering method, and adjusts the sputtering power of the two targets to achieve film preparation with different component ratios;
[0081] The thickness of the tungsten oxide and silicon oxide doped tin oxide films in this group is 100 nm, the oxygen content in the sputtering atmosphere is 0%, the sputtering pressure is 0.4 Pa, and the substrate temperature is set to room temperature; after patterning, the film is annealed in a high temperature oven at 350° C. in an air atmosphere for 60 minutes.
[0082] The composition ratio of the film is calibrated through characterization results such as scanning electron microscopy and X-ray fluorescence spectroscopy analysis, and some films with extremely low content are inferred by sputtering power.
[0083] The Hall electrical properties of the tin dioxide film of Example 1 are shown in FIG. Figure 1 As shown;
[0084] The Hall electrical properties of the metal oxide semiconductor composite oxide film of Example 1 are shown in FIG. Figure 2 As shown, Figure 2 Example 1 corresponds to an X-axis sputtering power of 20 W;
[0085] The etching rate and etching selection of the composite oxide film of Example 1 and metal aluminum and metal molybdenum in the acidic etching solution are as follows: Figure 3 shown.
[0086] Example 2
[0087] This embodiment provides a thin film transistor and a method for manufacturing the same, specifically:
[0088] The active layer of the thin film transistor is the metal oxide semiconductor in Example 1: tungsten oxide and silicon oxide are doped into tin oxide (SnO2) to form a tin silicon tungsten oxide (SnSiWO) oxide semiconductor material, wherein the atomic ratio of Sn, W and Si in the tin silicon tungsten oxide is Sn:W:Si=0.75:0.05:0.20;
[0089] The active layer of the thin film transistor is prepared by co-sputtering three ceramic targets of tungsten oxide (WO3) and tin oxide (SnO2) doped with silicon oxide (SiO2).
[0090] The thickness of the active layer thin film of the group of thin film transistors is 5nm, the oxygen content in the sputtering atmosphere is 0%, the sputtering pressure is 0.4Pa, the substrate temperature is set to room temperature, and the substrate of the group of thin film transistors is an aluminum oxide substrate;
[0091] The thin film transistor electrodes of this group are ITO electrodes with an electrode thickness of 150nm. The oxygen content in the sputtering atmosphere is 0%, the sputtering pressure is 1.0Pa, and the thin film transistor devices are annealed in a high temperature oven at 350°C in an air atmosphere for 60 minutes after patterning.
[0092] In Example 2, the materials and preparation methods of the functional layers of the thin film transistor are as follows:
[0093] The schematic diagram of the thin film transistor structure of Example 2 is as follows Figure 4 As shown;
[0094] The output characteristic curve of the thin film transistor of Example 2 is as follows: Figure 5 As shown;
[0095] The transfer characteristic curve of Example 2 is shown in FIG. Figure 6 shown.
[0096] Example 3
[0097] This embodiment provides a metal oxide semiconductor and a method for preparing the same. The difference between this embodiment and Embodiment 1 is that the atomic ratio of Sn, W and Si is Sn:W:Si=0.71:0.04:0.25, and the other conditions are the same.
[0098] The Hall electrical properties of the metal oxide semiconductor composite oxide film of Example 3 are shown in FIG. Figure 2 As shown in the figure, increasing the SiO2 ratio reduces the carrier mobility, while reducing the WO3 ratio and increasing the carrier concentration.
[0099] Figure 2 Example 3 corresponds to an X-axis sputtering power of 30W.
[0100] Example 4
[0101] The difference between this embodiment and embodiment 2 is that the metal oxide semiconductor of embodiment 3 is used, and the other conditions are the same.
[0102] Example 5
[0103] This embodiment provides a metal oxide semiconductor and a method for preparing the same. The difference between this embodiment and Embodiment 1 is that the atomic ratio of Sn, W and Si is Sn:W:Si=0.78:0.06:0.15, and the other conditions are the same.
[0104] The Hall electrical properties of the metal oxide semiconductor composite oxide film of Example 5 are shown in FIG. Figure 2 As shown in the figure, there is no obvious change in carrier mobility when the SiO2 ratio is reduced, while there is no obvious change when the WO3 ratio is increased and the carrier concentration fluctuates within an order of magnitude.
[0105] Figure 2 Example 5 corresponds to an X-axis sputtering power of 10W.
[0106] Example 6
[0107] The difference between this embodiment and embodiment 2 is that the metal oxide semiconductor of embodiment 5 is used, and the other conditions are the same.
[0108] A group of thin film transistors adopts a back channel etching structure, and its structural schematic diagram is shown in Figure 3As shown, it is provided with: a substrate 01, a gate 02 located on the substrate 01, a gate insulating layer 03 located on the substrate 01 and the gate 02, an active layer 04 covering the upper surface of the gate insulating layer 03 and corresponding to the gate 02, a source electrode 05-1 and a drain electrode 05-2 electrically connected to the two ends of the active layer 04, wherein the active layer 04 is an active layer 04 formed by the thin film described in Example 1; the substrate 01 is a glass substrate; the material of the gate 02 is a molybdenum-aluminum-molybdenum (Mo / Al / Mo) metal stacked structure prepared by magnetron sputtering, with a thickness of 50 / 200 / 50nm; the gate insulating layer 03 is aluminum oxide (Al2O3, with a thickness of 350nm) prepared by chemical vapor deposition; the aluminum oxide is in contact with the gate 02 at the lower layer and the active layer 04 at the upper layer;
[0109] The source 05-1 and the drain 05-2 are made of metal aluminum (Al) with a thickness of 200 nm;
[0110] Test Example 1
[0111] This test example tests the Hall electrical performance diagram of the tin dioxide thin film and the Hall electrical performance diagram of the metal oxide semiconductor in Example 1.
[0112] Depend on Figure 1 and Figure 2 It can be seen that the incorporation of tungsten oxide and silicon oxide has a very obvious effect on the performance of the film. The film without tungsten oxide and silicon oxide has a relatively low mobility. However, after a certain amount of tungsten oxide and silicon oxide are doped, the carrier mobility of the film is significantly improved. Of course, with the increase of tungsten or silicon content, the mobility and other characteristics of the film are further degraded. When excessive tungsten and silicon are doped, the mobility of the device is significantly degraded, which greatly limits its application field. Therefore, in practical applications, it is necessary to weigh the relationship between the two and select an appropriate doping amount.
[0113] according to Figure 1 and Figure 2 It can be seen that after doping a certain amount of tungsten oxide and silicon oxide, the carrier mobility of the film is significantly improved, greatly enhancing its potential in practical applications.
[0114] Considering the comprehensive performance of the film, Figure 2 It can be seen that when tungsten oxide and silicon oxide are doped into the active layer formed by the tin oxide semiconductor film, when the atomic ratio is 0.70-1.0:0.01-0.06:0.1-0.30, the comprehensive performance of the film is better.
[0115] Test Example 2
[0116] This test example tests the output characteristic curve and transfer characteristic curve of the transistor.
[0117] Figure 4The output characteristic curve in Example 2 of the present invention is characterized as follows. Figure 4 It can be seen that the oxide thin film transistor prepared by the composite oxide semiconductor in Example 1 exhibits typical field effect transistor output characteristics. Figure 5 The characterization results of the transfer characteristic curve in Example 2 of the present invention. Figure 5 It can be seen that the oxide thin film transistor prepared by the composite oxide semiconductor in Example 1 has typical switching characteristics, and the switching ratio is greater than 10 6 , saturation mobility greater than 7cm 2 ·V -1 ·S -1 .
[0118] In general, in the present invention, the thickness of the active layer of the thin film transistor prepared by doping tungsten oxide and silicon oxide into tin oxide material is preferably 3nm-10nm, and most preferably 3nm-5nm. In the most preferred state, the current switching ratio is between 106 and 107.
[0119] The above-mentioned embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.
Claims
1. A metal oxide semiconductor, characterized in that: In terms of molar ratio, the composition of the metal oxide semiconductor is include: Sn: W:Si is 0.70~1.0:0.01~0.06:0.1~0.
30.
2. The metal oxide semiconductor according to claim 1, characterized in that In terms of molar ratio, the sum of the molar numbers of Sn:W and Si is not less than 2.
3. A method for preparing a metal oxide semiconductor as claimed in claim 1 or 2, characterized in that: The following steps are involved: The sputtering power of tungsten oxide and silicon oxide is adjusted under a fixed sputtering power of tin dioxide for doping, and a metal oxide semiconductor is obtained by magnetron sputtering.
4. The preparation method according to claim 3, characterized in that: The sputtering gas pressure in the magnetron sputtering process is 0.1-0.6Pa.
5. The preparation method according to claim 3, characterized in that: The substrate temperature in the magnetron sputtering process is 0-300°C.
6. A thin film transistor, characterized in that: The thin film transistor comprises an active layer, and the active layer is prepared from the metal oxide semiconductor according to any one of claims 1 to 5.
7. The thin film transistor according to claim 6, characterized in that: The preparation method includes at least one of a physical vapor deposition process, a chemical vapor deposition process, an atomic layer deposition process, a laser deposition process and a solution method.
8. The thin film transistor according to claim 7, characterized in that: When the preparation method is a physical vapor deposition process, the sputtering pressure is 0.1-0.6 Pa, the volume proportion of oxygen in the sputtering atmosphere is 0%, and the substrate temperature is 0-40°C.
9. The thin film transistor according to claim 6, characterized in that: The thin film transistor also includes a substrate, a gate, a gate insulating layer and a source and drain electrode.
10. Use of the thin film transistor according to claim 6 in a display panel or a detector.