Preparation method of PAA system high-toughness pole piece, pole piece and battery

By grafting polymerization of acrylic acid on the polyvinyl alcohol side chain, PVA-g-PAA copolymer was prepared as a binder, and segmented rolling technology was used to solve the problem of insufficient toughness of the pole sheet of the PAA system and improve the battery performance and lifespan.

CN118969945APending Publication Date: 2024-11-15ZHUHAI KECHUANG SODIUM ELECTRIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411011930.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing PAA system electrode sheet has poor toughness and cannot effectively withstand the stress caused by volume expansion of active substances, affecting battery electrical performance and process processing.

Method used

By grafting polymerization of acrylic acid on the polyvinyl alcohol side chain, PVA-g-PAA copolymer is prepared as a new water-soluble binder, and segmented rolling technology is used during the preparation of the electrode sheet to improve the toughness of the electrode sheet.

Benefits of technology

It significantly improves the toughness and battery performance of the pole plate, extends the battery life, and enhances the battery's rate performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, in particular to a preparation method of a PAA system high-toughness pole piece, the pole piece and a battery. According to the invention, a preparation method of a PAA binder is changed, a PVA functional group is added into the PAA binder for modification to obtain a novel water-soluble binder as an electrode binder, and segmented rolling is carried out during electrode piece rolling, so that the toughness of an electrode piece can be effectively improved, the deformation of the electrode piece is inhibited, and the electrical performance of a battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and more specifically, to a method for preparing a PAA system high-toughness pole piece, a pole piece and a battery. Background Art

[0002] The PAA (polyacrylic acid) system pole pieces in the prior art generally use a PAA-type polymer prepared by a cross-linked polymerization method as a negative electrode material binder. PAA is a high molecular polymer, so it has excellent adhesion, dispersibility, and corrosion inhibition, which can stabilize the network structure in the negative electrode slurry, evenly disperse the active material, and extend the life of the pole piece. However, since the polar groups will cause hydrogen bonds to form in the long molecular chains of PAA polymers, hindering the free rotation of the PAA molecular chains, resulting in greater molecular chain rigidity, the toughness of the PAA system pole pieces is generally poor, which is not conducive to bearing the stress caused by the volume expansion of the active material in the pole piece, and is not conducive to the winding process of the battery cell, affecting the improvement of the battery's electrical performance. Summary of the invention

[0003] Based on the above technical background, the purpose of the present invention is to provide a method for preparing a high-toughness pole piece of a PAA system to overcome the shortcomings of the prior art.

[0004] To achieve the above object, the present invention adopts the following technical solution:

[0005] A method for preparing a PAA system high-toughness pole piece comprises the following steps:

[0006] (1) subjecting a polyvinyl alcohol solution to a free radical graft polymerization reaction with acrylic acid under the action of an initiator to obtain a PVA-g-PAA copolymer;

[0007] (2) uniformly mixing the PVA-g-PAA copolymer, the electrode active material, the conductive agent, and the dispersant according to a mass ratio to prepare an electrode slurry;

[0008] (3) The electrode slurry is coated on the current collector, and continuous rolling is performed at different pressures in the designed electrode length range to produce a PAA system high-toughness electrode.

[0009] Preferably, the initiator in step (1) is ammonium persulfate.

[0010] Preferably, the polyvinyl alcohol solution in step (1) is polymerized with acrylic acid at 65±5° C. under vacuum conditions.

[0011] Preferably, the electrode active material in step (2) is a positive electrode active material or a negative electrode active material.

[0012] Preferably, in step (2), the mass ratio of the PVA-g-PAA copolymer, the electrode active material, the conductive agent and the dispersant is (2-6):(88-92):5:1.

[0013] The present invention obtains a novel water-soluble PVA-g-PAA binder by grafting PAA onto the side chain of PVA (polyvinyl alcohol) with good toughness and modifying PAA by adding functional groups. The novel water-soluble binder not only improves the flexibility of the PAA system binder, but also fully combines the excellent bonding property of PVA. The free radical graft polymerization can introduce elasticity to make up for the structural defects of the pure PAA system binder. When preparing the pole piece, different rolling pressures are used to continuously roll the pole piece in segmented sections at set pole piece length intervals to improve the pole piece toughness, make the pole piece less likely to deform, improve the specific capacity of the electrode pole piece, improve the rate performance of the battery, and extend the battery life.

[0014] Preferably, the length of the pole piece length interval described in step (3) is the length of a winding core pole piece, and the pole piece length interval is divided into at least two sections; the rolling pressure increases step by step from the head of the pole piece to the tail of the pole piece, and the compaction density of the tail of the pole piece is increased by 15-20% compared with the compaction density of the head of the pole piece.

[0015] Preferably, the pole piece is wound from a low compaction density pole piece section to a high compaction density pole piece section.

[0016] Preferably, the current collector in step (3) is aluminum foil or copper foil with a thickness of 5-20 μm.

[0017] Another object of the present invention is to provide a pole piece produced by the aforementioned method for producing a PAA system high-toughness pole piece, and a battery produced by the pole piece.

[0018] The present invention has the following beneficial effects: by changing the preparation method of the PAA-type binder, adding PVA functional groups to modify it to obtain a new water-soluble binder as an electrode binder, and performing segmented rolling when rolling the electrode sheet, the toughness of the electrode sheet can be effectively improved, the deformation of the electrode sheet can be inhibited, and the electrical performance of the battery can be improved. DETAILED DESCRIPTION

[0019] The present application is further described in detail below with reference to the embodiments.

[0020] Example 1

[0021] (1) Preparation of PVA-g-PAA copolymer

[0022] ① Add polyvinyl alcohol (PVA) solid (1.5 g) to deionized water (98.5 g) and stir at 95°C until completely dissolved, until a clear PVA solution is obtained.

[0023] ② After the PVA solution is cooled to room temperature, add the solution into a 250 ml Schlenk bottle, add 4.5 g acrylic acid to the PVA solution, then add 0.1 g initiator ammonium persulfate, 0.03 g sodium bisulfite, and add the water evaporated by dissolving the PVA.

[0024] ③ Use a circulating water multi-purpose vacuum pump to evacuate the mixture in the Schlenk bottle for about 30 seconds, then maintain the vacuum condition at 65°C with stirring for 2.5 hours to obtain PVA-g-PAA copolymer.

[0025] (2) Preparation of electrode slurry

[0026] ① Glue preparation: Add appropriate amount of N-methylpyrrolidone (NMP) and 4wt% PVA-g-PAA copolymer to a double planetary stirring tank, stir slowly for 10min at a speed of 20r / min for revolution and 200r / min for dispersion, lower the stirring tank and use a silicone scraper to scrape the powder on the paddle, then stir quickly for 180min at a speed of 20r / min for revolution and 1800r / min for dispersion;

[0027] ② Add conductive agent: add 5wt% conductive carbon black (SP), stir slowly for 10min at a speed of 20r / min for revolution and 200r / min for dispersion, lower the stirring tank and use a silicone scraper to scrape the powder on the paddle, then stir quickly for 90min at a speed of 20r / min for revolution and 1800r / min for dispersion;

[0028] ③ Add dispersant: Add 1wt% of positive electrode dispersant (SDS or PEG), rotate at 20r / min, and disperse at 1800r / min for 30min;

[0029] ④ Adding electrode active materials: adding 90wt% of positive electrode active materials or negative electrode active materials, stirring slowly for 10min at a speed of 20r / min for revolution and 200r / min for dispersion, lowering the stirring tank and using a silicone scraper to scrape the powder on the paddle, and then stirring quickly for 240min at a speed of 20r / min for revolution and 1800r / min for dispersion; wherein the positive electrode active material is sodium iron pyrophosphate Na4Fe3(PO4)2P2O7 of a polyanion system, and the negative electrode active material is iron-doped sodium titanium phosphate.

[0030] ⑤ After degassing, pass through a 150-mesh sieve to complete the preparation of the electrode slurry.

[0031] (3) Preparation of pole piece

[0032] ① The positive electrode slurry prepared above is coated on a 20μm thick current collector aluminum foil to form a pole roll. After the pole roll is baked, different pressures are used to continuously roll the designed pole piece length interval to obtain a positive electrode sheet. The length of the pole piece length interval is the length of a winding core pole piece, and the pole piece length interval is divided into three sections; the rolling pressure increases gradually from the pole piece head to the pole piece tail, and the single-sided surface density of the pole piece is controlled to be 15±2.5mg / cm 2 The compaction density of the pole piece tail is 2.5±0.05g / cm 3 , the compaction density of the middle part of the pole piece is 2.3±0.05g / cm 3 , the compaction density of the pole piece head is 2.1±0.05g / cm 3 The compaction density of the pole piece tail is 15-20% higher than that of the pole piece head.

[0033] ② The negative electrode slurry prepared above is coated on a current collector aluminum foil with a thickness of 20μm, and the designed electrode length interval is continuously rolled with different pressures to obtain a negative electrode sheet. The length of the electrode length interval is the length of a winding core electrode, and the electrode length interval is divided into three sections; the rolling pressure increases gradually from the head of the electrode to the tail of the electrode, and the single-sided surface density of the electrode is controlled to be 15±2.5mg / cm 2 The compaction density of the pole piece tail is 2.5±0.05g / cm 3 , the compaction density of the middle part of the pole piece is 2.3±0.05g / cm 3 , the compaction density of the pole piece head is 2.1±0.05g / cm 3 The compaction density of the pole piece tail is 15-20% higher than that of the pole piece head.

[0034] (4) Winding

[0035] The positive and negative electrode plates and the alumina ceramic-coated PE separator are wound from the lower compaction density electrode plate side to the higher compaction density side to form a battery cell.

[0036] (5) Assembly

[0037] The battery cells are insulated and coated, the poles are welded, and after being inserted into the shell, the shell is sealed and welded and helium inspected. After the battery is assembled, it is placed in an oven for baking. After baking, the battery is disassembled and the moisture content is measured. When the moisture value is below 200PPM, it is injected with liquid at a rate of 5g / Ah. After injection, the battery is prepared after aging, formation, secondary injection, aging and capacity separation.

[0038] Example 2

[0039] Compared with Example 1, the difference is that the mass ratio of the PVA-g-PAA copolymer, the electrode active material, the conductive agent and the dispersant in the electrode slurry is 5:89:5:1.

[0040] Example 3

[0041] Compared with Example 1, the difference is that the mass ratio of the PVA-g-PAA copolymer, the electrode active material, the conductive agent and the dispersant in the electrode slurry is 6:88:5:1.

[0042] Example 4

[0043] Compared with Example 1, the difference is that the mass ratio of the PVA-g-PAA copolymer, the electrode active material, the conductive agent and the dispersant in the electrode slurry is 3:91:5:1.

[0044] Example 5

[0045] Compared with Example 1, the difference is that the mass ratio of the PVA-g-PAA copolymer, the electrode active material, the conductive agent and the dispersant in the electrode slurry is 2:92:5:1.

[0046] Comparative Example 1

[0047] Compared with Example 1, the difference is that the PVA-g-PAA copolymer in the electrode slurry is replaced by PAA.

[0048] Comparative Example 2

[0049] Compared with Example 1, the difference is that a constant pressure is used to roll the electrode sheet, and the compaction density of the entire electrode sheet is controlled to be 2.5±0.05g / cm 3 .

[0050] Comparative Example 3

[0051] Compared with Example 1, the difference is that a constant pressure is used to roll the electrode sheet, and the compaction density of the entire electrode sheet is controlled to be 2.3±0.05g / cm 3 .

[0052] Comparative Example 4

[0053] Compared with Example 1, the difference is that a constant pressure is used to roll the electrode sheet, and the compaction density of the entire electrode sheet is controlled to be 2.1±0.05g / cm 3 .

[0054] Comparative Example 5

[0055] Compared with Example 1, the difference is that the PVA-g-PAA copolymer in the electrode slurry is replaced by PAA, and the electrode sheet is rolled with a constant pressure to control the compaction density of the entire electrode sheet to be 2.5±0.05g / cm3 .

[0056] Performance Testing

[0057] (1) Toughness test: The positive electrode sheet after rolling was cut into a fixed size of 5 cm*25 cm, placed on a platform of a certain height, and pressed against the electrode sheet at the edge of the platform with a flat plate to allow the electrode sheet to sag naturally. The lateral length of the electrode sheet extending out of the platform when it sags 5 cm was measured to evaluate the flexibility of the electrode sheet. The shorter the lateral length, the better the flexibility. The test results are shown in Table 1.

[0058] (2) Peel strength test: A metal plate was used as a carrier, and double-sided tape was pasted on its surface. The positive electrode sheet coated with PVA-g-PAA slurry was then pasted on the other side of the tape. The copper foil was stretched and peeled off 180° at a speed of 100 mm / min. The test results are shown in Table 1.

[0059] (3) Capacity retention rate test: At 25°C and normal pressure (0.1MPa), the sodium ion battery prepared in the embodiment and the comparative example is charged at a constant current of 0.2C rate to a voltage of 4.05V, and then discharged at a constant current of 0.2C rate to a voltage of 2.5V after standing for 15 minutes. The discharge capacity is recorded as the first discharge gram capacity of the sodium ion battery. The sodium ion battery is subjected to 200 cycles of charge and discharge test according to the above method, and the discharge gram capacity of the 200th cycle is detected. The capacity retention rate (%) of the sodium ion battery after 200 cycles = discharge gram capacity of the 200th cycle / first discharge gram capacity*100%. The test results are shown in Table 1.

[0060] Table 1 Performance test table

[0061]

[0062] It can be seen from Table 1 that the lateral length of the pole piece extending out of the platform in Examples 1-5 is smaller than that in Comparative Examples 1-5, indicating that by changing the preparation method of the PAA-type binder, adding PVA-g-PAA obtained by modifying the PVA functional group as an electrode binder can improve the toughness of the pole piece, and having a peel strength of more than 36 N / m can reduce the risk of the pole piece falling off the current collector after multiple swellings; when rolling the pole piece, segmented rolling can effectively improve the toughness of the pole piece, inhibit pole piece deformation, and improve the electrical performance of the battery.

[0063] The above specific embodiments are merely explanations of the present application and are not limitations of the present application. After reading this specification, those skilled in the art may make modifications to the embodiments without any creative contribution as needed. However, as long as they are within the scope of the claims of the present application, they are protected by the patent law.

Claims

1. A method for preparing a PAA system high-toughness pole piece, characterized in that: The following steps are involved: (1) subjecting a polyvinyl alcohol solution to a free radical graft polymerization reaction with acrylic acid under the action of an initiator to obtain a PVA-g-PAA copolymer; (2) uniformly mixing the PVA-g-PAA copolymer, the electrode active material, the conductive agent, and the dispersant according to a mass ratio to prepare an electrode slurry; (3) The electrode slurry is coated on the current collector, and continuous rolling is performed at different pressures in the designed electrode length range to produce a PAA system high-toughness electrode.

2. The method for preparing a PAA system high-toughness pole piece according to claim 1, characterized in that: The initiator in step (1) is ammonium persulfate.

3. The method for preparing a PAA system high-toughness pole piece according to claim 1, characterized in that: The polyvinyl alcohol solution in step (1) is polymerized with acrylic acid at 65±5° C. under vacuum conditions.

4. The method for preparing a PAA system high-toughness pole piece according to claim 1, characterized in that: The electrode active material in step (2) is a positive electrode active material or a negative electrode active material.

5. The method for preparing a PAA system high-toughness pole piece according to claim 1, characterized in that: In step (2), the mass ratio of PVA-g-PAA copolymer, electrode active material, conductive agent and dispersant is (2-6):(88-92):5:

1.

6. The method for preparing a PAA system high-toughness pole piece according to claim 1, characterized in that: The length of the pole piece length interval described in step (3) is the length of a winding core pole piece, and the pole piece length interval is divided into at least three sections; the rolling pressure increases step by step from the head of the pole piece to the tail of the pole piece, and the compaction density of the tail of the pole piece is increased by 15-20% compared with the compaction density of the head of the pole piece.

7. The method for preparing a PAA system high-toughness pole piece according to claim 1, characterized in that: The pole piece is wound from a low compaction density pole piece section to a high compaction density pole piece section.

8. The method for preparing a PAA system high-toughness pole piece according to claim 1, characterized in that: The current collector in step (3) is aluminum foil or copper foil with a thickness of 5-20 μm.

9. A pole piece, characterized in that: It is prepared by the preparation method of the PAA system high-toughness pole piece according to any one of claims 1 to 8.

10. A battery, characterized in that: Including the pole piece as claimed in claim 9.