Double-layer coated sodium ferric sulfate positive electrode material, preparation method thereof, positive plate and battery
Through the double-layer cladding structure, polypolysaccharides and conductive polymers are used to improve the hydrophobicity and conductivity of sodium ferrosulfate positive electrode material, solving the problem of easy water absorption and deterioration of the material, and significantly improving the sodium storage capacity and magnification of sodium ion batteries performance.
Patent Information
- Application Number
- CN202411032663.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The existing sodium ferrosulfate positive electrode materials are easy to absorb water, deteriorate, and are prone to inactivation, resulting in poor sodium storage capacity, poor rate performance and reduced circulation capacity retention. The combination of inorganic conductive carbon materials with sodium ferrosulfate at low sintering temperature Insufficient force affects electrochemical properties.
Using a double-layer cladding structure, the first cladding layer is formed by carbonization of polypolysaccharides, and the second cladding layer is a conductive polymer. Through specific sintering temperature and time control, the hydrophobicity and conductivity of the material are improved, and the iron sulfate is enhanced. The binding force of sodium.
The hydrophobicity, conductivity and sphericality of the sodium ferric sulfate cathode material is significantly improved, the sodium storage capacity and rate performance of sodium ion batteries are improved, and the circulation stability of the material is extended.
Smart Images

Figure CN118969995A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of sodium ion batteries and relates to new energy batteries, and specifically relates to a double-layer coated sodium iron sulfate positive electrode material and a preparation method and application thereof. Background Art
[0002] Sodium ion batteries are ideal secondary batteries for future low-speed electric vehicles and large-scale energy storage systems due to their significant advantages such as abundant sodium salt reserves, low raw material costs, and a wide operating temperature range. x Fe y (SO4) z It has significant advantages such as high operating voltage and low production cost. x Fe y (SO4) z The material easily absorbs water, deteriorates and deactivates, resulting in poor sodium storage gram capacity (specific capacity), poor rate performance and significantly reduced cycle capacity retention rate; at the same time, the intrinsic conductivity of its pure phase material is low, which seriously affects the sodium storage electrochemical performance of this type of positive electrode material, showing low sodium storage specific capacity, poor long-cycle stability and high-rate performance, etc., which hinders the practical application of this type of positive electrode material.
[0003] Many literatures have reported that inorganic conductive carbon materials (such as carbon nanotubes, carbon fibers, reduced graphene oxide or graphene, etc.) can enhance the Na x Fe y (SO4) z The mechanism of the electrochemical properties of the material, but the inorganic conductive carbon material is sintered at a lower temperature with Na x Fe y (SO4) z The binding force is weak and the ideal coating effect cannot be achieved (synthetic Na x Fe y (SO4) z The sintering temperature of the material is lower than 400°C. If it exceeds this temperature, it is easy to produce impurities, and when the temperature is greater than 450°C, NaxFey(SO4)z will decompose due to structural instability). Therefore, coating NaxFey(SO4)z with an organic carbon source is an effective method to improve its low conductivity and electrochemical properties. Some conductive polymers have certain ion exchange effects and are easily wetted by electrolytes, which can improve the ion migration kinetics of positive electrode materials. Therefore, they are also used to improve the electrochemical properties of NaxFey(SO4)z. In addition, the performance of NaxFey(SO4)z positive electrode materials can be further improved by mixing conductive polymers with conductive carbon materials or organic carbon sources.
[0004] However, due to the lack of design of the coating layer structure, the coating strategy using a combination of multiple carbon sources failed to give full play to the advantages of each carbon source, so that the specific capacity, rate performance and storage performance of the NaxFey(SO4)z cathode material did not meet expectations. Therefore, under the premise of a sintering temperature below 400°C, how to find a suitable carbon source and what kind of structural design to make for the coating layer, and then prepare a coated sodium iron sulfate cathode material with excellent performance to cope with the challenges of low gram capacity, poor rate performance, strong water absorption, poor storage performance, and high preparation cost, is an urgent problem to be solved in this field.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The purpose of the present invention includes providing a double-layer coated sodium ferric sulfate positive electrode material and a preparation method and application thereof, aiming to improve the hydrophobicity and conductivity of the sodium ferric sulfate positive electrode material, thereby improving the sodium storage gram capacity and rate performance of the sodium ion battery.
[0007] In a first aspect, the present invention provides a double-layer coated sodium ferric sulfate positive electrode material, which includes sodium ferric sulfate, a first coating layer on the outer surface of the sodium ferric sulfate, and a second coating layer outside the first coating layer; the first coating layer is formed by carbonization of polysaccharide, and the second coating layer is a conductive polymer.
[0008] In some embodiments of the present invention, the molecular formula of sodium ferric sulfate is Na x Fe y (SO4) z , where 1≤x / y≤2, x+2y=2z.
[0009] In some embodiments of the present invention, the polysaccharide includes at least one of hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose, ethyl cellulose, hydroxymethyl cellulose, hydroxypropyl cellulose, carboxymethyl cellulose, hydroxypropyl starch ether and cyclodextrin; the conductive polymer includes at least one of polypyrrole, polyaniline, polyindole, polycarbazole, polythiophene, polyacetylene and polyphenylene vinylene.
[0010] In some embodiments of the present invention, the carbon content of the double-layer coated sodium iron sulfate positive electrode material is 1.50%-2.10%.
[0011] In some embodiments of the present invention, the median particle size Dv(50) of the double-layer coated sodium iron sulfate positive electrode material is 0.8-2.5 μm.
[0012] In some embodiments of the present invention, at least one of the following features 1-2 is met:
[0013] Feature 1: The resistance of the obtained sodium iron sulfate positive electrode material powder is 70-110Ω·cm;
[0014] Feature 2: The wetting angle of the sodium iron sulfate positive electrode material powder is 90-120°.
[0015] In a second aspect, the present invention also provides a method for preparing a double-layer coated sodium iron sulfate positive electrode material, comprising the following steps:
[0016] Step 1: mixing a sodium source, an iron source, an antioxidant and the polysaccharide, and then crushing the mixture to obtain a precursor;
[0017] Step 2: sintering the precursor for the first time and crushing it to obtain a pre-sintered material;
[0018] Step 3: uniformly mixing the pre-burned material and the conductive polymer to obtain a process material;
[0019] Step 4: After the process material is sintered for the second time, the double-layer coated sodium iron sulfate positive electrode material is obtained.
[0020] In some embodiments of the present invention, the preparation method of the double-layer coated sodium iron sulfate positive electrode material satisfies at least one of the following characteristics I-III:
[0021] Feature I: The sodium source includes at least one of anhydrous sodium sulfate and sodium sulfate hydrate;
[0022] Feature II: The iron source includes at least one of anhydrous ferrous sulfate and ferrous sulfate hydrate;
[0023] Feature III: The antioxidant includes at least one of ascorbic acid, citric acid, oxalic acid, hydrazine and paraformaldehyde.
[0024] In some embodiments of the present invention, the preparation method of the double-layer coated sodium iron sulfate positive electrode material satisfies at least one of the following characteristics ad:
[0025] Feature a: The polysaccharide accounts for 0.01%-15% of the mass of the sodium source;
[0026] Feature b: The mass of the antioxidant is 0.01%-10% of the mass of the sodium source;
[0027] Feature c: The mass of the conductive polymer is 0.01%-3.5% of the mass of the pre-sintered material;
[0028] Feature d: The mass ratio of the sodium source to the iron source is 25%-51%.
[0029] In some embodiments of the present invention, the preparation method of the double-layer coated sodium iron sulfate positive electrode material satisfies at least one of the following characteristics 1-2:
[0030] Feature 1: The temperature of the first sintering is 280°C-350°C, and the sintering time is 4-24h;
[0031] Feature 2: The temperature of the second sintering is 150°C-390°C, and the sintering time is 6-12h.
[0032] In some embodiments of the present invention, the pulverizing process in step 1 uses a jet mill, the pulverizing pressure of the jet mill is 0.2-0.4 MPa, the feeding frequency is 20-35 Hz, and the classification frequency is 200-260 Hz.
[0033] In some embodiments of the present invention, the mixing in step 3 is high-speed mixing. In the mixing process of the high-speed mixer, the first stage speed is 200-280 rpm, and the mixing time is 2-8 min; the second stage speed is 800-1200 rpm, and the mixing time is 10-20 min; the third stage speed is 1400-1800 rpm, and the mixing time is 25-35 min.
[0034] In a third aspect, the present invention further provides a positive electrode plate, which comprises the double-layer coated sodium iron sulfate positive electrode material provided by the present invention or the double-layer coated sodium iron sulfate positive electrode material prepared by the preparation method provided by the present invention.
[0035] In a fourth aspect, the present invention further provides a sodium ion battery, comprising the positive electrode plate provided by the present invention.
[0036] The beneficial effects of the present invention include:
[0037] The present invention provides a double-layer coated sodium iron sulfate positive electrode material, wherein the first coating layer on the outer surface of the sodium iron sulfate is formed by carbonization of polysaccharide, and the main component is amorphous carbon, and the second coating layer outside the first coating layer is a conductive polymer. The double-layer coating synergistically improves the hydrophobicity, sphericity, conductivity and wettability of the positive electrode material to the electrolyte, thereby improving the sodium storage capacity and rate performance of the positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0039] Figure 1 A process flow chart for preparing a sodium iron sulfate positive electrode material provided in an embodiment of the present invention;
[0040] Figure 2This is the XRD pattern of the sodium iron sulfate positive electrode material obtained in Example 1;
[0041] Figure 3 is a SEM image of the sodium iron sulfate positive electrode material obtained in Example 1;
[0042] Figure 4 This is a SEM image of the sodium iron sulfate positive electrode material obtained in Comparative Example 1;
[0043] Figure 5 This is the SEM image of the sodium iron sulfate positive electrode material obtained in Comparative Example 4. DETAILED DESCRIPTION
[0044] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0045] The endpoints and any values of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be considered as specifically disclosed in this article.
[0046] In an embodiment of the present invention, a double-layer coated sodium ferric sulfate positive electrode material is provided, which includes sodium ferric sulfate, a first coating layer on the outer surface of the sodium ferric sulfate, and a second coating layer outside the first coating layer. The first coating layer is formed by sintering polysaccharide, and the second coating layer is formed by sintering a conductive polymer.
[0047] In this embodiment, the first coating layer is a coating carbon layer formed by carbonization of polysaccharide. On the one hand, the coating carbon layer mainly exists in the form of amorphous carbon and is graphitized to a certain extent. It has good conductivity and stable structure, ensuring rapid electron transmission and improving sodium storage capacity and rate performance. On the other hand, polysaccharide is used as a carbon source and can be carbonized at a temperature below 400°C, ensuring a high degree of crystallization of the main crystal phase without introducing impurities. Moreover, after carbonization, polysaccharide can react with Na x Fe y (SO4) z It has a strong binding force, thus forming a stable coating structure; further, the coated carbon layer exhibits good hydrophobicity, which effectively prevents the sodium iron sulfate active material from reacting with water in the air and causing deterioration.
[0048] In this embodiment, the second coating layer is a conductive polymer. On the one hand, the conductive polymer and the first coating layer together form a double hydrophobic structure, further reducing the influence of moisture in the air and increasing the content of active substances in the positive electrode material; on the other hand, the conductive polymer has ion exchange properties and is easily wetted by the electrolyte; finally, the coating of the conductive polymer improves the sphericity of the positive electrode material.
[0049] Therefore, through the setting of a specific double-coating structure, the hydrophobicity, conductivity and sphericity of the sodium iron sulfate material are significantly improved, further improving the sodium storage capacity and rate performance of the sodium ion battery.
[0050] In some embodiments of the present invention, the median particle size Dv(50) of the double-layer coated sodium iron sulfate positive electrode material is 0.8-2.5 μm, specifically 0.8 μm, 1.0 μm, 1.5 μm, 2.0 μm, 2.5 μm or any value between 0.8-2.5 μm.
[0051] The present invention provides a method for preparing a double-layer coated sodium iron sulfate positive electrode material, the preparation process is as follows Figure 1 As shown, a sodium source, an iron source, an antioxidant and a polysaccharide are mixed, crushed to obtain a precursor, and then sintered for the first time and crushed to obtain a pre-burned material; a conductive polymer is added and evenly mixed to obtain a process material; and after a second sintering, the double-layer coated sodium iron sulfate positive electrode material is obtained.
[0052] In some embodiments, in step 1, the polysaccharide is 0.01%-15% of the mass of the sodium source, specifically 0.01%, 0.1%, 0.5%, 1%, 3%, 5%, 10%, 15% or any value between 0.01% and 15%. If the amount of polysaccharide is too little, the first layer coating of sodium ferric sulfate is insufficient, the structural stability of the first coating layer is reduced, and the hydrophobic effect is poor, reducing the purity of sodium ferric sulfate; thereby reducing the electron transfer efficiency, affecting the sodium storage capacity and rate performance of the sodium battery. If the amount of polysaccharide is too much, the specific capacity of the positive electrode material will be reduced, so the coating amount of polysaccharide needs to be set within a reasonable range.
[0053] In some embodiments, the mixing equipment in step 1 is one or more of a ribbon mixer, a double cone mixer, a plowshare mixer, a double-shaft paddle mixer, and a high-speed mixer.
[0054] In some embodiments, the atmosphere of the first sintering in step 2 and the second sintering in step 4 is an inert atmosphere, and the specific inert atmosphere can be at least one of argon, nitrogen, helium, argon-hydrogen mixed gas, and nitrogen-hydrogen mixed gas.
[0055] In some embodiments, in step 2, the first sintering temperature is 320-350°C, and the sintering time is 4-24h. The specific sintering temperature can be 320°C, 330°C, 340°C, 350°C or any value between 320-350°C, and the specific sintering time can be 4h, 5h, 10h, 15h, 20h, 24h or any value between 4-24h. A lower sintering temperature and / or a shorter sintering time will result in a lower degree of carbonization of the first coating layer formed by the polysaccharide, and Na x Fe y (SO4) z The crystallinity is not high, and the first coating layer and Na x Fe y (SO4) z The bonding force is low; while too high sintering temperature and / or long sintering time will lead to the generation of impurities, reduce active sites, and weaken the electrochemical performance.
[0056] In some embodiments, in step 3, the mass of the conductive polymer is 0.01%-3.5% of the mass of the pre-sintered material, and specifically can be 0.01%, 0.05%, 0.1%, 0.5%, 1%, 2%, 3%, 3.5% or any value between 0.01% and 3.5%. If the amount of conductive polymer is too small, the surface of the positive electrode material cannot be uniformly coated, and the hydrophobicity of the material is affected; thereby reducing the ion exchangeability and electrolyte wettability, as well as the storage performance of the positive electrode material. If the amount of conductive polymer is too much, it not only increases the cost, but also reduces the specific capacity of the positive electrode material, so the coating amount of the conductive polymer needs to be set within a reasonable range.
[0057] In some embodiments, in step 4, the temperature of the second sintering is 150°C-390°C, and the sintering time is 6-12h. The specific sintering temperature can be 150°C, 200°C, 250°C, 300°C, 350°C, 390°C or any value between 150-390°C, and the specific sintering time can be 6h, 7h, 8h, 9h, 10h, 11h, 12h or any value between 6-12h. A lower sintering temperature and / or a shorter sintering time will result in a decrease in the bonding force of the second coating layer formed by the conductive polymer, and will not effectively improve the sphericity of the particles and the compacted density of the powder; while an excessively high sintering temperature and / or a longer sintering time will result in the active material being decomposed due to high temperature or the particles being melted and grown, reducing the purity of the main crystal phase and deteriorating the electrochemical performance.
[0058] The present invention also provides a positive electrode plate, comprising the double-layer coated sodium ferric sulfate positive electrode material described in any one of the aforementioned embodiments or the double-layer coated sodium ferric sulfate positive electrode material prepared by any one of the preparation methods described.
[0059] The present invention also provides a sodium ion battery, which is obtained by assembling positive electrode plates.
[0060] The present invention provides a method for preparing a double-layer coated sodium iron sulfate positive electrode material. Please refer to the process flow chart Figure 1 The features and performances of the present invention are further described in detail below in conjunction with the embodiments.
[0061] Example 1
[0062] Step 1: Weigh anhydrous sodium sulfate, ferrous sulfate heptahydrate, ascorbic acid, and ethyl cellulose, add them into a double cone mixer and mix thoroughly, wherein the mass of the anhydrous sodium sulfate is 30.05% of the mass of ferrous sulfate heptahydrate, the mass of the ascorbic acid is 4.03% of the mass of the anhydrous sodium sulfate, and the mass of the ethyl cellulose is 12.22% of the mass of the sodium source. Then grind them in a jet mill, and discharge the material to obtain a precursor. The jet mill is set to a pressure of 0.35 MPa, a feed frequency of 25 Hz, and a classification frequency of 250 Hz.
[0063] Step 2: The precursor was transferred to a tube furnace, sintered at 340° C. in a nitrogen atmosphere for 8 h, and then crushed to obtain a pre-sintered material.
[0064] Step 3: Evenly mix the pre-sintered material and polyaniline in a high-speed mixer, and discharge the material to obtain the process material. The polyaniline is 0.25% of the mass of the pre-sintered material, and the mixing parameters of the high-speed mixer are: the first stage speed is 250 rpm, the mixing time is 5 minutes; the second stage speed is 1000 rpm, the mixing time is 15 minutes; the third stage speed is 1500 rpm, and the mixing time is 30 minutes.
[0065] Step 4: The process material was transferred to a tube furnace and sintered for 8 h in a nitrogen atmosphere at 380 °C to obtain a double-layer coated sodium iron sulfate positive electrode material.
[0066] The SEM results are as follows Figure 3 As shown in the figure, the median particle size Dv(50) of the double-layer coated sodium iron sulfate positive electrode material is 1.1μm, the particle size uniformity is relatively high, and there is no obvious local agglomeration phenomenon. Such uniform fine particles can shorten the transmission distance of sodium ions in the sodium iron sulfate particles and accelerate the migration kinetics of sodium ions.
[0067] The XRD spectrum of sodium iron sulfate material is as follows Figure 2 As shown, the XRD spectrum is consistent with that reported in other literatures, basically no impurity phase is generated, and the crystallinity is good. This is because after the iron source and the sodium source are crushed, the particle size is reduced, which increases the reaction activity between the particles. In the first sintering stage, the crystal water of hydrated ferrous sulfate can be removed, which promotes the reaction of the iron source and the sodium source without generating impurity phases.
[0068] Example 2
[0069] The difference between this embodiment and embodiment 1 is that, in step 3, the polyaniline accounts for 0.14% of the mass of the pre-sintered material, and other conditions and parameters are exactly the same as those in embodiment 1.
[0070] The median particle size Dv(50) of the obtained double-layer coated sodium iron sulfate positive electrode material is 1.05 μm.
[0071] Example 3
[0072] The only difference between this embodiment and embodiment 1 is that in step 3, the polyaniline is replaced by polypyrrole, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0073] The median particle size Dv(50) of the obtained double-layer coated sodium iron sulfate positive electrode material is 1.12 μm.
[0074] Example 4
[0075] The only difference between this embodiment and embodiment 1 is that in step 1, the polysaccharide substance is replaced by hydroxypropyl cellulose, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0076] The median particle size Dv(50) of the obtained double-layer coated sodium iron sulfate positive electrode material is 1.08 μm.
[0077] Example 5
[0078] The difference between this embodiment and embodiment 1 is that, in step 3, the polyaniline is 0.01% of the mass of the pre-sintered material, and other conditions and parameters are exactly the same as those in embodiment 1.
[0079] The median particle size Dv(50) of the obtained double-layer coated sodium iron sulfate positive electrode material is 0.87 μm.
[0080] Example 6
[0081] The difference between this embodiment and embodiment 1 is that, in step 3, the polyaniline is 0.1% of the mass of the pre-sintered material, and other conditions and parameters are exactly the same as those in embodiment 1.
[0082] The median particle size Dv(50) of the obtained double-layer coated sodium iron sulfate positive electrode material is 0.96 μm.
[0083] Example 7
[0084] The only difference between this embodiment and embodiment 1 is that in step 4, the temperature of the second sintering is 150° C., and the other conditions and parameters are exactly the same as those in embodiment 1.
[0085] The median particle size Dv(50) of the obtained double-layer coated sodium iron sulfate positive electrode material is 1.03 μm.
[0086] Example 8
[0087] Step 1: Weigh anhydrous sodium sulfate, ferrous sulfate heptahydrate, citric acid, and ethyl cellulose, add them into a double cone mixer and mix thoroughly, the mass of the anhydrous sodium sulfate is 25.04% of the mass of ferrous sulfate heptahydrate, the mass of the citric acid is 0.01% of the mass of the anhydrous sodium sulfate, and the mass of the ethyl cellulose is 15% of the mass of the sodium source. Then grind them in a jet mill, and discharge the material to obtain a precursor. The jet mill is set to a pressure of 0.35 MPa, a feed frequency of 25 Hz, and a classification frequency of 250 Hz.
[0088] Step 2: The precursor is transferred to a tube furnace, sintered for 24 hours in a nitrogen atmosphere at 280° C., and then crushed to obtain a pre-sintered material.
[0089] Step 3: The pre-burned material and polyaniline are uniformly mixed in a high-speed mixer, wherein the polyaniline is 0.01% of the mass of the pre-burned material, and the high-speed mixer is added, and the mixing parameters are set as follows: the first stage speed is 250 rpm, and the mixing time is 5 min; the second stage speed is 1000 rpm, and the mixing time is 15 min; the third stage speed is 1500 rpm, and the mixing time is 30 min, and the process material is obtained by discharging.
[0090] Step 4: The process material was transferred to a tube furnace and sintered for 12 h in a nitrogen atmosphere at 150°C to obtain a double-layer coated sodium iron sulfate positive electrode material with a median particle size Dv(50) of 0.82 μm.
[0091] Example 9
[0092] Step 1: Weigh anhydrous sodium sulfate, ferrous sulfate heptahydrate, oxalic acid, and ethyl cellulose, add them into a double cone mixer and mix thoroughly, the mass of the anhydrous sodium sulfate is 50.08% of the mass of ferrous sulfate heptahydrate, the mass of the oxalic acid is 10% of the mass of the anhydrous sodium sulfate, and the mass of the ethyl cellulose is 0.01% of the mass of the sodium source. Then grind them in a jet mill, and discharge the material to obtain a precursor. The jet mill is set to a pressure of 0.35 MPa, a feed frequency of 25 Hz, and a classification frequency of 250 Hz.
[0093] Step 2: The precursor was transferred to a tube furnace, sintered at 350° C. in a nitrogen atmosphere for 4 h, and then crushed to obtain a pre-sintered material.
[0094] Step 3: The pre-burned material and polyaniline are uniformly mixed in a high-speed mixer, wherein the polyaniline accounts for 3.5% of the mass of the pre-burned material. The high-speed mixer is added, and the mixing parameters are set as follows: the first stage speed is 250 rpm, and the mixing time is 5 min; the second stage speed is 1000 rpm, and the mixing time is 15 min; the third stage speed is 1500 rpm, and the mixing time is 30 min. The process material is obtained by discharging.
[0095] Step 4: The process material was transferred to a tube furnace and sintered for 6 h in a nitrogen atmosphere at 390 °C to obtain a double-layer coated sodium iron sulfate positive electrode material with a median particle size Dv(50) of 1.93 μm.
[0096] Comparative Example 1
[0097] Step 1: Weigh anhydrous sodium sulfate, ferrous sulfate heptahydrate, ascorbic acid, and carbon nanotubes, add them into a double cone mixer and mix thoroughly, wherein the mass of the anhydrous sodium sulfate is 30.05% of the mass of ferrous sulfate heptahydrate, the mass of the ascorbic acid is 4.03% of the mass of the anhydrous sodium sulfate, and the mass of the carbon nanotubes is 4.67% of the mass of the sodium source. Then grind them in a jet mill, and discharge the material to obtain a precursor. The jet mill is set to a pressure of 0.35 MPa, a feed frequency of 25 Hz, and a classification frequency of 250 Hz.
[0098] Step 2: The precursor was transferred to a tube furnace, sintered at 340° C. in a nitrogen atmosphere for 8 h, and then crushed to obtain a pre-sintered material.
[0099] Step 3: Add the pre-burned material into a high-speed mixer for stirring, and set the mixing parameters as follows: the first stage speed is 250 rpm, the time is 5 minutes; the second stage speed is 1000 rpm, the time is 15 minutes; the third stage speed is 1500 rpm, the time is 30 minutes, and the process material is obtained by discharging.
[0100] Step 4: The process material was transferred to a tube furnace and sintered for 8 h in a nitrogen atmosphere at 380° C. to obtain a carbon nanotube-coated sodium iron sulfate positive electrode material with a median particle size Dv(50) of 2.3 μm.
[0101] Its SEM picture is as follows Figure 4 As shown, compared to Figure 3 and Figure 5 The particle size distribution of the powders of Example 1 and Comparative Example 4 shows that the particle size uniformity of Comparative Example 1 is worse, the particle size range is mainly 1.2-5 μm, and there is obvious agglomeration in some parts.
[0102] Comparative Example 2
[0103] Step 1: Weigh anhydrous sodium sulfate, ferrous sulfate heptahydrate, ascorbic acid, ethyl cellulose, and polyaniline, add them into a double cone mixer and mix them thoroughly, wherein the mass of the anhydrous sodium sulfate is 30.05% of the mass of ferrous sulfate heptahydrate, the mass of the ascorbic acid is 4.03% of the mass of the anhydrous sodium sulfate, the mass of the ethyl cellulose is 12.22% of the mass of the sodium source, and the mass of the polyaniline is 0.25% of the mass of the sodium source. Then, grind them in an air flow mill, and discharge the material to obtain a precursor. The air flow mill is set to a pressure of 0.35 MPa, a feed frequency of 25 Hz, and a classification frequency of 250 Hz.
[0104] Step 2: The precursor was transferred to a tube furnace, sintered at 340° C. in a nitrogen atmosphere for 8 h, and then crushed to obtain a pre-sintered material.
[0105] Step 3: Add the pre-burned material into a high-speed mixer for stirring, and set the mixing parameters as follows: the first stage speed is 250 rpm, the time is 5 minutes; the second stage speed is 1000 rpm, the time is 15 minutes; the third stage speed is 1500 rpm, the time is 30 minutes, and the process material is obtained by discharging.
[0106] Step 4: The process material was transferred to a tube furnace and sintered for 8 hours at 380°C in a nitrogen atmosphere to obtain a mixed carbon composite sodium iron sulfate positive electrode material with a median particle size Dv(50) of 1.8 μm.
[0107] Comparative Example 3
[0108] Step 1: Weigh anhydrous sodium sulfate, ferrous sulfate heptahydrate, and ascorbic acid, add them into a double cone mixer and mix them thoroughly, wherein the mass of the anhydrous sodium sulfate is 30.05% of the mass of the ferrous sulfate heptahydrate, and the mass of the ascorbic acid is 4.03% of the mass of the anhydrous sodium sulfate. Add the above mixture into a jet mill for pulverization, set the pressure to 0.35 MPa, the feed frequency to 25 Hz, the classification frequency to 250 Hz, and discharge to obtain a precursor.
[0109] Step 2: The precursor was transferred to a tube furnace, sintered at 340° C. in a nitrogen atmosphere for 8 h, and then crushed to obtain a pre-sintered material.
[0110] Step 3: Add the pre-burned material, ethyl cellulose and polyaniline into a high-speed mixer for mixing, wherein the mass of ethyl cellulose is 4.55% of the mass of the pre-burned material, and the mass of polyaniline is 0.14% of the mass of the pre-burned material. Set the mixing parameters as follows: the first stage speed is 250 rpm, the mixing time is 5 minutes; the second stage speed is 1000 rpm, the mixing time is 15 minutes; the third stage speed is 1500 rpm, the mixing time is 30 minutes, and the process material is obtained by discharging.
[0111] Step 4: The process material was transferred to a tube furnace and sintered for 8 h in a nitrogen atmosphere at 380°C to obtain a single-layer mixed-coated sodium iron sulfate positive electrode material with a median particle size Dv(50) of 1.2 μm.
[0112] Comparative Example 4
[0113] The difference between this comparative example and Example 1 is that in step 3, during the high-speed uniform mixing process, no conductive polymer is introduced, and the other conditions and parameters are exactly the same as those in Example 1. The SEM results are shown in FIG. Figure 5 As shown, the median particle size Dv(50) is 0.93 μm.
[0114] Comparative Example 5
[0115] Step 1: Weigh anhydrous sodium sulfate, ferrous sulfate heptahydrate, ascorbic acid, and carbon nanotubes, add them into a double cone mixer and mix thoroughly, wherein the mass of the anhydrous sodium sulfate is 30.05% of the mass of ferrous sulfate heptahydrate, the mass of the ascorbic acid is 4.03% of the mass of the anhydrous sodium sulfate, and the mass of the carbon nanotubes is 12.22% of the mass of the sodium source. Then grind them in a jet mill, and discharge the material to obtain a precursor. The jet mill is set at a pressure of 0.35 MPa, a feeding frequency of 25 Hz, and a classification frequency of 250 Hz.
[0116] Step 2: The precursor was transferred to a tube furnace, sintered at 340° C. in a nitrogen atmosphere for 8 h, and then crushed to obtain a pre-sintered material.
[0117] Step 3: The pre-burned material and ethyl cellulose are uniformly mixed in a high-speed mixer, wherein the ethyl cellulose accounts for 0.25% of the mass of the pre-burned material. The mixing parameters are set as follows: the first stage speed is 250 rpm, the mixing time is 5 min; the second stage speed is 1000 rpm, the mixing time is 15 min; the third stage speed is 1500 rpm, the mixing time is 30 min, and the process material is obtained by discharging.
[0118] Step 4: The process material was transferred to a tube furnace and sintered for 8 h in a nitrogen atmosphere at 380 °C to obtain a double-layer coated sodium iron sulfate positive electrode material with a median particle size Dv(50) of 2.58 μm.
[0119] Comparative Example 6
[0120] Step 1: Weigh anhydrous sodium sulfate, ferrous sulfate heptahydrate, and ascorbic acid, add them into a double cone mixer and mix them thoroughly. The mass of the anhydrous sodium sulfate is 30.05% of the mass of the ferrous sulfate heptahydrate, and the mass of the ascorbic acid is 4.03% of the mass of the anhydrous sodium sulfate. Then grind them in a jet mill to obtain a precursor. The jet mill is set at a pressure of 0.35 MPa, a feeding frequency of 25 Hz, and a classification frequency of 250 Hz.
[0121] Step 2: The precursor was transferred to a tube furnace, sintered at 340° C. in a nitrogen atmosphere for 8 h, and then crushed to obtain a pre-sintered material.
[0122] Step 3: The pre-burned material and polyaniline are uniformly mixed in a high-speed mixer, wherein the polyaniline accounts for 0.25% of the mass of the pre-burned material, and the mixing parameters are set as follows: the first stage speed is 250 rpm, the mixing time is 5 min; the second stage speed is 1000 rpm, the mixing time is 15 min; the third stage speed is 1500 rpm, the mixing time is 30 min, and the process material is obtained by discharging.
[0123] Step 4: The process material was transferred to a tube furnace and sintered at 380°C in a nitrogen atmosphere for 8 hours to obtain a double-layer coated sodium iron sulfate positive electrode material with a median particle size Dv(50) of 0.76 μm.
[0124] Effect Example 1
[0125] In order to verify the performance of the sodium ferric sulfate product of the present invention, the sodium ferric sulfate materials prepared in each embodiment and comparative example were tested for carbon content. The equipment used was an infrared carbon-sulfur instrument. The specific steps were as follows:
[0126] Debug the equipment to the standard test mode, weigh an appropriate amount of sodium ferric sulfate positive electrode material sample, and then fully cover the sample surface with flux; turn on the combustion furnace and set the working pressure of the combustion furnace; when the "carbon voltage" on the test software is stable, correct the reference sample so that its value is 0; finally test the sample and record the data.
[0127] The test results are shown in Table 1.
[0128] Effect Example 2
[0129] In order to verify the performance of the sodium iron sulfate product of the present invention, the sodium iron sulfate materials prepared in each embodiment and comparative example were subjected to a water contact angle test. The equipment used was an automatic optical contact angle measuring instrument. The specific steps were as follows:
[0130] The equipment was adjusted to the standard test mode. An appropriate amount of sodium iron sulfate positive electrode material sample was taken and dried, and then pressed into a cylindrical tablet with a diameter of 10 mm and a thickness of 1 mm in a pressurized mold. Deionized water was used as the test liquid, and the static contact angle was calculated using the width-height method. Three groups of static contact angle data were tested in parallel and the average value was taken.
[0131] The test results are shown in Table 1.
[0132] Effect Example 3
[0133] In order to verify the performance of the sodium ferric sulfate product of the present invention, the resistivity of the sodium ferric sulfate materials prepared in each embodiment and comparative example was tested using a powder resistivity meter. The specific steps are as follows:
[0134] The four-probe method is used for testing: first, take an appropriate amount of sodium iron sulfate positive electrode material sample and pour it into the feeding cup, then adjust the height to provide a reference point for measuring the sample thickness later; then rotate the handwheel to manually pressurize to 8MPa, and finally read and collect data in the display window.
[0135] The test results are shown in Table 1.
[0136] Effect Example 4
[0137] In order to verify the performance of the sodium ferric sulfate product of the present invention, the sodium ferric sulfate materials prepared in each embodiment and comparative example were tested for moisture content. The equipment used was a coulometric moisture tester. The specific test steps were as follows:
[0138] The instrument was calibrated with a blank sample at 170°C, and then an appropriate amount of sodium iron sulfate positive electrode material sample was weighed and sealed, placed in the instrument, and the amount of electricity electrolyzed by iodine was recorded. According to Faraday's law of electrolysis, the amount of electricity electrolyzed by iodine is equivalent to the amount of electricity electrolyzed by water, and the moisture content was obtained.
[0139] The test results are shown in Table 1.
[0140] Table 1 Performance test results of sodium ferric sulfate materials in the embodiments and comparative examples
[0141]
[0142] As can be seen from Table 1, Examples 1-9 and Comparative Examples 1-6 show that the sodium iron sulfate products prepared by the present invention have ideal physical properties, the carbon content of each product is 1.57-2.01%, the resistance of each product is below 105.6Ω·cm, the powder wetting angle of each product is above 92°, and the moisture content of the finished products after being exposed to the air for 14 days is below 795ppm, and even after being exposed to the air for 28 days, the moisture content is still below 1550ppm.
[0143] In comparison, the preparation method of sodium iron sulfate used in Comparative Examples 1-6 cannot achieve the technical effects of the preparation method provided by the present invention, including the conductivity of the positive electrode material powder and the waterproof effect of the hydrophobic modification of the material, and its performance is significantly lower than that of the material prepared by the present invention.
[0144] Effect Example 5
[0145] In order to verify the product of the present invention and the use effect of the product, the sodium iron sulfate prepared in each embodiment and comparative example was used to prepare a button-type sodium ion half-cell, and the preparation method was as follows:
[0146] The sodium iron sulfate positive electrode material, Super-P, and PVDF were weighed in a mass ratio of 90:5:5, and the above three materials were dispersed in NMP solvent, mixed evenly, and coated on aluminum foil, and dried at 110°C for 2h to obtain a positive electrode sheet. In the glove box, the components were placed in a CR2032 button battery in the order of spring sheet, gasket, sodium sheet, sodium perchlorate electrolyte, diaphragm, sodium perchlorate electrolyte, and positive electrode sheet, and the sodium ion half-cell was obtained after packaging.
[0147] The obtained button half-cell was tested for cycle performance and rate performance at various gradient rates ranging from 0.1C to 20C at a charge and discharge voltage range of 2.0-4.5V. The specific test steps are as follows:
[0148] The button-type half-cells obtained in the above-mentioned embodiments and comparative examples were simultaneously subjected to charge and discharge tests on a blue electric test system, with the voltage range set to 2.0-4.5V, and the test steps set to 0.1C, 5C, and 20C in sequence. After the half-cell was cycled 10 times at a rate of 20C, the performance at 0.1C was tested, and the cycle was repeated 10 times at each rate. The following table was obtained by calculating the average values of the 6 sets of data collected for each embodiment and comparative example.
[0149] Table 2 Performance test results of batteries made of positive electrode materials in Examples and Comparative Examples
[0150]
[0151]
[0152] The test results are shown in Table 2. It can be obtained from Examples 1-9 and Comparative Examples 1-6 that the positive electrode material obtained by the preparation method provided by the present invention obtains the corresponding sodium battery, which has excellent rate performance and cycle stability. In the rate performance test, the discharge capacity at 0.1C can reach more than 95.0mAh / g, of which the highest discharge capacity can reach 107.1mAh / g; the discharge capacity at 5C can reach more than 65.7mAh / g, of which the highest discharge capacity can reach 76.8mAh / g; the discharge capacity at a current of 20C can still reach more than 50.2mAh / g. When the half-battery is cycled 10 times at a rate of 20C, the current changes from 20C to 0.1C, and its discharge capacity can be restored to more than 92.6mAh / g, and the highest discharge capacity can reach 102.2mAh / g.
[0153] In comparison, the preparation method of the sodium iron sulfate positive electrode material adopted in Comparative Examples 1-6 did not adopt a specific coating type, coating method or coating order, and therefore failed to constitute the special double-layer coating structure involved in the present invention. Therefore, the sodium battery obtained by the positive electrode material obtained by the preparation method provided by the present invention has a rate performance that is significantly better than the corresponding sodium battery prepared in Comparative Documents 1-6.
[0154] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A double-layer coated sodium iron sulfate positive electrode material, characterized in that: The double-layer coated sodium ferric sulfate positive electrode material includes sodium ferric sulfate, a first coating layer on the outer surface of the sodium ferric sulfate, and a second coating layer outside the first coating layer; the first coating layer is formed by carbonization of polysaccharide, and the second coating layer is a conductive polymer.
2. A double-layer coated sodium iron sulfate material according to claim 1, characterized in that: The molecular formula of the sodium ferric sulfate is Na x Fe y (SO4) z , where 1≤x / y≤2, x+2y=2z; The polysaccharide comprises at least one of hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose, ethyl cellulose, hydroxymethyl cellulose, hydroxypropyl cellulose, carboxymethyl cellulose, hydroxypropyl starch ether and cyclodextrin; The conductive polymer comprises at least one of polypyrrole, polyaniline, polyindole, polycarbazole, polythiophene, polyacetylene and polyphenylene vinylene; The carbon content of the double-layer coated sodium iron sulfate positive electrode material is 1.50%-2.10%.
3. A double-layer coated sodium iron sulfate positive electrode material according to claim 1 or 2, characterized in that: The median particle size Dv(50) of the double-layer coated sodium iron sulfate positive electrode material is 0.8-2.5 μm.
4. A double-layer coated sodium iron sulfate positive electrode material according to any one of claims 1 to 3, characterized in that: Satisfies at least one of the following characteristics 1-2: Feature 1: The resistance of the obtained sodium iron sulfate positive electrode material powder is 70-110Ω·cm; Feature 2: The wetting angle of the sodium iron sulfate positive electrode material powder is 90-120°.
5. A method for preparing a double-layer coated sodium iron sulfate positive electrode material according to any one of claims 1 to 4, characterized in that: The following steps are involved: Step 1: mixing a sodium source, an iron source, an antioxidant and the polysaccharide, and then crushing the mixture to obtain a precursor; Step 2: sintering the precursor for the first time and crushing it to obtain a pre-sintered material; Step 3: uniformly mixing the pre-burned material and the conductive polymer to obtain a process material; Step 4: After the process material is sintered for the second time, the double-layer coated sodium iron sulfate positive electrode material is obtained.
6. The method for preparing the double-layer coated sodium iron sulfate positive electrode material according to claim 5, characterized in that: Satisfy at least one of the following characteristics I-III: Feature I: The sodium source includes at least one of anhydrous sodium sulfate and sodium sulfate hydrate; feature II: The iron source includes at least one of anhydrous ferrous sulfate and ferrous sulfate hydrate; Feature III: The antioxidant includes at least one of ascorbic acid, citric acid, oxalic acid, hydrazine and paraformaldehyde.
7. The method for preparing the double-layer coated sodium iron sulfate positive electrode material according to claim 5, characterized in that: Meet at least one of the following characteristics: Feature a: The mass of the polysaccharide is 0.01%-15% of the mass of the sodium source; Feature b: The mass of the antioxidant is 0.01%-10% of the mass of the sodium source; feature c: The mass of the conductive polymer is 0.01%-3.5% of the mass of the pre-sintered material; Feature d: The mass ratio of the sodium source to the iron source is 25%-51%.
8. The method for preparing the double-layer coated sodium iron sulfate positive electrode material according to claim 5, characterized in that: Satisfy at least one of the following characteristics 1-2: Feature 1: The temperature of the first sintering is 280°C-350°C, and the sintering time is 4-24h; Feature 2: The temperature of the second sintering is 150°C-390°C, and the sintering time is 6-12h.
9. A positive electrode sheet, characterized in that: The positive electrode plate comprises a double-layer coated sodium iron sulfate positive electrode material according to any one of claims 1 to 4 or a double-layer coated sodium iron sulfate positive electrode material prepared by the preparation method according to any one of claims 5 to 8.
10. A sodium ion battery, characterized in that: The sodium ion battery comprises the positive electrode sheet according to claim 9.
Citation Information
Cited By
A high-stability doped sodium ferric sulfate positive electrode material and a preparation method thereof
CN119764381B