Halide solid electrolyte prepared from hydrate and preparation method and application thereof
By using silicon-containing hydrates to replace rare earth metal chlorides and adjusting the lithium ion-vacancy ratio, halide solid electrolytes were prepared. This solved the problems of air stability and cost of halide solid electrolytes, improved conductivity and energy density, and enhanced compatibility with lithium metal.
Patent Information
- Application Number
- CN202411017903.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing halide solid electrolytes have poor stability in air, high cost, and poor compatibility with lithium metal, which limits the energy density and large-scale production of all-solid-state batteries.
By using silicon-containing hydrates instead of rare earth metal chlorides as raw materials, and by introducing tetravalent silicon ions to regulate the ratio of lithium ions to vacancies, ion transport channels are increased, reduction potential is reduced, and humid air stability is improved, forming a moisture-resistant intermediate to prepare a halide solid electrolyte.
It improves the ionic conductivity, energy density, and humid air stability of halide solid electrolytes, reduces production costs, enhances compatibility with lithium metal, expands the electrochemical window, and reduces interfacial side reactions.
Smart Images

Figure CN118970151A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to a halide solid electrolyte prepared from hydrates, a preparation method thereof and applications thereof. Background Art
[0002] All-solid-state batteries use solid electrolytes instead of traditional liquid electrolytes, which have higher safety and stability. Due to its high energy density and safety, it has great development prospects in the field of large-scale energy storage. At present, solid electrolytes mainly include sulfide solid electrolytes, oxide electrolytes, and chloride solid electrolytes. Oxyhalide solid electrolytes are a type of halide solid electrolyte. Oxyhalide solid electrolytes are a type of solid electrolyte with high room temperature ionic conductivity, excellent chemical / electrochemical stability, and high positive electrode stability. Therefore, they have become the key to the practical application of all-solid-state batteries and have received widespread attention.
[0003] Since silicon resources are abundant, cheap, and evenly distributed in the earth's crust, they can replace expensive rare earth metal chlorides and reduce costs, making all-solid-state batteries have broad market application prospects in the field of large-scale energy storage. Hydrates can replace oxides, hydroxides, peroxides, etc. as oxygen sources to introduce oxygen atoms. Using silicon-containing hydrates as raw materials for synthesizing oxyhalide solid electrolytes has the advantages of low price, environmental protection, and easy recycling.
[0004] Similar technical solutions: Publication No. CN116960441A reported an antiperovskite-type halide solid electrolyte. Due to the use of Zr element, it solved the high production cost caused by the use of expensive rare earth element La in halide solid electrolyte materials and the high temperature and energy consumption during LLZO synthesis. However, this antiperovskite-type halide solid electrolyte has a high reduction potential and poor compatibility with metal negative electrodes; Publication No. CN116683018A reported a halide solid electrolyte with good structural stability and high ionic conductivity at room temperature or high temperature, but it needs to use organic solvents in the synthesis process, the preparation process is cumbersome, and it cannot be safe, environmentally friendly and non-toxic.
[0005] Disadvantages of existing technology:
[0006] First, the halide solid electrolytes reported so far have poor wet air stability and are easily deliquescent in the air. They need to be synthesized under the protection of an inert gas, argon, and are difficult to produce on a large scale.
[0007] Secondly, the raw materials of common halide electrolytes contain expensive rare earth metal elements, which makes the raw material cost high and hinders the commercial application of all-solid-state batteries.
[0008] Finally, the halide solid electrolyte has a high reduction potential, poor compatibility with lithium metal, poor interface stability, and interfacial side reactions that lead to increased resistance. It is necessary to construct an interfacial buffer layer or a lithium-indium / sodium-tin alloy negative electrode, which reduces the energy density of the all-solid-state battery and increases the process steps, further increasing the cost. Summary of the invention
[0009] The technical problem to be solved by the present invention is: the air stability and energy density of the solid electrolyte of the current all-solid-state secondary battery need to be improved. The present invention provides a halide solid electrolyte prepared by hydrate and its preparation method and application to solve the above problems. The silicon-containing hydrate used can be used as an oxygen source to introduce oxygen atoms and silicon ions to regulate the ratio of lithium ions and vacancies, provide lithium ion or sodium ion transmission channels, and improve the ionic conductivity of the solid electrolyte.
[0010] The present invention is achieved through the following technical solutions:
[0011] A halide solid electrolyte prepared from hydrate, the general chemical formula is:
[0012] A x Si y B z X m O n ;in:
[0013] A is lithium or sodium;
[0014] B is one or more of the third sub-group metal elements, the fourth sub-group metal elements, the fifth sub-group metal elements, and the thirteenth main group metal elements;
[0015] X is a halogen element;
[0016] 1≤x≤20, 1≤y≤20, 1≤z≤30, 1≤m≤50, 1≤n≤20;
[0017] A x Si y B z X m O n The preparation raw materials include: halide of A, halide of B and silicon-containing hydrate.
[0018] The present invention uses silicon-containing hydrates to replace expensive rare earth metal chlorides (preferably, the molar ratio of rare earth metal chlorides to silicon-containing hydrates is set to 0.1-0.9). Silicon-containing hydrates have high abundance in the earth's crust and low raw material costs, thereby reducing the amount of rare earth metal chloride raw materials and improving ionic conductivity, thereby reducing costs and facilitating the commercial application of solid-state batteries.
[0019] The present invention increases the number of vacancies by anode substitution to increase the ion transmission channel. B is +3 valence, Si is +4 valence, and the introduction of Si 4+ The number of vacancies will increase. 2- Replace Cl - The concentration of lithium\sodium ions will increase, and the concentration of ions that can be transported in the solid electrolyte will increase, which will also increase the ionic conductivity. The lithium ion concentration and vacancy content can be regulated by controlling the proportion of introduced O and Si, and the ratio of lithium ion concentration to vacancy content is between 0.1-0.9. Therefore, the present invention introduces high-valent silicon ions, adjusts the concentration of lithium ions and vacancies, generates more vacancies and disorder to provide additional transmission pathways for lithium ion migration, reduces the energy barrier for lithium ion migration, helps lithium ions to diffuse rapidly, and improves ionic conductivity, thereby improving the capacity retention rate of all-solid-state batteries.
[0020] The present invention can reduce the reduction potential of the halide solid electrolyte by introducing tetravalent silicon ions, so that it has high oxidation stability and low reduction stability, expands its electrochemical window, reduces interface side reactions, improves the coulombic efficiency of the all-solid-state battery, and improves the energy density.
[0021] The present invention aims to regulate the crystal structure by introducing tetravalent silicon ions, so that the crystal structure can form a moisture-resistant intermediate in wet air, which is not easy to decompose, thereby improving its wet air stability.
[0022] Preferably, the molar ratio of the halide of A, the halide of B and the silicon-containing hydrate is 10 mol%-70 mol%, 30 mol%-85 mol%, 1 mol%-40 mol%.
[0023] Further optionally, 50 mol% of the halide of A, 30 mol% of the halide of B, and 20 mol% of the silicon-containing hydrate, wherein the halogen element is Cl;
[0024] and / or, the third sub-main group element is La or Sc; and / or, the fourth sub-main group element is Zr or Hf; and / or, the fifth sub-main group element is Ta or Nb; and / or, the thirteenth main group element is Al or In;
[0025] And / or, the silicon-containing hydrate is sodium metasilicate hydrate
[0026] Further optionally,
[0027] The chloride of A is the chloride of A;
[0028] And / or, the halide of B is chloride of B;
[0029] And / or, the silicon-containing hydrate is sodium metasilicate nonahydrate.
[0030] Further optionally, the preparation of the raw materials comprises, by mole percentage:
[0031] 10 mol% - 70 mol% of halide A, 30 mol% - 85 mol% of halide B, 1 mol% - 40 mol% of silicon-containing hydrate.
[0032] Further optionally, the preparation raw material comprises, by mole percentage, 50 mol % of halide A, 30 mol % of halide B, and 20 mol % of silicon-containing hydrate.
[0033] A method for preparing a halide solid electrolyte prepared from a hydrate, for preparing the above-mentioned halide solid electrolyte prepared from a hydrate, comprising the steps of:
[0034] After all the raw materials are mixed, they are subjected to ball milling, tablet pressing and annealing treatment to obtain a halide solid electrolyte.
[0035] More specifically, the steps include:
[0036] a) Weighing materials: Weigh and mix the three raw materials according to the molar ratio and put them into a ball mill;
[0037] b) Ball milling: After the ball milling jar is placed in the ball mill, it is ball milled and fully mixed and reacted;
[0038] c) Annealing: the ball-milled mixture is pressed into tablets through a tabletting mold, and then placed in a high-temperature resistant glass bottle for high-temperature sintering;
[0039] d) Grinding: Grinding the sintered sheet into powder using a mortar to obtain a halide solid electrolyte.
[0040] Further optionally, in the ball milling process: the rotation speed is 200 rpm-700 rpm, the ball-to-material ratio is 20:1-80:1, and the ball milling time is 0.5h-50h;
[0041] More preferably, the rotation speed is 500 rpm, and / or the ball-to-material ratio is 5:1-40:1, and / or the ball milling time is 1 h-30 h.
[0042] And / or, in the annealing treatment: the sintering temperature is 200° C.-700° C., and the annealing time is 1 h-20 h.
[0043] More preferably, the sintering temperature is 200° C.-400° C., and / or the annealing time is 1 h-14 h.
[0044] More preferably, in the present invention, the ball milling speed is 500 rpm, the ball-to-material ratio is 40:1, the ball milling time is 3 h, the annealing sintering temperature is 260° C., and the sintering time is 3 h.
[0045] The invention discloses an application of a halide solid electrolyte prepared from hydrate in a battery.
[0046] A battery comprises the above-mentioned halide solid electrolyte prepared from hydrate, or an electrolyte prepared by the above-mentioned method for preparing a halide solid electrolyte prepared from hydrate.
[0047] The present invention has the following advantages and beneficial effects:
[0048] 1. The present invention uses silicon-containing hydrates to replace the expensive rare earth metal chlorides, thereby reducing the amount of rare earth metal chloride raw materials and improving ionic conductivity, thereby reducing costs and facilitating the commercial application of solid-state batteries.
[0049] 2. The present invention introduces high-valent silicon ions, adjusts the concentration of lithium ions and vacancies, generates more vacancies and disorder to provide additional transmission pathways for lithium ion migration, reduces the energy barrier for lithium ion migration, helps lithium ions to diffuse rapidly, improves ion conductivity, and thus improves the capacity retention rate of all-solid-state batteries.
[0050] 3. The introduction of tetravalent silicon ions in the present invention can reduce the reduction potential of the halide solid electrolyte, make it have high oxidation stability and low reduction stability, expand its electrochemical window, reduce interface side reactions, and improve the coulombic efficiency of the all-solid-state battery; improve the compatibility with metallic lithium / sodium, can directly contact with the metal negative electrode, and improve the energy density.
[0051] 4. The present invention introduces tetravalent silicon ions to regulate the crystal structure, so that it can form a moisture-resistant intermediate in wet air, which is not easy to decompose, thereby improving its wet air stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] The drawings described herein are used to provide a further understanding of the embodiments of the present invention, constitute a part of this application, and do not constitute a limitation of the embodiments of the present invention. In the drawings:
[0053] Figure 1 This is the XRD of the oxyhalide solid electrolyte prepared in Example 1. DETAILED DESCRIPTION
[0054] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments and drawings. The exemplary embodiments of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.
[0055] Performance Testing
[0056] 1. Ionic conductivity: Place 100mg-150mg electrolyte in a battery mold with a diameter of 10mm, apply 500Mpa pressure for cold pressing, and measure its impedance in an electrochemical workstation. The ionic conductivity calculation formula is:
[0057] σ=l / (A·R)
[0058] Where l is the thickness of the electrolyte and A is the area, which is approximately 0.785 cm 2 , R is the impedance.
[0059] 2. Air stability: 0.5 g of solid electrolyte powder was placed in a chamber filled with N2 with the same humidity as the air. 2 The moisture resistance test was conducted by exposing the sample to a vacuum desiccator for 6 hours. The ion conductance before and after the test was measured, and the decrease in ion conductance before and after the reaction was calculated.
[0060] 3. Energy density: the product of the discharge platform voltage and specific capacity.
[0061] 4. Cycle stability: Calculate the capacity retention rate after 200 cycles.
[0062] Example 1
[0063] This embodiment provides a halide oxide solid electrolyte Na prepared from a hydrate. 6 SiAl 12 O 12 Cl 24 , the specific preparation method is as follows:
[0064] Step 1, weigh the ingredients:
[0065] Three raw materials: sodium chloride, aluminum chloride, and sodium metasilicate nonahydrate are weighed and mixed according to different molar ratios and then put into a ball mill;
[0066] Step 2, ball milling:
[0067] After placing the ball mill jar into the ball mill, set the ball mill speed to 500 rpm, the ball-to-material ratio to 40:1, and the ball milling time to 3 h to fully mix and react;
[0068] Step 3, annealing:
[0069] The ball-milled mixture was pressed into tablets through a tabletting mold, and then placed in a high-temperature resistant glass bottle and sintered at high temperature for 3 hours;
[0070] Step 4, Grinding:
[0071] The sintered sheet is ground into powder with a mortar to obtain a halide solid electrolyte; an all-solid-state battery is assembled using the layered metal oxide P2 as the positive electrode, the prepared halide solid electrolyte as the electrolyte, and sodium metal as the negative electrode.
[0072] Embodiment 2-4
[0073] Examples 2-4 all provide a halide oxide solid electrolyte prepared from a hydrate, wherein the electrolytes are: Na 6 SiAl 12 O 12 Cl 24 、Na 9 SiAl 11 O 12 Cl 24 、Na 12 SiAl 10 O 12 Cl 24 、Na 5 SiAl 13 O 12 Cl 24 The specific preparation method is as follows:
[0074] The steps for preparing the oxyhalide solid electrolyte provided in Examples 2-4 are the same as those in Example 1, except that the raw material ratios are different. For details, see Table 1:
[0075] Table 1. Performance comparison of electrolytes prepared using different raw material ratios in Examples 1-4
[0076]
[0077] It can be seen from Table 1 that when the molar ratio of raw materials is 5:3:2, the ion conductivity, capacity retention rate, energy density of the halide oxide solid electrolyte are higher and the air stability is better.
[0078] Embodiment 5-7
[0079] Examples 5-7 all provide a halide oxide solid electrolyte Na prepared from a hydrate. 6 SiAl 12 O 12 Cl 24 The specific preparation method is as follows:
[0080] The steps for preparing the oxyhalide solid electrolyte provided in Examples 5-7 are the same as those in Example 1, except that the ball milling speed is different. For details, see Table 2:
[0081] Table 2. Comparison of the performance of oxyhalide solid electrolytes prepared by different ball milling speeds in Example 1 and Examples 5-7
[0082]
[0083] It can be seen from Table 2 that when the ball milling speed is 500 rpm, the ionic conductivity, capacity retention rate, energy density and air stability of the oxyhalide solid electrolyte are higher.
[0084] Examples 8-10
[0085] Examples 8-10 all provide a halide oxide solid electrolyte Na prepared from a hydrate. 6 SiAl 12 O 12 Cl 24 The specific preparation method is as follows:
[0086] The steps for preparing the oxyhalide solid electrolyte provided in Examples 8-10 are the same as those in Example 1, except for the different ball milling times. For details, see Table 3:
[0087] Table 3. Performance comparison of oxyhalide solid electrolytes prepared by different ball milling times in Example 1 and Examples 8-9
[0088]
[0089] It can be seen from Table 3 that when the ball milling time is 3 h, the ionic conductivity, capacity retention rate, energy density and air stability of the oxyhalide solid electrolyte are higher.
[0090] Examples 11-13
[0091] Examples 11-13 all provide a halide oxide solid electrolyte Na prepared from a hydrate. 6 SiAl 12 O 12 Cl 24 The specific preparation method is as follows:
[0092] The steps for preparing the oxyhalide solid electrolyte provided in Examples 11-13 are the same as those in Example 1, except that the ratio of pellet to material is different. For details, see Table 4:
[0093] Table 4. Performance comparison of oxyhalide solid electrolytes prepared using different pellet to material ratios in Example 1 and Examples 11-13
[0094]
[0095] It can be seen from Table 4 that when the ball-to-material ratio is 40:1, the ion conductivity, capacity retention rate, energy density of the halide oxide solid electrolyte are higher and the air stability is better.
[0096] Examples 14-16
[0097] Examples 14-16 all provide a halide oxide solid electrolyte Na prepared from a hydrate. 6 SiAl 12 O 12 Cl 24 The specific preparation method is as follows:
[0098] The steps for preparing the oxyhalide solid electrolyte provided in Examples 14-16 are the same as those in Example 1, except for the sintering temperature. For details, see Table 5:
[0099] Table 5. Performance comparison of oxyhalide solid electrolytes prepared at different sintering temperatures in Example 1 and Examples 14-16
[0100]
[0101]
[0102] It can be seen from Table 5 that when the sintering temperature is 260°C, the ionic conductivity, capacity retention rate, energy density of the halide oxide solid electrolyte are higher and the air stability is better.
[0103] Examples 17-19
[0104] Examples 17-19 all provide a halide oxide solid electrolyte Na prepared from a hydrate. 6 SiAl 12 O 12 Cl 24 The specific preparation method is as follows:
[0105] The steps for preparing the oxyhalide solid electrolyte provided in Examples 17-19 are the same as those in Example 1, except for the sintering time. For details, see Table 6:
[0106] Table 6. Comparison of the performance of oxyhalide solid electrolytes prepared by different sintering times in Example 1 and Examples 17-19
[0107]
[0108] It can be seen from Table 6 that when the sintering time is 3 h, the ionic conductivity, capacity retention rate, energy density and air stability of the oxyhalide solid electrolyte are higher.
[0109] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A halide solid electrolyte prepared from a hydrate, It is characterized in that The general chemical formula is: A x Si y B z X m O n ;in: A is lithium or sodium; B is one or more of the third sub-group metal elements, the fourth sub-group metal elements, the fifth sub-group metal elements, and the thirteenth main group metal elements; X is a halogen element; 1≤x≤20, 1≤y≤20, 1≤z≤30, 1≤m≤50, 1≤n≤20; A x Si y B z X m O n The preparation raw materials include: halide of A, halide of B and silicon-containing hydrate.
2. A halide solid electrolyte prepared from a hydrate according to claim 1, It is characterized in that The halogen element is Cl; and / or, the third sub-main group element is La or Sc; and / or, the fourth sub-main group element is Zr or Hf; and / or, the fifth sub-main group element is Ta or Nb; and / or, the thirteenth main group element is Al or In; And / or, the silicon-containing hydrate is sodium metasilicate hydrate.
3. A halide solid electrolyte prepared from a hydrate according to claim 2, It is characterized in that The chloride of A is the chloride of A; And / or, the halide of B is chloride of B; And / or, the silicon-containing hydrate is sodium metasilicate nonahydrate.
4. A halide solid electrolyte prepared from a hydrate according to any one of claims 1 to 3, It is characterized in that The raw materials for preparation include, by mole percentage: 10 mol% - 70 mol% of halide A, 30 mol% - 85 mol% of halide B, 1 mol% - 40 mol% of silicon-containing hydrate.
5. A halide solid electrolyte prepared from a hydrate according to claim 4, It is characterized in that The raw materials for preparation include, by mole percentage: 50 mol% A halide, 30 mol% B halide, 20 mol% silicon-containing hydrate.
6. A method for preparing a halide solid electrolyte prepared from a hydrate, It is characterized in that A method for preparing a halide solid electrolyte prepared from a hydrate according to any one of claims 1 to 5, comprising the steps of: After all the raw materials are mixed, they are subjected to ball milling, tablet pressing and annealing treatment to obtain a halide solid electrolyte.
7. A method for preparing a halide solid electrolyte prepared from a hydrate according to claim 6, It is characterized in that During ball milling: the rotation speed is 200rpm-700rpm, the ball-to-material ratio is 20:1-80:1, and the ball milling time is 0.5h-50h; And / or, in the annealing treatment: the sintering temperature is 200° C.-700° C., and the annealing time is 1 h-20 h.
8. Use of an electrolyte prepared by the halide solid electrolyte prepared from a hydrate as claimed in any one of claims 1 to 5 or the method for preparing a halide solid electrolyte prepared from a hydrate as claimed in claim 6 or 7 in a battery.
9. A battery, It is characterized in that An electrolyte comprising a halide solid electrolyte prepared from a hydrate as described in any one of claims 1 to 5, or an electrolyte prepared by the preparation method of a halide solid electrolyte prepared from a hydrate as described in claim 6 or 7.
Citation Information
Patent Citations
Solid electrolyte, solid electrolyte layer, and solid electrolyte battery
CN114207895A
Aluminosilicate lithium ion solid electrolyte and preparation method thereof
CN115411353A
Solid electrolyte material and preparation method and application thereof
CN117438641A
Solid electrolyte and method of manufacturing the same
JP2003238236A