Ceramic wiring member
By using tungsten or molybdenum as the main component in the conductive part of the ceramic wiring member, and adding nickel, cobalt or iron, combining alloy and glass phase, the problem of insufficient resistance and adhesion strength of the conductive part is solved, and low resistance and high density are achieved A comprehensive ceramic wiring member.
Patent Information
- Application Number
- CN202380031262.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-31
- Publication Date
- 2024-11-15
AI Technical Summary
The conventional ceramic wiring members have shortcomings in reducing the resistance of the conductive part and increasing the adhesion strength between the main body part of the ceramic and the conductive part, especially the resistance of the conductive part cannot be sufficiently reduced and the adhesion strength is insufficient.
The conductive part containing tungsten (W) or molybdenum (Mo) as the main component, and nickel (Ni), cobalt (Co) or iron (Fe) is added as the second metal component to the conductive part, and the alloy and glass phase are passed. Combined, the area ratio of the conductive phase and the glass phase is controlled to reduce the intrusion of the glass phase and to promote the sintering of the metal powder.
The resistance of the conductive part is effectively reduced, and the adhesion strength between the main body part of the ceramic is improved, thereby achieving low resistance and high adhesion of the conductive part.
Smart Images

Figure CN118975411A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a ceramic wiring member. Background Art
[0002] A ceramic wiring component is known, comprising: a main body portion made of ceramic having a plate-like portion; and a conductive portion arranged in contact with the plate-like portion. Such a ceramic wiring component is used as a component for holding electronic components. The conductive portion constitutes a part of a current path for current to flow into or out of an electronic component (for example, refer to Japanese Patent Gazette No. 2020-92234 (Patent Document 1)). In such a ceramic wiring component, it is important to reduce the resistance of the conductive portion. From this point of view, the use of a metal with low resistivity as a metal constituting the conductive portion has been studied. In addition, as a raw material for the metal constituting the conductive portion, the use of a raw material powder with a small particle size has been studied. Prior art literature Patent Literature
[0003] Patent Document 1: Japanese Patent Application Publication No. 2020-92234 Summary of the invention Technical problem to be solved by the invention
[0004] However, even when adopting the countermeasures of adopting the metal with low resistivity and adopting raw material powder with small particle size, the resistance of the conductive part may not be sufficiently reduced. In addition, even if the resistance is reduced, the adhesion strength between the conductive part and the main body made of ceramic may not be sufficient.
[0005] One of the objects of the present disclosure is to provide a ceramic wiring member capable of reducing the resistance of a conductive portion and obtaining sufficient adhesion strength between the conductive portion and a ceramic main body portion. Solutions for solving technical problems
[0006] The ceramic wiring component according to the present disclosure comprises a main body portion made of ceramic and a conductive portion arranged in contact with the main body portion. The composition of the conductive portion includes a ceramic component, a first metal component as a main component, and a second metal component whose total is greater than 0.1% and less than 10% relative to the first metal component, the first metal component is at least any one of W (tungsten) and Mo (molybdenum), and the second metal component is selected from at least one of Ni (nickel), Co (cobalt) and Fe (iron). The structure of the conductive portion includes: a conductive phase, which includes an alloy of the first metal component and the second metal component; and a glass phase, which is dispersed in the conductive phase, and the area ratio in the cross section of the conductive portion is greater than 3% and less than 20%, and includes the above-mentioned ceramic component. Here, "%" refers to the mass ratio (mass %), and the same applies to subsequent descriptions unless a different definition is explicitly stated. Effects of the Invention
[0007] According to the ceramic wiring member, it is possible to reduce the electrical resistance of the conductive portion and obtain sufficient adhesion strength between the conductive portion and the ceramic main body portion. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] Figure 1 It is a schematic cross-sectional view showing the structure of a ceramic wiring member. Figure 2 It is a schematic cross-sectional view showing the structure near the interface between the main body portion (plate-shaped portion) and the conductive portion. Figure 3 This is a flowchart schematically showing a method for manufacturing a ceramic wiring member. Figure 4 This is a schematic cross-sectional view showing the structure of a ceramic wiring member in the second embodiment. Figure 5 This is a schematic cross-sectional view showing the structure of a ceramic wiring member in the third embodiment. Figure 6 This is a graph showing the relationship between the amount of the second metal component added and the resistivity. DETAILED DESCRIPTION
[0009] [Overview of Embodiments] First, the embodiments of the present disclosure are listed and described. The ceramic wiring component of the present disclosure comprises a main body portion made of ceramic and a conductive portion arranged in contact with the main body portion. The composition of the conductive portion includes: a first metal component as a main component, which is at least one of W and Mo; and a second metal component, which is 0.1% or more and 10% or less in total relative to the first metal component, and is selected from at least one of Ni, Co and Fe. The structure of the conductive portion includes a conductive phase, and the conductive phase includes an alloy of the first metal component and the second metal component.
[0010] The present inventors have studied the reason why the resistance of the conductive portion cannot be sufficiently reduced even when measures such as using the metal with low resistivity and using raw material powder with a small particle size are taken. As a result, the inventors have obtained the following findings.
[0011] The ceramic wiring components as described above are generally manufactured by preparing a raw sheet of ceramics constituting the main body, printing a paste containing metal powder constituting the conductive part on the raw sheet, and firing it. At this time, according to the research of the inventors, during the sintering process of the metal powder contained in the above-mentioned paste, the molten glass phase composed of the ceramic component invades the gap of the metal powder due to the capillary phenomenon. The glass phase hinders the sintering of the metal powder and becomes the cause of the increase in the resistance of the conductive part. In addition, the glass phase itself that invades the conductive part also becomes the cause of the increase in the resistance of the conductive part.
[0012] In the ceramic wiring component disclosed in the present invention, the composition of the conductive part includes a second metal component selected from at least one of Ni, Co and Fe, which is 0.1% or more and 10% or less relative to the first metal component as the main component, and the first metal component is at least any one of W and Mo. According to the research of the inventors, by adding the above-mentioned second metal component, the intrusion of the glass phase into the conductive part can be reduced. In addition, by adding the above-mentioned second metal component, the sintering of the metal powder can be promoted. As a result, the resistance of the conductive part is reduced. As described above, according to the ceramic wiring component disclosed in the present invention, the resistance of the conductive part can be reduced. In addition, by making the addition amount of the second metal component relative to the first metal component an appropriate ratio, the adhesion strength between the ceramic main body and the conductive part can also be ensured. Here, the first metal component as the main component of the conductive part can account for more than 80% by mass of the entire conductive part. In addition to the first metal component and the second metal component, the conductive part may also include, for example, less than 0.05% by mass of Au, Ag, etc. of the entire conductive part. The proportion of the conductive phase in the structure of the conductive part can be more than 80% in terms of area ratio. The average particle size of the first metal component before sintering (raw material powder) may be 0.1 μm to 5.5 μm. The average particle size of the second metal component before sintering (raw material powder) may be 0.1 μm to 10 μm.
[0013] In the above-mentioned ceramic wiring component, the composition of the conductive part may also contain a ceramic component. The structure of the conductive part may also contain a glass phase, which is dispersed in the conductive phase and contains a ceramic component in an area ratio of 3% to 20%, preferably 8% to 20%, in the cross section of the conductive part. It should be noted that in the present application, the glass phase refers to: in addition to the glass component contained in the main body, it may also contain a certain amount of crystals of the main ceramic component (aluminum oxide) contained in the main body and the metal component in the conductive part. In addition, the glass phase may also contain a glass component that is not contained in the main body.
[0014] From the viewpoint of reducing the difference in linear expansion coefficient between the conductive part and the main body, the glass phase can be dispersed in the conductive phase. In this case, by setting the proportion of the glass phase to 20% or less in terms of the area ratio in the cross section of the conductive part, the increase in the resistance of the conductive part can be suppressed. By setting the proportion of the glass phase to 3% or more, and further to 8% or more, the adhesion between the conductive part and the main body can be improved.
[0015] In the ceramic wiring member, the average particle size of the metal particles constituting the conductive phase may be 1.2 μm or more and 5.5 μm or less. Thus, a ceramic wiring member having good resistance of the conductive portion and good adhesion between the conductive portion and the main body can be obtained. The average particle size of the metal particles constituting the conductive phase may be 1.2 μm or more and 1.6 μm or less.
[0016] In the above-mentioned ceramic wiring member, it is preferable that the structure of the conductive portion does not include an intermetallic compound phase including an intermetallic compound of the first metal component and the second metal component.
[0017] The intermetallic compound of the first metal component and the second metal component has lower electrical conductivity than the alloy of the first metal component and the second metal component. Therefore, by not including the intermetallic compound phase, an increase in the resistance of the conductive portion can be suppressed.
[0018] In the above-mentioned ceramic wiring member, the main body may also have a plate-shaped portion. The conductive portion may also include: a first portion, which contacts the first main surface of the plate-shaped portion; and a second portion, which contacts the second main surface, and the second main surface is located on the side opposite to the first main surface in the thickness direction of the plate-shaped portion. In this way, the first main surface side and the second main surface side of the plate-shaped portion are electrically connected through the conductive portion with reduced resistance, thereby obtaining a high-performance ceramic wiring member that can cope with power saving and high-speed communication.
[0019] [Specific example of embodiment] Next, specific embodiments of the ceramic wiring member of the present disclosure will be described with reference to the drawings. In the following drawings, the same or corresponding parts are denoted by the same reference numerals, and their description will not be repeated.
[0020] (Implementation Method 1) Figure 1 2 is a schematic cross-sectional view showing the structure of a ceramic wiring member in one embodiment of the present disclosure. Figure 1 The ceramic wiring member 1 of the present embodiment includes a conductive portion 20 and a main body portion 10 made of ceramic. The ceramic constituting the main body portion 10 is not particularly limited, and for example, alumina can be used. In addition, the ceramic constituting the main body portion 10 may also contain a glass component as a sintering aid, and the glass component is selected from at least one of an oxide containing Si, an oxide containing Ca, an oxide containing Mg, an oxide containing Mn, and an oxide containing Ba. The main body portion 10 includes: a bottom wall portion 11 having a plate-like shape as a first plate-like portion; and a side wall portion 12 having a plate-like shape as a second plate-like portion. The bottom wall portion 11 has a flat plate shape. The bottom wall portion 11 includes a first main surface 11A and a second main surface 11B located on the opposite side of the first main surface 11A in the thickness direction. The planar shape of the bottom wall portion 11 (the shape observed in a direction perpendicular to the first main surface 11A) is, for example, a rectangle.
[0021] The side wall portion 12 has a plate-like shape rising from the outer edge of the first main surface 11A of the bottom wall portion 11. More specifically, it has a shape formed by connecting four flat plates corresponding to the respective sides of the outer edge of the first main surface 11A of the bottom wall portion 11 having a rectangular planar shape. When viewed in a direction perpendicular to the first main surface 11A, the side wall portion 12 may be configured, for example, to surround the space on the first main surface 11A, i.e., the cavity 10A. The side wall portion 12 includes: a planar first end surface 12A; and a planar end surface, i.e., a second end surface 12B, on the side opposite to the first end surface 12A in the thickness direction of the bottom wall portion 11. The side wall portion 12 is connected to the first main surface 11A of the bottom wall portion 11 at the second end surface 12B. The first end surface 12A is located on a single plane throughout the entire area. As a result, the cavity 10A can be closed by placing a flat cover member on the first end surface 12A. An electronic component such as a crystal oscillator which requires airtightness can be housed in the cavity 10A. Such a ceramic wiring member 1 is used as a ceramic package.
[0022] In the present embodiment, the ceramic wiring member 1 includes a pair of conductive parts 20. Each conductive part 20 includes: an internal terminal 21 as a first part arranged in contact with the first main surface 11A; an external terminal 25 as a second part arranged in contact with the second main surface 11B; and an internal wiring 23 arranged inside the bottom wall portion 11. Each conductive part 20 also includes: a first connecting part 22 connecting the internal terminal 21 and the internal wiring 23; and a second connecting part 24 connecting the internal wiring 23 and the external terminal 25. The internal wiring 23, the first connecting part 22, and the second connecting part 24 are the third part that connects the internal terminal 21 as the first part and the external terminal 25 as the second part. The internal terminal 21, the external terminal 25, the internal wiring 23, the first connecting part 22, and the second connecting part 24 are all parts of the conductive part 20 arranged in contact with the bottom wall portion 11 as the first plate-shaped portion. It should be noted that as a modified example of the first connecting part 22 and the second connecting part 24, for example, a castellated structure may be provided on the side of the bottom wall portion 11. ( Castellation ) , a conductive portion is provided on the surface of the castellated structure.
[0023] The composition of at least one of the internal terminal 21, the external terminal 25, the internal wiring 23, the first connection part 22 and the second connection part 24 constituting the conductive part 20, preferably all of them includes: a first metal component as a main component, the first metal component is at least one of W and Mo; and a second metal component, the second metal component is 0.1% or more and 10% or less relative to the first metal component, and is selected from at least one of Ni, Co and Fe. In addition, the structure of at least one of the internal terminal 21, the external terminal 25, the internal wiring 23, the first connection part 22 and the second connection part 24 constituting the conductive part 20, preferably all of them includes a conductive phase, and the conductive phase includes an alloy of the first metal component and the second metal component. It should be noted that the alloy here means: in addition to containing a solid solution, it also includes a mixture, the solid solution contains the first metal component and the second metal component, and the mixture is a mixture of the first metal component and the second metal component that are not dissolved.
[0024] In the ceramic wiring member 1 of the present embodiment, by adding the second metal component as the metal component of the conductive portion 20, the intrusion of the glass phase into the conductive portion 20 can be reduced. In addition, by adding the second metal component, the sintering of the metal powder constituting the conductive portion 20 can be promoted. As a result, the ceramic wiring member 1 becomes a ceramic wiring member in which the resistance of the conductive portion 20 is reduced.
[0025] Figure 2 2 is a schematic cross-sectional view showing the structure near the interface between the main body 10 and the conductive part 20. Figure 2 , the conductive part 20 is arranged in contact with the main body 10. The conductive part 20 may contain a ceramic component in addition to the above-mentioned metal component. Furthermore, the structure of the conductive part 20 may contain a glass phase 32 in addition to the conductive phase 31, and the glass phase 32 is dispersed in the conductive phase 31, and contains the above-mentioned ceramic component in an area ratio of 3% or more and 20% or less in the cross section in the thickness direction of the bottom wall part 11 as the first plate-shaped part. By making the area ratio of the glass phase less than 20%, the increase in the resistance of the conductive part 20 can be suppressed, and by making the area ratio of the glass phase more than 3%, preferably more than 8%, the difference in the linear expansion coefficient between the conductive part 20 and the main body 10 can be reduced. The glass phase 32 in the conductive part 20 basically invades from the main body by capillary phenomenon during sintering, and the glass phase 32 may also contain glass components that are not contained in the main body 10. From the viewpoint of electrical resistance and strength, the area ratio of voids 31A not filled with glass phase 32 in the cross section of conductive portion 20 is preferably 5% or less, and more preferably 1% or less.
[0026] In addition, it is preferred that the structure of the conductive portion does not include an intermetallic compound phase, which includes an intermetallic compound of the first metal component and the second metal component. The intermetallic compound phase becomes a cause of reduced conductivity, so it is preferably reduced as much as possible, and more preferably not included. Here, the state of not including the intermetallic compound phase means that when the conductive portion 20 is analyzed by X-ray diffraction, the peak corresponding to the crystallization of the intermetallic compound phase is below the noise level.
[0027] In addition, in the structure of the conductive part 20, the average particle size of the metal particles constituting the conductive phase is preferably greater than 1.2 μm and less than 5.5 μm. If it is less than 1.2 μm, the resistance of the conductive part 20 becomes high. On the other hand, if it exceeds 5.5 μm, the adhesion strength of the conductive part 20 relative to the main body is reduced. It should be noted that the average particle size of the conductive phase can be adjusted by changing the firing temperature, firing time, and the particle size of the metal powder (raw material powder) of the first and second metal components. In addition, it can also be adjusted by increasing or decreasing the proportion of the glass phase 32 contained in the conductive part 20.
[0028] Next, an example of a method for manufacturing ceramic wiring member 1 in the present embodiment will be described. Figure 3 1 is a flowchart schematically showing a method for manufacturing a ceramic wiring member. Figure 3 In the manufacturing method of the ceramic wiring component 1 of the present embodiment, first, as step S10, a green sheet preparation step is implemented. In this step S10, a green sheet to become the main body 10 is prepared. Specifically, a ceramic powder constituting the main body 10, such as alumina powder, sintering aid powder, and a resin and solvent that do not constitute the main body 10 (i.e., disappear during firing) are mixed using a ball mill to obtain a slurry. The slurry is processed into a green sheet by a scraper method. In this way, a green sheet to become the main body 10 is obtained. Here, refer to Figure 1 As the green sheet to be the bottom wall portion 11, a plurality of green sheets having a rectangular planar shape are prepared. In addition, a plurality of green sheets to be the side wall portion 12 are also prepared. As the green sheet to be the side wall portion 12, a ring-shaped green sheet having a rectangular planar shape and having a portion (central portion) corresponding to the cavity 10A removed is prepared.
[0029] Next, as step S20, a conductive portion printing step is performed. In this step S20, a paste to be the conductive portion 20 is printed on the raw sheet prepared in step S10. Specifically, first, a first metal component, a second metal component, and additives, resins, solvents, etc. are combined, and ceramic powder is added as needed to mix, thereby making a paste, wherein the first metal component is a main component and is at least one of W and Mo, and the second metal component is selected from at least one of Ni, Co and Fe. The ceramic powder may be the same as the ceramic powder constituting the main body 10, or may be different.
[0030] For example, the paste is printed on the green sheet prepared in step S10 by screen printing. Figure 1 As the green sheet to be the bottom wall portion 11, a green sheet with the above-mentioned paste printed on the region corresponding to the external terminal 25, a green sheet with the above-mentioned paste printed on the region corresponding to the second connection portion 24, a green sheet with the above-mentioned paste printed on the region corresponding to the internal wiring 23, a green sheet with the above-mentioned paste printed on the region corresponding to the first connection portion 22, and a green sheet with the above-mentioned paste printed on the region corresponding to the internal terminal 21 are prepared, and after drying, they are sequentially stacked. Drying can be performed, for example, under the condition of heating to 110° C. and maintaining for 5 minutes.
[0031] Furthermore, a plurality of green sheets (ring-shaped green sheets obtained by removing portions corresponding to the cavities 10A) to be the side wall portions 12 prepared in step S10 are further stacked. In this way, a stack of green sheets is obtained.
[0032] Next, as step S30, a firing step is performed. In this step, the stack of green sheets prepared in step S20 is fired. Firing can be performed, for example, by heating to a temperature of 800° C. or higher and 1600° C. or lower in an atmosphere mixed with hydrogen, nitrogen, and water vapor. The heating temperature is selected from a temperature range that can suppress the formation of an intermetallic compound phase in the structure of the conductive portion 20 in consideration of sufficient sintering, the intermetallic compound phase containing an intermetallic compound of a first metal component and a second metal component. Through the above steps, the ceramic wiring member 1 of the present embodiment can be manufactured.
[0033] (Implementation Method 2) Next, Embodiment 2 which is another embodiment of the present disclosure will be described. Figure 4 This is a schematic cross-sectional view showing the structure of a ceramic wiring member in the second embodiment. Figure 4 The same as that referred to in the description of Implementation 1 Figure 1 Corresponding figure. Figure 4 and Figure 1The ceramic wiring member 1 of the second embodiment basically has the same structure as that of the first embodiment and has the same effect. However, the ceramic wiring member 1 of the second embodiment is different from that of the first embodiment mainly in the arrangement and structure of the conductive portion. Hereinafter, the second embodiment will be described with the differences from the first embodiment as the center.
[0034] Reference Figure 4 The conductive portion 20 of the ceramic wiring member 1 of the second embodiment includes: an upper terminal 26 as a first portion arranged in contact with the first end surface 12A; a lower terminal 28 as a second portion arranged in contact with the second end surface 12B; and a third connecting portion 27 connecting the upper terminal 26 and the lower terminal 28. The lower terminal 28 is arranged in contact with the first main surface 11A of the bottom wall portion 11. The upper terminal 26, the lower terminal 28, and the third connecting portion 27 are all parts of the conductive portion 20 arranged in contact with the side wall portion 12 as the second plate-shaped portion.
[0035] The composition of at least one of the upper terminal 26, the lower terminal 28, and the third connecting portion 27 constituting the conductive portion 20, preferably all of them, similarly to the internal terminal 21 of the first embodiment, contains: a first metal component as a main component, the first metal component being at least one of W and Mo; and a second metal component, the second metal component being 0.1% or more and 10% or less in total relative to the first metal component, and being at least one selected from Ni, Co, and Fe. Furthermore, the above-mentioned at least one of the structures of the upper terminal 26, the lower terminal 28, and the third connecting portion 27 constituting the conductive portion 20, preferably all of them, similarly to the internal terminal 21 of the first embodiment, contains a conductive phase containing an alloy of the first metal component and the second metal component. Furthermore, the above-mentioned at least one of the structures of the upper terminal 26, the lower terminal 28, and the third connecting portion 27 constituting the conductive portion 20, preferably all of them, contains a glass phase 32, the glass phase 32 containing a ceramic component in an area ratio of 3% or more and 20% or less in the cross section of the conductive portion 20.
[0036] The ceramic wiring member 1 of the present embodiment can also obtain the same effects as those of the case of the first embodiment. In addition, the ceramic wiring member 1 of the present embodiment can be manufactured in the same manner as that of the case of the first embodiment except that the arrangement of the conductive portion 20 is mainly changed. It should be noted that in the present embodiment, the bottom wall portion 11 is made of ceramic as an insulator, but a conductor such as metal may be used as a material constituting the bottom wall portion 11.
[0037] (Implementation method 3) Next, Embodiment 3 which is still another embodiment of the present disclosure will be described. Figure 5 This is a schematic cross-sectional view showing the structure of a ceramic wiring member in the third embodiment. Figure 5 The same as that referred to in the description of Implementation 1 Figure 1 Corresponding figure. Figure 5 and Figure 1 The ceramic wiring member 1 of the third embodiment basically has the same structure as the first embodiment and has the same effect. However, the ceramic wiring member 1 of the third embodiment mainly differs from the first embodiment in the structure of the main body, the arrangement and structure of the conductive part. Hereinafter, the third embodiment will be described with the differences from the first embodiment as the center.
[0038] Reference Figure 5 , the side wall portion 12 of the ceramic wiring member 1 of the third embodiment includes a protrusion 121 that protrudes toward the area opposite to each other across the cavity 10A. The protrusion 121 includes: a first surface 121B, which is opposite to the first main surface 11A of the bottom wall portion 11; a second surface 121A, which is located on the side opposite to the first surface 121B in the thickness direction of the bottom wall portion 11; and a third surface 121C, which is an end surface connecting the first surface 121B and the second surface 121A. The area of the first surface 121B including the end connected to the third surface 121C is opposite to the first main surface 11A, and the other area (the area corresponding to the vicinity of the root of the protrusion 121) is not opposite to the first main surface 11A.
[0039] The conductive portion 20 includes an upper terminal 26 as a first portion arranged in contact with the first end surface 12A, a lower terminal 28 as a second portion arranged in contact with the second end surface 12B, and a third connection portion 27 connecting the upper terminal 26 and the lower terminal 28. The conductive portion 20 also includes an intermediate terminal 30 arranged in contact with the first surface 121B, and a fourth connection portion 29 connecting the intermediate terminal 30 and the third connection portion 27. The intermediate terminal 30 is arranged in contact with the first main surface 11A of the bottom wall portion 11. The upper terminal 26, the lower terminal 28, the third connection portion 27, the intermediate terminal 30, and the fourth connection portion 29 are all parts of the conductive portion 20 arranged in contact with the side wall portion 12.
[0040] At least one of the upper terminal 26, the lower terminal 28, the third connecting portion 27, the intermediate terminal 30, and the fourth connecting portion 29 constituting the conductive portion 20, and preferably all of the compositions include: a first metal component as a main component, the first metal component being at least one of W and Mo; and a second metal component, the second metal component being 0.1% or more and 10% or less in total relative to the first metal component, and being selected from at least one of Ni, Co, and Fe. Furthermore, at least one of the structures of the upper terminal 26, the lower terminal 28, and the third connecting portion 27 constituting the conductive portion 20, and preferably all of the structures include a conductive phase, and the conductive phase includes an alloy of the first metal component and the second metal component, similarly to the internal terminal 21, etc. of the first embodiment. In addition, at least one of the upper terminal 26, the lower terminal 28, the third connecting part 27, the intermediate terminal 30 and the fourth connecting part 29 constituting the conductive part 20, and preferably all of them, contains a glass phase 32, which contains a ceramic component in an area ratio of more than 3% and less than 20% in the cross section of the conductive part 20.
[0041] In the ceramic wiring component 1 of the present embodiment, the same effects as those in the case of the first embodiment can also be obtained. In addition, the ceramic wiring component 1 of the present embodiment can be manufactured in the same manner as the case of the first embodiment, except that the structure of the main body 10 and the arrangement of the conductive portion 20 are mainly changed. It should be noted that in the present embodiment, the bottom wall 11 is made of ceramic as an insulator, but a conductor such as metal can also be used as a material constituting the bottom wall 11. In addition, in the above-mentioned embodiment, the shape of the main body 10 is illustrated, but the shape of the main body of the present disclosure is not limited thereto. As the shape of the main body, various shapes such as a rectangular parallelepiped shape, a spherical shape, and a film shape can be adopted. Example
[0042] An experiment was conducted to confirm the resistance reduction effect of adding the second metal component. The experimental procedure is as follows.
[0043] The conductive portion disposed in contact with the main body portion was formed by the same steps as the manufacturing method described in the above embodiment, and the resistivity of the conductive portion was examined. Specifically, in step S10, a green sheet containing alumina powder was prepared.
[0044] Next, in step S20, a paste containing a first metal component and a second metal component is printed on the raw sheet prepared by step S10 and dried. No ceramic component is added to the paste. Drying is carried out under the condition of heating to 110°C and maintaining for 5 minutes. At this time, W or Mo is used as the first metal component. As the metal powder (raw material powder) of the first metal component, in principle, a metal powder with an average particle size of 1 μm is used, but a part of a metal powder with a particle size of 2.5 μm is also used. In addition, as the second metal component, Ni, Co, and Fe are used. At this time, from the perspective of confirming the appropriate amount of addition, the amount of addition is changed. In addition, for comparison, a sample without the addition of the second metal component is also produced. As the second metal component, in principle, one of Ni, Co and Fe is used, but samples with both Ni and Co added are also produced.
[0045] Then, in step S30, the green sheet printed with the paste is fired. The firing is performed by heating in an atmosphere mixed with hydrogen, nitrogen and water vapor. The heating temperature is generally 1400°C when W is used as the first metal component, and 1300°C when Mo is used as the first metal component. For comparison, a sample at 1550°C when W is used as the first metal component and a sample at 1400°C when Mo is used as the first metal component were also prepared. With respect to the conductive portion after firing, the voids not filled with the glass phase are less than 1% in terms of area ratio.
[0046] The resistivity of the obtained sample was investigated. Specifically, for the obtained sample, the resistance was first measured by the four-terminal method. The resistance was measured using RM3544-01 manufactured by Hioki Electric Co., Ltd. Then, the resistivity was calculated from the obtained resistance and the length of the conductive part and the cross-sectional area perpendicular to the length direction. In addition, for the obtained sample, the adhesion strength of the conductive part relative to the main body was measured. Specifically, a Ni plating layer with a thickness of 2 to 3 μm was applied to the conductive part with a width of 2 mm and a length of 5 mm, and a 5 mm portion of a metal L-shaped retaining member with a width of 0.7 mm, a length of 5 mm, and a height of 2.5 mm in a direction perpendicular to the length direction was joined by brazing. Next, the retaining member and the sample were held separately, and the end portion of the retaining member with a height of 2.5 mm was pulled in a direction perpendicular to the interface between the conductive part and the main body, and the load at the moment when the conductive part was peeled off from the main body was measured as the adhesion strength. The measurement used a digital dynamometer (model ZP200N) manufactured by IMADA Co., Ltd. If the adhesion strength is 9.8 N (1 kgf) or more, it can be determined that it is sufficient, and if it is less than 9.8 N, it can be determined that it is insufficient.
[0047] The contents and resistivity of each sample are shown in Table 1. In addition, for Samples 1 to 11 and Samples 19 to 23 in Table 1, the relationship between the amount of the second metal component and the resistivity is shown in Figure 6 . Figure 6 In the figure, the horizontal axis represents the relative amount of the second metal component relative to the first metal component. For example, if the horizontal axis is 2%, it means that the mass of the second metal component is 2 when the mass of the first metal component is 100. Figure 6 In the figure, the vertical axis represents resistivity. Figure 6 In the figure, the data points marked with solid circles correspond to samples 1 to 11 using W as the first metal component in Table 1. The data points marked with hollow circles correspond to samples 19 to 23 using Mo as the first metal component in Table 1.
[0048] [Table 1] Referring to Table 1, the amount of the second metal component of Sample 1 and Sample 2 among Samples 1 to 11 is lower than the lower limit of the present disclosure. On the other hand, the amount of the second metal component of Sample 11 is higher than the upper limit of the present disclosure. In addition, the amount of the second metal component of Sample 19 among Samples 19 to 23 is lower than the lower limit of the present disclosure. On the other hand, the amount of the second metal component of Sample 23 is higher than the upper limit of the present disclosure.
[0049] The results of these experiments are shown in Fig. Figure 6 It can be confirmed that no matter which of W and Mo the first metal component is, by setting the addition amount of Ni as the second metal component to the range disclosed in the present invention, that is, 0.1% or more, the resistivity can be reduced. Furthermore, by making the addition amount of the second metal component 0.5% or more, the reduction in resistivity becomes clearer. On the other hand, referring to Table 1, if the addition amount of the second metal exceeds 10%, the adhesion strength between the ceramic main body and the conductive part is reduced. It can be considered that the reason is that due to the excessive addition amount of the second metal, the sintering of the raw material powder in the main body is excessive in the sintering process of step S30. In addition, if the addition amount of the second metal exceeds 1.5%, the reduction in resistivity is saturated. From the above experimental results, it can be confirmed that from the perspective of reducing the resistivity, the addition amount of the second metal component needs to be 0.1% or more relative to the first metal component, preferably 0.5% or more. On the other hand, from the perspective of the adhesion strength between the conductive part and the ceramic main body, the addition amount of the second metal is preferably 10% or less, and since the resistivity is reduced to saturation, it can be said that it can be 1.5% or less.
[0050] In addition, referring to Table 1, in samples 12 to 15, Co or Fe is used as the second metal component instead of Ni in samples 1 to 11. From the resistivity of these samples, it can be confirmed that even when Co or Fe is used as the second metal component, the same effect as when Ni is used can be obtained. Furthermore, in sample 16, Ni and Co are added as the second metal component by 0.5% each relative to the first metal component. In this case, it can also be confirmed that the same effect as when Ni is used as the second metal component can be obtained.
[0051] Furthermore, the results of Samples 17 and 18 confirm that even when the average particle size of the raw material powder of the first metal component is changed, the resistivity of Sample 18 to which the second metal component is added is clearly reduced compared to Sample 17 to which the second metal component is not added. This confirms that even when the average particle size of the raw material powder of the first metal component is changed, the resistance can be reduced by adding an appropriate amount of the second metal component.
[0052] In addition, the firing temperature was set relatively high in Samples 24 and 25. When the second metal component is Ni, the firing temperature of 1550°C of Sample 24 using W as the first metal component and the firing temperature of 1400°C of Sample 25 using Mo as the first metal component are both within the temperature range for generating an intermetallic compound between the first metal component and the second metal component. The conductive portion of sample 29 was analyzed using an X-ray diffraction device (MiniFlex II) manufactured by Rigaku Co., Ltd., and the peak corresponding to the intermetallic compound of W and Ni was detected at a size exceeding the noise level. The same measurement was performed on sample 30, and the peak corresponding to the intermetallic compound of Mo and Ni was detected at a size exceeding the noise level. On the other hand, no peak corresponding to such an intermetallic compound was detected in samples 1 to 28.
[0053] From the above experimental results, it was confirmed that the ceramic wiring member of the present disclosure can reduce the resistance of the conductive portion.
[0054] Furthermore, an experiment was conducted to examine the influence of the area ratio of the glass phase and the average particle size of the metal particles constituting the conductive phase after firing on the resistivity of the conductive portion and the adhesion strength of the conductive portion to the main body portion.
[0055] The samples shown in Table 2 were further prepared by the same method as the samples shown in Table 1 above, and for samples 26 to 40, the area ratio of the glass phase in the conductive part in the cross section in the thickness direction of the plate-like part was investigated. Specifically, for the obtained samples, the cross section of the conductive part 20 was observed with a scanning electron microscope. Then, for the obtained image data, after black and white binarization using image processing software, the area of the glass phase 32 was totaled, and the area ratio of the glass phase 32 in the conductive part 20 was calculated. The above image processing uses ImageJ (free software). It should be noted that the numerical value of the second metal component represents the addition amount (mass %) of the second metal component relative to 100 mass % of the first metal component. In addition, the firing temperature is all set to 1400°C. Furthermore, the method for determining the average particle size of the conductive phase after firing is as follows. First, the surface or cross section of the conductive part after firing is observed with a scanning electron microscope, and an image is taken. Then, a reference line is drawn in the conductive part of the obtained image, and the distance of the reference line in the image between the starting point and the end point is calculated. Next, count the number of particles of the conductive phase in contact with the baseline. The number of conductive phase particles in contact with the baseline is preferably 20 or more. In order to make the number of conductive phase particles in contact with the baseline more than 20, the length of the baseline can be adjusted. Calculate the value obtained by dividing the distance between the start point and the end point of the baseline in the image by the number of conductive phase particles in contact with the baseline. Repeat this three times in different baselines, and take the average of the three values obtained as the average particle size of the conductive phase after sintering.
[0056] [Table 2]
[0057] In Table 2, regarding the resistivity, the case where the resistivity is lower than that in the case where the second metal component is not mixed is evaluated as "qualified". Regarding the close contact strength, 9.8N or more is evaluated as "qualified", and less than 9.8N is evaluated as "unqualified". Regarding the comprehensive judgment, the sample in which at least one of the above two evaluation items is evaluated as "unqualified" is evaluated as "unqualified", and the sample in which none of the above two evaluation items is evaluated as "unqualified" is evaluated as "qualified".
[0058] Referring to Table 2, W is used as the first metal component in samples 26 to 37. In sample 26, the area ratio of the glass phase is outside the range of 3% or more and 20% or less. Specifically, the area ratio of the glass phase exceeds 20%. As a result, the resistivity is above 0.2Ω·μm, and from the perspective of resistance, sample 26 cannot be said to be ideal. It is thus confirmed that since the second metal component is not incorporated, the glass phase of the sintering aid derived from the main body 10 invades the conductive part 20 from the main body 10 due to the capillary phenomenon, and the resistance value becomes insufficient.
[0059] In contrast, the area ratio of the glass phase was within the range of 3% to 20% in samples 27 to 36. When the second metal component was any one of Ni, Fe, and Co, these samples were judged as "acceptable" in any of the items of resistivity and adhesion strength, and it can be said that ideal characteristics were obtained.
[0060] In sample 37, the area ratio of the glass phase is outside the range of 3% or more and 20% or less. Specifically, the area ratio of the glass phase is less than 3%. As a result, the adhesion strength is less than 9.8N (less than 1kgf), and from the perspective of the adhesion strength of the conductive part 20 to the main body 10, sample 37 cannot be said to be ideal. It is thus confirmed that the formation of the glass phase 32 derived from the sintering aid of the main body 10 contributes to improving the adhesion strength of the conductive part 20 to the main body 10, and if the glass phase 32 is reduced to less than 3%, the adhesion strength becomes insufficient.
[0061] In addition, in samples 38 to 40, Mo is used as the first metal component instead of W in samples 26 to 37. From these experimental results, it was confirmed that even when Mo is used as the first metal component, the same tendency as when W is used is observed.
[0062] The above experimental results confirm that if the area ratio of the glass phase is 3% or more and 20% or less, both the resistivity and the adhesion are good. Furthermore, it is confirmed that by making the area ratio of the glass phase 8% or more and 20% or less, a higher adhesion strength can be obtained, specifically, an adhesion strength of 19.6N (2kgf) or more.
[0063] In addition, it can be confirmed that if the average particle size of the metal particles constituting the conductive phase after firing is greater than 1.2 μm and less than 5.5 μm, both the resistivity and the adhesion can obtain good results. Furthermore, it is confirmed that by making the average particle size of the metal particles constituting the conductive phase greater than 1.2 μm and less than 1.6 μm, a higher adhesion strength can be obtained, specifically, a adhesion strength of more than 19.6 N (2 kgf). Regarding the average particle size of the metal particles constituting the conductive phase after sintering, a correlation is obtained that if the proportion of the glass phase in the conductive part 20 is increased, it becomes smaller, and if the proportion of the second metal component is increased, it becomes larger. Furthermore, regarding the average particle size of the metal particles constituting the conductive phase after firing, it can also be adjusted by changing the size of the average particle size of the raw material powder before firing, or by adding a glass component to the conductive part component before firing.
[0064] It should be noted that, in the above-mentioned embodiment, the case where the main body 10 includes the side wall 12 is described, but the ceramic wiring member of the present disclosure is not limited to this, and may also include a flat main body 10 in which the side wall 12 is omitted. Such a ceramic wiring member 1 is used as a ceramic wiring substrate on which electronic components are mounted. In addition, from the viewpoint of reducing contact resistance, etc., a plating layer including a Ni (nickel) layer, an Au (gold) layer, etc. may be formed on the surface of the internal terminal 21 and the external terminal 25.
[0065] It should be understood that the embodiments and examples disclosed this time are illustrative in all aspects and are not restrictive in any aspect. The scope of the present disclosure is not defined by the above description but by the claims, and is intended to include all changes within the meaning and scope equivalent to the claims. Description of symbols
[0066] 1: ceramic wiring member; 10: main body; 10A: cavity; 11: bottom wall; 11A: first main surface; 11B: second main surface; 12: side wall; 12A: first end surface; 12B: second end surface; 20: conductive portion; 21: internal terminal; 22: first connecting portion; 23: internal wiring; 24: second connecting portion; 25: external terminal; 26: upper terminal; 27: third connecting portion; 28: lower terminal; 29: fourth connecting portion; 30: intermediate terminal; 31: conductive phase; 32: glass phase; 121: protrusion; 121A: second surface; 121B: first surface; 121C: third surface.
Claims
1. A ceramic wiring member comprising: a main body portion made of ceramic; and a conductive portion arranged in contact with the main body portion, The conductive part comprises: A first metal component as a main component, the first metal component being at least one of W and Mo; A second metal component, the second metal component accounts for 0.1% to 10% of the first metal component in total, and is at least one selected from Ni, Co, and Fe; and Ceramic components, The structure of the conductive part includes: a conductive phase comprising an alloy of the first metal component and the second metal component; and A glass phase is dispersed in the conductive phase, has an area ratio of 3% to 20% in a cross section of the conductive portion, and contains the ceramic component.
2. The ceramic wiring member according to claim 1, wherein The area ratio of the glass phase in the cross section of the conductive portion is 8% to 20%.
3. The ceramic wiring member according to claim 1 or 2, wherein The average particle size of the metal particles constituting the conductive phase is 1.2 μm or more and 5.5 μm or less.
4. The ceramic wiring member according to claim 3, wherein The metal particles have an average particle size of 1.2 μm or more and 1.6 μm or less.
5. The ceramic wiring member according to any one of claims 1 to 4, wherein The structure of the conductive portion does not include an intermetallic compound phase including an intermetallic compound of the first metal component and the second metal component.
6. The ceramic wiring member according to any one of claims 1 to 5, wherein The main body has a plate-shaped portion, The conductive part comprises: a first portion in contact with a first main surface of the plate-shaped portion; and A second portion is in contact with a second main surface located on the opposite side to the first main surface in the thickness direction of the plate-like portion.