Beta-cyclodextrin magnetic modified charcoal as well as preparation method and application thereof
By modifying β-cyclodextrin and two ball mills on walnut shell biochar, β-cyclodextrin magnetically modified biochar is formed, which solves the problems of low adsorption capacity of adsorbent and blocked pores, and achieves efficient removal of estrogen in water and the recyclability of the material.
Patent Information
- Application Number
- CN202411177123.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-19
AI Technical Summary
When removing estrogen pollutants in water, the adsorption capacity of the adsorbent material is low, the cost is high, and the regeneration is difficult. The pores of the biochar are blocked after magnetic and chemical modification, and the adsorption capacity is reduced.
By modifying β-cyclodextrin and two ball mills on walnut shell biochar, the surface functional groups and active sites are increased, and Fe2+/Fe3+ is loaded to form β-cyclodextrin magnetically modified biochar, which improves its estrogen Adsorption and recycling.
The adsorption capacity and recovery rate of β-cyclodextrin magnetically modified biochar was significantly improved, reaching an estrogen removal rate of 92.4% and a recovery rate of 93.8%, solving the problems of pore blockage and reduced adsorption capacity.
Smart Images

Figure CN118976470A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water pollution treatment, and specifically relates to a beta-cyclodextrin magnetically modified biochar and a preparation method and application thereof. Background Art
[0002] Endocrine disrupting chemicals, abbreviated as EDCs, detected in agricultural, industrial, and domestic sewage are becoming a serious problem that threatens human health and ecosystems. Among them, estradiol, abbreviated as E2, is considered the most influential due to its strong estrogenic activity. In order to reduce estrogen pollution in the environment, various methods have been explored to remove estrogen, such as advanced oxidation processes, membrane filtration, and adsorption. However, advanced oxidation requires strict operating requirements and can cause secondary pollution to the environment. Membrane filtration devices are easily clogged, which requires high operating costs. Compared with these methods, adsorption is considered to be a promising method for removing estrogen from aqueous solutions due to its accessibility and high efficiency. Many adsorbent materials have been reported for removing estrogen from water, including molecularly imprinted polymers, powdered activated carbon, and carbon nanotubes. However, due to low adsorption capacity, high cost, and difficulty in regeneration, it is subject to some limitations in large-scale application. Therefore, it is necessary to develop an economical, renewable, and adsorbent with excellent adsorption performance for the removal of estrogen pollutants based on waste resource utilization.
[0003] At present, biochar has the advantages of large specific surface area, developed pores and low cost, and has become a research hotspot for the adsorption of organic pollutants. However, the original biochar has insufficient adsorption active sites and is difficult to separate from aqueous solution. The most economical and effective way to solve this problem is to load magnetic materials such as Fe and their oxides on biochar to make it magnetic. Secondly, chemical modification of biochar can further improve its adsorption capacity for organic pollutants, but after magnetite is deposited on biochar, the pores on the surface of biochar are blocked, causing the adsorption performance of biochar materials to decrease. Physical and mechanical treatment, especially ball milling, can reduce the hydrodynamic radius of biochar, increase the specific surface area and pore volume, and promote oxygen-containing functional groups. However, most of the current studies are ball milling, and the magnetic biochar after ball milling will also be blocked and the adsorption capacity will be reduced. To this end, the present invention provides a recyclable β-cyclodextrin magnetic modified biochar material for adsorbing estrogen in wastewater. Summary of the invention
[0004] In order to solve the above problems, the present invention provides a β-cyclodextrin magnetically modified biochar and its preparation method and application. The present invention modifies the biochar with β-cyclodextrin to provide more surface functional groups and active sites. 2+ / Fe3+ The problem of biochar being difficult to recycle was solved, and the disadvantage of pore blockage in magnetic biochar materials was improved by double ball milling, thereby increasing the adsorption capacity for estrogen.
[0005] The present invention solves the above technical problems through the following technical solutions.
[0006] The first object of the present invention is to provide a method for preparing β-cyclodextrin magnetically modified biochar, comprising the following steps:
[0007] S1, grinding the walnut shell biomass, and then pyrolyzing it at 500° C. to 700° C. to obtain walnut shell biochar;
[0008] S2, ball-milling the walnut shell biochar, adding a first alkaline solution to perform an etching reaction, and obtaining alkaline biochar;
[0009] S3. Under a protective gas atmosphere, add alkaline biochar to the Fe 2+ and Fe 3+ The mixed solution of 1,2-dihydro-1,4 ...
[0010] S4. Add β-cyclodextrin to the second alkaline solution, then add a cross-linking agent, carry out a grafting reaction at room temperature, and then add magnetic biochar to continue the reaction. The cross-linking agent cross-links with the magnetic biochar, and under the catalytic action of hydroxide ions, the β-cyclodextrin, the cross-linking agent and the magnetic biochar form a ternary epoxide, and the magnetic biochar is modified to increase adsorption functional groups to obtain modified biochar. After washing and drying, the modified biochar is subjected to secondary ball milling. During the secondary ball milling, the biochar is oxidized by air to activate the biochar, and the heat and kinetic energy generated by the ball milling process promote the solid phase reaction to produce chemical bonds, thereby obtaining β-cyclodextrin magnetic modified biochar.
[0011] Furthermore, the pyrolysis was carried out at 15 °C min -1 The heating rate is increased to 500℃~700℃, and then the pyrolysis is continued for 1h.
[0012] Furthermore, the conditions for the first ball milling are: ball milling at 300 r / min to 600 r / min for 60 min, stopping the ball milling for 10 min, and then changing the rotation direction and ball milling at 300 r / min to 600 r / min for 60 min; the material-to-ball ratio of the ball milling is 1:10 to 15.
[0013] Furthermore, the conditions for the secondary ball milling are: ball milling at 400 r / min-500 r / min for 60-100 min, stopping the ball milling for 10 min, then changing the rotation direction, ball milling at 500 r / min for 60-100 min, stopping the ball milling for 10 min, and then changing the rotation direction, ball milling at 400 r / min-500 r / min for 60 min; the material-to-ball ratio of the ball milling is 1:10-15.
[0014] Furthermore, the dosage ratio of the magnetic biochar, β-cyclodextrin and cross-linking agent is 1.5g-2g:15g-20g:7.5mL-10mL, the cross-linking agent is epichlorohydrin, the solid-liquid ratio of β-cyclodextrin and the second alkaline solution is 1.5g-2g:100mL, and the second alkaline solution is 0.8mol·L -1 ~1mol·L -1 of NaOH aqueous solution or KOH aqueous solution.
[0015] Furthermore, the grafting reaction time is 6h to 8h, and the continued reaction time is 5h. After the grafting reaction is completed, water and ethanol solutions are used to wash in sequence, and then dried to obtain modified biochar.
[0016] Furthermore, the Fe 2+ The molar concentration of Fe is 0.16mol / L~0.27mol / L, 3+ The molar concentration is 0.27 mol / L to 0.37 mol / L, and the solid-liquid ratio of the alkaline biochar to the mixed solution is 4 g to 6 g: 100 mL.
[0017] Furthermore, in the process of preparing magnetic biochar, the protective gas is nitrogen, the co-precipitation reaction time is 1h to 2h, the divalent soluble iron salt is ferric sulfate, and the trivalent soluble iron salt is ferric chloride. After the co-precipitation reaction is completed, it is collected by an external magnetic field, and then washed with water and freeze-dried to obtain magnetic biochar.
[0018] Furthermore, in the process of preparing alkaline biochar, the liquid ratio of walnut shell biochar to the first alkaline solution is 3g-25g:100mL, and the first alkaline solution is 2mol·L -1 ~4mol·L -1 The etching reaction is carried out at 160 r·min. -1 The mixture was stirred and etched for 1 h, and then the biochar was washed with water to remove impurities until the pH was about 7.0, and then dried at 60 °C for 15 h to 20 h to obtain alkaline biochar.
[0019] The second object of the present invention is to provide β-cyclodextrin magnetically modified biochar prepared by the above preparation method.
[0020] The third object of the present invention is to provide the use of the above-mentioned β-cyclodextrin magnetically modified biochar as an adsorbent in removing estrogen from water, wherein the addition amount of the β-cyclodextrin magnetically modified biochar to the water to be treated is 1 mg·L -1 ~10mg·L -1 , further, the estrogen is E2.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] (1) In the process of preparing β-cyclodextrin magnetically modified biochar of the present invention, the walnut shell biochar is firstly ball-milled to increase the specific surface area and pore volume and promote oxygen-containing functional groups, and then etched with an alkaline solution to make the surface of the biochar material have more adsorption sites, which can well load magnetic iron, increase the specific surface area and micropore area, and enhance the hydrophobic effect and pore filling effect of the alkali-modified biochar; secondly, magnetic Fe3O4 nanoparticles are used to give the biochar magnetic properties, and rapid solid-liquid separation can be achieved under the condition of the external magnetic field, and then β-cyclodextrin is chemically modified to increase the adsorption functional groups. However, since the biochar is given magnetic properties and chemically modified, the pores of the biochar are blocked, the active sites are reduced, and the adsorption capacity is reduced, so a second ball milling is performed. After the second ball milling, the biochar can be activated, and the structure, composition and magnetic properties of the material are not changed or lost. The heat and kinetic energy generated by the ball milling process promote the solid-phase reaction to produce chemical bonds. Because ball milling is usually accompanied by crystal deformation and defects, the blockage of the biochar pores is partially relieved. With the restoration of surface functional groups, β-cyclodextrin magnetically modified biochar exhibited remarkable adsorption capacity.
[0023] (2) The mechanism of the adsorption of estrogen by the β-cyclodextrin magnetically modified biochar material prepared by the present invention is as follows: the surface of the modified biochar material is loaded with β-cyclodextrin, rich amino and hydroxyl functional groups, so that the recyclable β-cyclodextrin magnetically modified biochar material has a high adsorption capacity for estrogen. Different adsorption mechanisms are involved in the adsorption process, including pore filling, hydrogen bonding, functional group attraction, electrostatic attraction, ion exchange, π-π bond and hydrophobic effect.
[0024] (3) The removal rate of E2 by the β-cyclodextrin modified biochar material prepared by the present invention reached 92.4%. After two ball millings, the surface functional groups and specific surface area of the adsorbent were greatly restored, thereby increasing the recovery rate of the biochar material from 83.17% to 93.8%. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The present invention is a process flow chart for preparing recyclable β-cyclodextrin magnetically modified biochar material.
[0026] Figure 2This is a scanning electron microscope image of the β-cyclodextrin magnetically modified biochar prepared in Example 1 of the present invention, wherein: Figure 2 A is walnut shell biochar, and B is β-cyclodextrin magnetically modified biochar.
[0027] Figure 3 This is the infrared spectrum of the β-cyclodextrin magnetically modified biochar prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] It should be noted that the professional terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specifically stated, the various raw materials, reagents, instruments and equipment used in the following embodiments of the present invention can be purchased from the market or prepared by existing methods.
[0030] Biochar has the advantages of large specific surface area (SSA), developed pores and low cost, and has become a research hotspot for the adsorption of organic pollutants. It should be noted that the existing biochars, such as straw biochar and sludge biochar, have low structural density and poor permeability between biochar pores, and fail to form an effective channel structure. In the direct grinding process, the structure is severely damaged and the pores on the surface of the biochar are blocked. Walnut shell biochar is obtained by pyrolysis of walnut shell biomass. Since the walnut shell structure is dense, the biochar formed after pyrolysis has a high structure density, and the biochar pores form an effective channel structure with high surface reactivity. However, when the walnut shell biochar is endowed with magnetism and chemically modified, the micropores and mesopores on the surface of the walnut shell biochar are aggregated, which easily blocks the pores, reduces the specific surface area and pore volume, and reduces the oxygen-containing functional groups, that is, the adsorption active sites, which leads to poor modification effect and decreased adsorption performance. Based on this, on the one hand, the present invention provides a preparation method of β-cyclodextrin magnetically modified biochar, and the process flow is as follows: Figure 1 As shown, the following steps are included:
[0031] S1. Grind the walnut shell biomass into powder less than 2 mm, wash with water to remove residual sugar, dry at 65 °C for 12 h, and then purify under nitrogen at 15 °C min -1 The heating rate is increased to 500℃~700℃, and then the pyrolysis is continued for 1h to obtain walnut shell biochar;
[0032] S2, ball-milling the walnut shell biochar, adding the first alkaline solution to perform an etching reaction, and after the reaction, washing the biochar with water to remove impurities until the pH is about 7.0, and then drying at 60° C. for 15 h to 20 h to obtain alkaline biochar;
[0033] S3. Under a protective gas atmosphere, a mixed solution containing a divalent soluble iron salt and a trivalent soluble iron salt is added to the alkaline biochar, and after stirring evenly, the pH is adjusted to 10-12 with NH3·H2O, and the alkaline biochar is used as a carrier, and a co-precipitation reaction is carried out by stirring at 80°C to 120°C, and ferrosoferric oxide particles are loaded in situ to obtain magnetic biochar;
[0034] S4. Add β-cyclodextrin to the second alkaline solution, then add a cross-linking agent, carry out a grafting reaction at room temperature under alkaline conditions, and then add magnetic biochar to continue the reaction. The cross-linking agent cross-links with the magnetic biochar, and under the catalytic action of hydroxide ions, the β-cyclodextrin, the cross-linking agent and the magnetic biochar form a ternary epoxide, the magnetic biochar is modified, the adsorption functional groups are increased, and the modified biochar is obtained. After washing and drying, the modified biochar is subjected to secondary ball milling. During the secondary ball milling, the biochar is activated, oxidized by air, and the heat and kinetic energy generated by the ball milling process promote the solid-phase reaction to produce chemical bonds, break the pore wrapping, and produce new pores in the biochar for recovery. The ion exchange, π-π and hydrogen interactions are increased compared with the former, and the β-cyclodextrin magnetic modified biochar is obtained.
[0035] In the process of preparing beta-cyclodextrin magnetically modified biochar of the present invention, firstly, the walnut shell biochar is ball-milled once to increase the specific surface area and pore volume and promote oxygen-containing functional groups, and then the walnut shell biochar is etched by an alkaline solution so that the surface of the biochar material has more adsorption sites, which can well load magnetic iron, increase the specific surface area and micropore area, and enhance the hydrophobic effect and pore filling effect of the alkaline-modified biochar; secondly, magnetic Fe3O4 nanoparticles are used to give the biochar magnetic properties, and rapid solid-liquid separation can be achieved under the condition of the existence of an external magnetic field, and then beta-cyclodextrin is chemically modified to increase the adsorption functional groups, but since the biochar is given magnetic properties and chemically modified, the pores of the biochar are blocked, the active sites are reduced, and the adsorption capacity is reduced, so a secondary ball milling is performed, and the biochar can be activated after the secondary ball milling, and the structure, composition and magnetism of the material are not changed or lost, and the heat and kinetic energy generated by the ball milling process promote the solid phase reaction to produce chemical bonds, because ball milling is usually accompanied by crystal deformation and defects, and the blockage of the biochar pores is partially relieved. With the recovery of surface functional groups, β-cyclodextrin magnetically modified biochar showed significant adsorption capacity. The removal rate of E2 by the prepared β-cyclodextrin modified biochar material reached 92.4%. After two ball millings, the surface functional groups and specific surface area of the adsorbent were greatly restored, thereby increasing the recovery rate of the biochar material from 83.17% to 93.8%.
[0036] In a specific embodiment, pyrolysis is performed by placing the walnut shell biomass powder in a tube furnace at 15°C min -1 The heating rate is increased to 500℃~700℃, and then the pyrolysis is continued for 1h.
[0037] In a specific embodiment, the conditions for a ball milling are: ball milling at 300 r / min-600 r / min for 60 min, stopping the ball milling for 10 min, and then changing the rotation direction and ball milling at 300 r / min-600 r / min for 60 min; the material-to-ball ratio of the ball milling is 1:10-15.
[0038] In a specific embodiment, the conditions for secondary ball milling are: ball milling at 400 r / min-500 r / min for 60 min-100 min, stopping ball milling for 10 min, then changing the rotation direction, ball milling at 500 r / min for 60 min-100 min, stopping ball milling for 10 min, and then changing the rotation direction, ball milling at 400 r / min-500 r / min for 60 min; the material-to-ball ratio of ball milling is 1:10-15.
[0039] In the present invention, the first ball milling of biochar can reduce the hydrodynamic radius of walnut biochar, increase the specific surface area and pore volume and promote oxygen-containing functional groups. However, due to the magnetism of walnut biochar and the chemical modification of β-cyclodextrin, Fe3O4 aggregates micropores and mesopores on the surface of biochar, and the β-cyclodextrin magnet is only randomly dispersed on the surface of the carbonaceous substrate, rather than completely covering its surface. Since the functional groups on the biochar after ball milling can be bound and wrapped by magnetite and β-cyclodextrin, the active sites of biochar adsorption are reduced, so secondary ball milling is performed. After the secondary ball milling, the adsorbent can be activated, and the structure, composition and magnetic properties of the material are not changed or lost, which means that the composite material is not damaged. Even under strong grinding, the materials are closely connected. This is because after the modified biochar is ball milled twice, it can be oxidized by the air in the tank, and the heat and kinetic energy generated by the ball milling process promote the solid phase reaction to produce chemical bonds. Because ball milling is usually accompanied by crystal deformation and defects, the blockage of biochar pores is partially relieved. With the recovery of surface functional groups, the Zeta potential of the adsorbent is also restored to a certain extent. The ion exchange, π-π and hydrogen interactions increased compared with the former. Meanwhile, SSA and pore volume PV were recovered by utilizing the shear force from the co-grinded hard and ultrafine magnetite to break the pore wrapping and generate new pores in the biochar, thus also providing some additional adsorption sites. The β-cyclodextrin magnetically modified biochar showed a significant adsorption capacity.
[0040] In a specific embodiment, the amount ratio of the magnetic biochar, β-cyclodextrin and cross-linking agent is 1.5g~2g:15g~20g:7.5mL~10mL, the cross-linking agent is epichlorohydrin, the solid-liquid ratio of β-cyclodextrin and the second alkaline solution is 1.5g~2g:100mL, and the second alkaline solution is 0.8mol·L -1 ~1mol·L -1 NaOH aqueous solution or KOH aqueous solution. In the present invention, epichlorohydrin crosslinking agent is used. First, epichlorohydrin undergoes nucleophilic addition reaction with nucleophilic sites in the matrix, such as hydrogen, oxygen, nitrogen, etc., to form COC bonds; secondly, hydrogen atoms on the alkyl chain of epichlorohydrin are replaced by hydrogen ions to generate hydroxide ions. Finally, the hydroxide ions of the alkaline solution are used as catalysts to induce electrophilic ring-opening reaction on the epoxy group to form a ternary epoxide. The ternary epoxide further undergoes ring-opening reaction with nucleophilic sites in the matrix to form crosslinking points, thereby increasing the stability and durability of the material. In general, it is to increase the stability of the material.
[0041] In a specific embodiment, the grafting reaction time is 6h to 8h, and the continued reaction time is 5h. After the grafting reaction is completed, water and ethanol solutions are used to wash in sequence, and then dried to obtain modified biochar.
[0042] In a specific embodiment, the mixed solution contains Fe 2+ The molar concentration of Fe is 0.16mol / L~0.27mol / L, 3+ The molar concentration is 0.27mol / L~0.37mol / L, and the solid-liquid ratio of the alkaline biochar to the mixed solution is 4g~6g:100mL; wherein, the mass ratio of the alkaline biochar, divalent soluble iron salt and trivalent soluble iron salt is 4~6:2.5~4:4.5~6, and the solid-liquid ratio of the alkaline biochar to the mixed solution is 4g~6g:100mL. In the present invention, alkaline biochar is used as a carrier, and ferrous oxide is loaded in situ through a coprecipitation reaction. There is a strong interaction between the Fe-O functional group and E2, which increases the adsorption performance of biochar to E2, and at the same time gives the biochar superparamagnetism, which can be removed under the action of magnetic force, and is easy to separate from E2, and has good recyclability.
[0043] In a specific embodiment, during the preparation of magnetic biochar, the protective gas is nitrogen, the coprecipitation reaction time is 1h to 2h, the divalent soluble iron salt is ferric sulfate, and the trivalent soluble iron salt is ferric chloride. After the coprecipitation reaction is completed, an external magnetic field is used to collect, and then washed with water and freeze-dried to obtain magnetic biochar. In the present invention, the ionic reaction equation for the coprecipitation reaction of the divalent soluble iron salt, the trivalent soluble iron salt and the alkaline biochar is: Fe 2+ +2Fe 3+ +8OH - =Fe3O4↓+4H2O. The ferroferric oxide obtained by co-precipitation under alkaline conditions combines more firmly with the biochar, resulting in magnetic biochar with stable properties.
[0044] In a specific embodiment, during the preparation of alkaline biochar, the liquid ratio of walnut shell biochar to the first alkaline solution is 3g-25g:100mL, and the first alkaline solution is 2mol·L -1 ~4mol·L -1 The etching reaction is carried out at 160 r·min. -1 Stir and etch for 1h. In the present invention, after adding alkaline solution, it can react with the biochar skeleton, so that the surface of the modified biochar is smooth, the holes are increased, the specific surface area and the micropore area are increased, and the functional groups after modification do not change significantly. The target pollutant E2 is hydrophobic, so it can be hydrophobic and pore-filling with alkali-modified biochar, improve the adsorption of the target pollutant, and provide feasibility for the subsequent removal of the target pollutant. At the same time, alkali-modified biochar can be well loaded with magnetic iron to form a composite material because it has more adsorption sites.
[0045] On the other hand, the present invention provides β-cyclodextrin magnetically modified biochar prepared by the above preparation method. The use of β-cyclodextrin magnetically modified biochar as an adsorbent in removing estrogen from water, and the addition amount of β-cyclodextrin magnetically modified biochar in the water to be treated is 1 mg·L -1 ~10mg·L -1 , further, the estrogen is E2. In the present invention, the mechanism of adsorption of estrogen by β-cyclodextrin magnetically modified biochar material is as follows: the surface of the modified biochar material is loaded with β-cyclodextrin, rich amino and hydroxyl functional groups, so that the recyclable β-cyclodextrin magnetically modified biochar material has a high adsorption capacity for estrogen, and different adsorption mechanisms are involved in the adsorption process, including pore filling, hydrogen bonding, functional group attraction, electrostatic attraction, ion exchange, π-π bond and hydrophobic effect. The removal rate of E2 by β-cyclodextrin modified biochar material reaches 92.4%. After two ball millings, the surface functional groups and specific surface area of the adsorbent are greatly restored, thereby increasing the recovery rate of the biochar material from 83.17% to 93.8%.
[0046] The invention is further described below through specific examples.
[0047] Example 1
[0048] A method for preparing β-cyclodextrin magnetically modified biochar comprises the following steps:
[0049] S1. The walnut shell biomass was ground into powder less than 2 mm, washed with deionized water to remove residual sugar, and then dried in an electric blast drying oven at 65 °C for 12 h, and then dried in a nitrogen atmosphere at 15 °C min -1 The temperature was raised to 700°C at a rate of 1.5 °C, and then the pyrolysis was continued for 1 h to obtain walnut shell biochar.
[0050] S2. Put 80 mg of walnut shell biochar into a ball mill for one ball milling. Add 15 times the mass of 3 mm diameter stainless steel balls. Mill at 500 r / min for 60 min. Stop milling for 10 min. Change the rotation direction and mill at 500 r / min for 60 min. After one ball milling, add 3 mol·L -1 The KOH solution was added to a 100 mL flask containing 5.0 g of walnut shell biochar and heated at 160 r·min at room temperature. -1 After stirring and etching for 1 h, the walnut shell biochar was washed with deionized water to remove impurities until the pH was about 7.0, and then dried at 60 °C for 20 h to obtain alkaline biochar;
[0051] S3. Under a nitrogen atmosphere, 4.5 g of FeCl3·6H2O and 2.5 g of FeSO4·7H2O were mixed with 4 g of alkaline biochar in 100 mL of ultrapure water, stirred at room temperature for 30 min, and then the pH was adjusted to 10.5 with NH3·H2O. The coprecipitation reaction was stirred at 120°C for 1 h. After the reaction, the obtained material was collected by applying an external magnetic field, washed with ultrapure water and freeze-dried at -30°C for 15 h to obtain magnetic biochar.
[0052] S4. Add 100 mL of 0.875 mol·L -1 Then, 7.5 mL of epichlorohydrin crosslinking agent was added to the solution of NaOH, and the grafting reaction was carried out at room temperature for 6 h; 2 g of magnetic biochar was added and stirred for 5 h. After the reaction, the biochar was washed with ultrapure water and ethanol solution to obtain modified biochar;
[0053] S5. Put 80 mg of modified biochar into a ball mill for secondary ball milling, add stainless steel balls with a diameter of 3 mm and a mass 15 times that of the modified biochar, and ball mill at 500 r / min for 60 min. Stop ball milling for 10 min, then change the rotation direction, ball mill at 500 r / min for 60 min, stop ball milling for 10 min, and then change the rotation direction, ball mill at 500 r / min for 60 min to obtain β-cyclodextrin magnetically modified biochar.
[0054] Example 2
[0055] A method for preparing β-cyclodextrin magnetically modified biochar comprises the following steps:
[0056] S1. Grind the walnut shell biomass into powder less than 2 mm, wash with deionized water to remove residual sugar, dry it in an electric blast drying oven at 65 ° C for 12 h, and then heat it to 700 ° C at a rate of 15 ° C min-1 under a nitrogen atmosphere, and then keep it warm for 1 h to obtain walnut shell biochar;
[0057] S2. Put 80 mg of walnut shell biochar into a ball mill for one ball milling. Add 15 times the mass of 3 mm diameter stainless steel balls. Mill at 500 r / min for 60 min. Stop milling for 10 min. Change the rotation direction and mill at 500 r / min for 60 min. After one ball milling, add 3 mol·L -1 The KOH solution was added to a 100 mL flask containing 5.0 g of walnut shell biochar and heated at 160 r·min at room temperature. -1 After stirring and etching for 1 h, the walnut shell biochar was washed with deionized water to remove impurities until the pH was about 7.0, and then dried at 60 °C for 20 h to obtain alkaline biochar;
[0058] S3. Under a nitrogen atmosphere, 6 g of FeCl3·6H2O and 4.0 g of FeSO4·7H2O were mixed with 4 g of alkaline biochar in 100 mL of ultrapure water, stirred at room temperature for 30 min, and then the pH was adjusted to 10.5 with NH3·H2O. The coprecipitation reaction was stirred at 120°C for 1 h. After the reaction, the obtained material was collected by applying an external magnetic field, washed with ultrapure water and freeze-dried at -20°C for 24 h to obtain magnetic biochar;
[0059] S4. Add 100 mL of 0.875 mol·L -1 Then, 7.5 mL of epichlorohydrin crosslinking agent was added to the solution of NaOH, and the grafting reaction was carried out at room temperature for 6 h; 2 g of magnetic biochar was added and stirred for 5 h. After the reaction, the biochar was washed with ultrapure water and ethanol solution to obtain modified biochar;
[0060] S5. Put 80 mg of modified biochar into a ball mill for secondary ball milling, add stainless steel balls with a diameter of 3 mm and a mass 15 times that of the modified biochar, and ball mill at 500 r / min for 60 min. Stop ball milling for 10 min, then change the rotation direction, ball mill at 500 r / min for 60 min, stop ball milling for 10 min, and then change the rotation direction, ball mill at 500 r / min for 60 min to obtain β-cyclodextrin magnetically modified biochar.
[0061] Example 3
[0062] A method for preparing β-cyclodextrin magnetically modified biochar comprises the following steps:
[0063] S1. Grind the walnut shell biomass into powder less than 2 mm, wash with deionized water to remove residual sugar, dry it in an electric blast drying oven at 65 ° C for 12 h, and then heat it to 700 ° C at a rate of 15 ° C min-1 under a nitrogen atmosphere, and then keep it warm for 1 h to obtain walnut shell biochar;
[0064] S2. Put 80 mg of walnut shell biochar into a ball mill for one ball milling. Add 15 times the mass of 3 mm diameter stainless steel balls. Mill at 500 r / min for 60 min. Stop milling for 10 min. Change the rotation direction and mill at 400 r / min for 60 min. After one ball milling, add 3 mol·L -1 The KOH solution was added to a 100 mL flask containing 5.0 g of walnut shell biochar and heated at 160 r·min at room temperature. -1 After stirring and etching for 1 h, the walnut shell biochar was washed with deionized water to remove impurities until the pH was about 7.0, and then dried at 60 °C for 20 h to obtain alkaline biochar;
[0065] S3. Under a nitrogen atmosphere, 4.5 g of FeCl3·6H2O and 2.5 g of FeSO4·7H2O were mixed with 4 g of alkaline biochar in 100 mL of ultrapure water, stirred at room temperature for 30 min, and then the pH was adjusted to 10.5 with NH3·H2O. The coprecipitation reaction was stirred at 120°C for 1 h. After the reaction, the obtained material was collected by applying an external magnetic field, washed with ultrapure water and freeze-dried at -40°C for 12 h to obtain magnetic biochar.
[0066] S4. Add 100 mL of 0.875 mol·L -1 Then, 8.5 mL of epichlorohydrin crosslinking agent was added to the solution of NaOH, and the grafting reaction was carried out at room temperature for 6 h; 2 g of magnetic biochar was added and stirred for 5 h. After the reaction, the biochar was washed with ultrapure water and ethanol solution to obtain modified biochar;
[0067] S5. Put 80 mg of modified biochar into a ball mill for secondary ball milling, add stainless steel balls with a diameter of 3 mm and a mass 12 times that of the modified biochar, and ball mill at 500 r / min for 60 min. Stop ball milling for 10 min, then change the rotation direction, ball mill at 500 r / min for 60 min, stop ball milling for 10 min, and then change the rotation direction, ball mill at 500 r / min for 60 min to obtain β-cyclodextrin magnetically modified biochar.
[0068] Example 4
[0069] A method for preparing β-cyclodextrin magnetically modified biochar comprises the following steps:
[0070] S1. Grind the walnut shell biomass into powder less than 2 mm, wash with deionized water to remove residual sugar, dry it in an electric blast drying oven at 65 ° C for 12 h, and then heat it to 550 ° C at a rate of 15 ° C min-1 under a nitrogen atmosphere, and then keep it warm for 1 h to obtain walnut shell biochar;
[0071] S2. Put 80 mg of walnut shell biochar into a ball mill for one ball milling. Add 10 times the mass of 3 mm diameter stainless steel balls. Mill at 500 r / min for 60 min. Stop milling for 10 min. Change the rotation direction and mill at 450 r / min for 60 min. After one ball milling, 3 mol·L -1 The KOH solution was added to a 100 mL flask containing 5.0 g of walnut shell biochar and heated at 160 r·min at room temperature. -1 After stirring and etching for 1 h, the walnut shell biochar was washed with deionized water to remove impurities until the pH was about 7.0, and then dried at 60 °C for 20 h to obtain alkaline biochar;
[0072] S3. Under a nitrogen atmosphere, 4.5 g of FeCl3·6H2O and 2.5 g of FeSO4·7H2O were mixed with 4 g of alkaline biochar in 100 mL of ultrapure water, stirred at room temperature for 30 min, and then the pH was adjusted to 10.5 with NH3·H2O. The coprecipitation reaction was stirred at 120°C for 1 h. After the reaction, the obtained material was collected by applying an external magnetic field, washed with ultrapure water and freeze-dried at -30°C for 15 h to obtain magnetic biochar.
[0073] S4. Add 100 mL of 0.875 mol·L -1 Then, 7.5 mL of epichlorohydrin crosslinking agent was added to the solution of NaOH, and the grafting reaction was carried out at room temperature for 6 h; 2 g of magnetic biochar was added and stirred for 5 h. After the reaction, the biochar was washed with ultrapure water and ethanol solution to obtain modified biochar;
[0074] S5. Put 80 mg of modified biochar into a ball mill for secondary ball milling, add stainless steel balls with a diameter of 3 mm and a mass 10 times that of the modified biochar, and ball mill at 500 r / min for 60 min. Stop ball milling for 10 min, then change the rotation direction, ball mill at 500 r / min for 60 min, stop ball milling for 10 min, and then change the rotation direction, ball mill at 500 r / min for 60 min to obtain β-cyclodextrin magnetically modified biochar.
[0075] Comparative Example 1
[0076] A method for preparing magnetically modified biochar comprises the following steps:
[0077] S1. The walnut shell biomass was ground into powder less than 2 mm, washed with deionized water to remove residual sugar, and then dried in an electric blast drying oven at 65 °C for 12 h, and then dried in a nitrogen atmosphere at 15 °C min -1 The temperature was raised to 700°C at a rate of 1.5 °C, and then the pyrolysis was continued for 1 h to obtain walnut shell biochar.
[0078] S2. Put 80 mg of walnut shell biochar into a ball mill for one ball milling. Add stainless steel balls with a diameter of 3 mm and a mass 10 times that of the walnut shell biochar. Mill at 500 r / min for 60 min. Stop milling for 10 min. Change the rotation direction and mill at 500 r / min for 60 min. After one ball milling, add 3 mol·L -1 The KOH solution was added to a 100 mL flask containing 5.0 g of walnut shell biochar and heated at 160 r·min at room temperature. -1 After stirring and etching for 1 h, the walnut shell biochar was washed with deionized water to remove impurities until the pH was about 7.0, and then dried at 60 °C for 20 h to obtain alkaline biochar;
[0079] S3. Under a nitrogen atmosphere, 4.5 g of FeCl3·6H2O and 2.5 g of FeSO4·7H2O were mixed with 4 g of alkaline biochar in 100 mL of ultrapure water, stirred at room temperature for 30 min, and then the pH was adjusted to 10.5 with NH3·H2O. The coprecipitation reaction was stirred at 120°C for 1 h. After the reaction, the obtained material was collected by applying an external magnetic field, washed with ultrapure water and freeze-dried at -30°C for 15 h to obtain magnetic biochar.
[0080] S4. Put 80 mg of magnetic biochar into a ball mill for secondary ball milling, add stainless steel balls with a diameter of 3 mm and a mass 10 times that of the raw material, and ball mill at 500 r / min for 60 min. Stop ball milling for 10 min, then change the rotation direction, ball mill at 500 r / min for 60 min, stop ball milling for 10 min, and then change the rotation direction, ball mill at 500 r / min for 60 min to obtain modified biochar.
[0081] Comparative Example 2
[0082] A method for preparing β-cyclodextrin magnetically modified biochar comprises the following steps:
[0083] S1. The walnut shell biomass was ground into powder less than 2 mm, washed with deionized water to remove residual sugar, and then dried in an electric blast drying oven at 65 °C for 12 h, and then dried in a nitrogen atmosphere at 15 °C min -1 The temperature was raised to 700°C at a rate of 1.5 °C, and then the pyrolysis was continued for 1 h to obtain walnut shell biochar.
[0084] S2. Put 80 mg of walnut shell biochar into a ball mill for one ball milling. Add 15 times the mass of 3 mm diameter stainless steel balls. Mill at 500 r / min for 60 min. Stop milling for 10 min. Change the rotation direction and mill at 500 r / min for 60 min. After one ball milling, add 3 mol·L -1 The KOH solution was added to a 100 mL flask containing 5.0 g of walnut shell biochar and heated at 160 r·min at room temperature. -1 After stirring and etching for 1 h, the walnut shell biochar was washed with deionized water to remove impurities until the pH was about 7.0, and then dried at 60 °C for 20 h to obtain alkaline biochar;
[0085] S3. Under a nitrogen atmosphere, 4.5 g of FeCl3·6H2O and 2.5 g of FeSO4·7H2O were mixed with 4 g of alkaline biochar in 100 mL of ultrapure water, stirred at room temperature for 30 min, and then the pH was adjusted to 10.5 with NH3·H2O. The coprecipitation reaction was stirred at 120°C for 1 h. After the reaction, the obtained material was collected by applying an external magnetic field, washed with ultrapure water and freeze-dried at -30°C for 15 h to obtain magnetic biochar.
[0086] S4. Add 100 mL of 0.875 mol·L -1 Then, 7.5 mL of epichlorohydrin crosslinking agent was added to the NaOH aqueous solution and the grafting reaction was carried out at room temperature for 6 hours; 2 g of magnetic biochar was added and stirred for 5 hours. After the reaction, it was washed with ultrapure water and ethanol solution to obtain β-cyclodextrin magnetic modified biochar.
[0087] Comparative Example 3
[0088] A method for preparing β-cyclodextrin magnetically modified biochar comprises the following steps:
[0089] S1. The walnut shell biomass was ground into powder less than 2 mm, washed with deionized water to remove residual sugar, and then dried in an electric blast drying oven at 65 °C for 12 h, and then dried in a nitrogen atmosphere at 15 °C min -1 The temperature was raised to 700°C at a rate of 1.5 °C, and then the pyrolysis was continued for 1 h to obtain walnut shell biochar.
[0090] S2. Put 80 mg of walnut shell biochar into a ball mill for ball milling. Add 15 times the mass of 3 mm diameter stainless steel balls and mill at 500 r / min for 120 min. After the ball milling, 3 mol·L -1 The KOH solution was added to a 100 mL flask containing 5.0 g of walnut shell biochar and heated at 160 r·min at room temperature. -1 After stirring and etching for 1 h, the walnut shell biochar was washed with deionized water to remove impurities until the pH was about 7.0, and then dried at 60 °C for 20 h to obtain alkaline biochar;
[0091] S3. Under a nitrogen atmosphere, 4.5 g of FeCl3·6H2O and 2.5 g of FeSO4·7H2O were mixed with 4 g of alkaline biochar in 100 mL of ultrapure water, stirred at room temperature for 30 min, and then the pH was adjusted to 10.5 with NH3·H2O. The coprecipitation reaction was stirred at 120°C for 1 h. After the reaction, the obtained material was collected by applying an external magnetic field, washed with ultrapure water and freeze-dried at -30°C for 15 h to obtain magnetic biochar.
[0092] S4. Add 100 mL of 0.875 mol·L -1 Then, 7.5 mL of epichlorohydrin crosslinking agent was added to the solution of NaOH, and the grafting reaction was carried out at room temperature for 6 h; 2 g of magnetic biochar was added and stirred for 5 h. After the reaction, the biochar was washed with ultrapure water and ethanol solution to obtain modified biochar;
[0093] S5. Put 80 mg of modified biochar into a ball mill for secondary ball milling, add stainless steel balls with a mass 15 times that of the modified biochar and a diameter of 3 mm, and ball mill at 500 r / min for 180 min to obtain β-cyclodextrin magnetically modified biochar.
[0094] Embodiments 1 to 4 of the present invention all produce β-cyclodextrin magnetically modified biochar having similar structures. The β-cyclodextrin magnetically modified biochar prepared in Embodiment 1 is taken as an example to illustrate the structural advantages of the β-cyclodextrin magnetically modified biochar, and the results are as follows.
[0095] Figure 2 This is a scanning electron microscope image of the β-cyclodextrin magnetically modified biochar prepared in Example 1 of the present invention, wherein: Figure 2 A is walnut shell biochar, and B is β-cyclodextrin magnetic modified biochar. Figure 2 As shown in A in Figure 1, it can be observed that the cross-section of the walnut shell biochar is honeycomb-shaped, with slight depressions on the surface and no sediments observed; Figure 2 As shown in B, it can be observed that the surface of the β-cyclodextrin magnetically modified biochar material is covered with a large number of white clustered small particles and sediments, which may be β-cyclodextrin and Fe3O4 particles.
[0096] Figure 3 This is the infrared spectrum of the β-cyclodextrin magnetically modified biochar prepared in Example 1 of the present invention. Figure 3 As shown in the infrared spectra of walnut shell biochar and β-cyclodextrin magnetically modified biochar, the infrared spectra of walnut shell biochar and β-cyclodextrin magnetically modified biochar are 3433 cm –1 The peaks appearing near are attributed to the stretching vibrations of OH and NH. After modification, a new absorption peak appeared in the β-cyclodextrin magnetic modified biochar. It can be observed that at 1613 cm –1 / 1640cm –1 The absorption peak that appears is related to the stretching vibration of aromatic C=O, at 1262cm –1 The absorption peak that appears is related to the bending vibration of OH, at 1025cm –1 ~1107cm –1 The peaks in the range are related to the stretching vibration of COC or CO, which is due to the cross-linking of epichlorohydrin with β-cyclodextrin. In addition, a peak at 583 cm–1 The peak of Fe3O4 and β-cyclodextrin was attributed to the stretching vibration of Fe-O. The above results show that Fe3O4 and β-cyclodextrin were successfully modified on biochar.
[0097] The biochar that was ball-milled once in the process of preparing β-cyclodextrin magnetically modified biochar in Example 1 was recorded as BC-1, the biochar that was loaded with β-cyclodextrin magnetically modified was recorded as BC-2, and the biochar that was ball-milled twice was recorded as BC-3. The SSA and PV of BC-1, BC-2 and BC-3 are shown in Table 1. As can be seen from Table 1, the surface of BC-1 is smooth, and there are small particles on the surface of BC-2, which shows that it is the introduction of β-cyclodextrin and Fe3O4. The SSA and PV of BC-1, after the introduction of β-cyclodextrin magnetic modification, the SSA increased from 186.5m 2 / g dropped to 51.7m 2 / g, PV from 40.7m 3 / g dropped to 11.3cm 3 / g. This means that the surface of BC-2 is blocked, and the ultrafine magnetite aggregates in micropores and mesopores on the surface of the adsorbent. In addition, the functional groups of BC-2 are also reduced compared with BC-1. This is because the functional groups on the biochar after ball milling can be bound and wrapped by magnetite, and the number of carboxyl and phenolic groups of magnetite itself is also insufficient. The reduction of SSA, PV, and functional groups represents the reduction of active sites for adsorption. In order to solve the above problems, secondary ball milling was carried out to obtain BC-3; the adsorbent can be activated after secondary ball milling, and the structure, composition and magnetic properties of the material have not changed or lost, which means that the composite material is not damaged. Even under secondary strong milling, the materials are closely connected. The carboxyl, lactone and phenolic groups of BC-3 are gradually restored and reach 92.5% of the corresponding groups of BC-1, while the recovery rate of total acidic groups is as high as 96.7%, and the aromatic C–C increases. This is because after the modified biochar is ball milled, it can be oxidized by the air in the tank, and the heat and kinetic energy generated by the ball milling process promote the solid-phase reaction to produce chemical bonds. Because ball milling is usually accompanied by crystal deformation and defects, it is speculated that the blockage of the pores is partially relieved. With the recovery of surface functional groups, the Zeta potential of the adsorbent is also restored to a certain extent. BC-1 and BC-3 have similar Zeta potentials in water, but the adsorption amount of BC-1 at the zero charge point is much lower than that of BC-3. The surface functional groups and aromatic CC bonds of BC-3 are restored and increased, resulting in increased ion exchange, π-π and hydrogen interactions compared with the former. At the same time, the shear force of the ground hard and ultrafine magnetite breaks the pore wrapping in the biochar and creates new pores, allowing the SSA and PV to be restored, in addition to adding some additional adsorption sites. Therefore, BC-3 shows a significant adsorption capacity.
[0098] Table 1 Specific surface area and pore volume results of biochar materials
[0099] deal with <![CDATA[Specific surface area SSA (m 2 / g)]]> <![CDATA[Pore volume PV (cm 3 / g)]]> BC-1 186.5 40.7 BC-2 51.7 11.3 BC-3 199.6 39.8
[0100] The β-cyclodextrin magnetically modified biochar prepared in Examples 1 to 4, the modified biochar prepared in Comparative Example 1, the β-cyclodextrin magnetically modified biochar prepared in Comparative Example 2, and the β-cyclodextrin magnetically modified biochar prepared in Comparative Example 3 were used as adsorbents for the test of removing estrogen from water, including the following steps: All estrogen removal experiments were completed in a conical flask. The β-cyclodextrin magnetically modified biochar prepared in Examples 1 to 4, the modified biochar prepared in Comparative Example 1, the β-cyclodextrin magnetically modified biochar prepared in Comparative Example 2, and the β-cyclodextrin magnetically modified biochar prepared in Comparative Example 3 were added in an amount of 20 mg·L -1 , the addition amount of E2 is 1000μg·L -1 , 3 parallels were set for each treatment. All treatment groups were placed in a constant temperature shaking incubator at 25°C and 200rpm for 2h. After equilibrium adsorption, the exhausted adsorbent was separated and collected by a magnet. The adsorbent was further regenerated several times with ethanol until the supernatant became colorless and transparent. The removal rate of E2 and the recovery rate of biochar materials are shown in Table 2.
[0101] Table 2 Removal efficiency of E2 and recovery rate of biochar materials
[0102] deal with E2 removal rate Biochar material recovery rate Example 1 92.4%±d 93.8%±e Example 2 90.8%±c 91.2%±c Example 3 91.1%±c 92.7%±d Example 4 88.2%±c 91.5%±c Comparative Example 1 75.7%±a 83.17%±a Comparative Example 2 82.5%±b 85.27%±b Comparative Example 3 80.1%±b 86.30%±b
[0103] As shown in Table 2, the removal rates of Examples 1 to 4 are all higher than those of Comparative Examples 1 to 3, indicating that the β-cyclodextrin magnetically modified biochar material after two ball millings has a better removal effect on E2. From the recovery rate of the biochar material, the recovery rates of the biochar materials of Examples 1 to 4 are all higher than those of Comparative Examples 1 to 3, because the two ball millings improve the problem of pore blockage of the magnetic biochar material and improve the recovery rate of the material. It can be seen that the β-cyclodextrin magnetically modified biochar material of the present invention has a good application prospect in removing E2 from water.
[0104] The adsorption kinetics of E2 on the β-cyclodextrin magnetically modified biochar prepared in Examples 1 to 4, the modified biochar prepared in Comparative Example 1, the β-cyclodextrin magnetically modified biochar prepared in Comparative Example 2, and the β-cyclodextrin magnetically modified biochar prepared in Comparative Example 3 were analyzed, including the following steps: All E2 adsorption experiments were completed in a conical flask, and 100 mg·L -1 NaN3 was added to inhibit microbial degradation. The reaction medium was stirred with a temperature-controlled water bath and an oscillator was used at 180 rpm to keep the adsorbent uniformly dispersed in the water environment. In order to remove oxygen from all solutions, nitrogen was injected for 15 min. Unless otherwise required, the reaction temperature was room temperature. By adding 0.1 mol·L -1HCl or 0.1 mol·L -1 NaOH was used to adjust the initial pH of the solution. The biochar in Examples 1 to 4 and the biochar materials in Comparative Examples 1 to 3 were used for adsorption tests, and the type of estrogen was E2. In the batch experiment of E2, 1 mL of sample was filtered regularly using a 0.22 μm filter membrane. Each experiment was performed in triplicate. The adsorption kinetics of E2 was studied at 25°C. E2 was initially adsorbed at 1000 μg·L -1 The initial concentration of 100 μg / ml was added to the aqueous solution. All flasks were stirred at 180 rpm in the dark. Water samples were extracted after shaking for 10 min, 30 min, 60 min, 120 min, 360 min, 480 min and 720 min and immediately passed through a 0.22 μm filter for estrogen analysis. Adsorption and photodegradation of estrogens by glassware and soluble organic matter were considered to be minimal.
[0105] Kinetic studies give equilibrium times and describe the removal process, which is an important way to determine the mechanism. The results of the kinetic analysis are shown in Table 3.
[0106] Table 3 Kinetic analysis results of biochar removal of E2
[0107]
[0108]
[0109] As shown in Table 3, the adsorption of E2 by the biochar material includes physical adsorption and chemical adsorption. In addition, considering the positive correlation, the recyclable β-cyclodextrin magnetically modified biochar material of the present invention can improve the ability to remove E2.
[0110] It should be noted that when the present invention involves a numerical range, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as those in the embodiments, in order to avoid redundancy, the present invention describes a preferred embodiment. Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they know the basic creative concept. Therefore, the attached claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0111] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A method for preparing β-cyclodextrin magnetically modified biochar, characterized in that: The following steps are involved: The biochar is ball-milled once, and an alkaline solution is added to perform an etching reaction to obtain alkaline biochar; Under a protective gas atmosphere, alkaline biochar was added with Fe 2+ and Fe 3+ In a mixed solution, under alkaline conditions, alkaline biochar is used as a carrier, a co-precipitation reaction is carried out at 80°C to 120°C, and ferroferric oxide particles are loaded in situ to obtain magnetic biochar; Under alkaline conditions, β-cyclodextrin and a cross-linking agent are mixed at room temperature for a grafting reaction, and then the magnetic biochar is added to continue the reaction. The cross-linking agent cross-links with the magnetic biochar, and under the catalytic action of hydroxide ions, the β-cyclodextrin, the cross-linking agent and the magnetic biochar form a ternary epoxide, and the magnetic biochar is modified to obtain modified biochar. The modified biochar is subjected to secondary ball milling. During the secondary ball milling process, the biochar is oxidized by air to activate the biochar, and the solid-phase reaction is promoted to produce chemical bonds, thereby obtaining β-cyclodextrin magnetic modified biochar.
2. The method for preparing β-cyclodextrin magnetically modified biochar according to claim 1, characterized in that: The conditions for the first ball milling are: ball milling at 300 r / min-600 r / min for 60 min, stopping the ball milling for 10 min, and then changing the rotation direction and ball milling at 300 r / min-600 r / min for 60 min; the material-to-ball ratio of the ball milling is 1:10-15.
3. The method for preparing β-cyclodextrin magnetically modified biochar according to claim 1, characterized in that: The conditions for the secondary ball milling are: ball milling at 400 r / min-500 r / min for 60-100 min, stop ball milling for 10 min, then change the rotation direction, ball milling at 500 r / min for 60-100 min, stop ball milling for 10 min, then change the rotation direction, ball milling at 400 r / min-500 r / min for 60 min; the material-to-ball ratio of ball milling is 1:10-15.
4. The method for preparing β-cyclodextrin magnetically modified biochar according to claim 1, characterized in that: The dosage ratio of the magnetic biochar, β-cyclodextrin and cross-linking agent is 1.5g-2g: 15g-20g: 7.5mL-10mL, and the cross-linking agent is epichlorohydrin; the alkaline condition is: adding 0.8mol·L -1 ~1mol·L -1 of NaOH aqueous solution or KOH aqueous solution.
5. The method for preparing β-cyclodextrin magnetically modified biochar according to claim 1, characterized in that: The grafting reaction time is 6 hours to 8 hours, and the continued reaction time is 5 hours.
6. The method for preparing β-cyclodextrin magnetically modified biochar according to claim 1, characterized in that: The mixed solution contains Fe 2+ The molar concentration of Fe is 0.16mol / L~0.27mol / L, 3+ The molar concentration is 0.27 mol / L to 0.37 mol / L, and the solid-liquid ratio of the alkaline biochar to the mixed solution is 4 g to 6 g: 100 mL.
7. The method for preparing β-cyclodextrin magnetically modified biochar according to claim 1, characterized in that: In the process of preparing magnetic biochar, the protective gas is nitrogen, the coprecipitation reaction time is 1h to 2h, and the Fe 2+ is ferric sulfate, the Fe 3+ It is ferric chloride.
8. The method for preparing β-cyclodextrin magnetically modified biochar according to claim 1, characterized in that: In the process of preparing alkaline biochar, the liquid ratio of biochar to alkaline solution is 3g~25g:100mL, and the alkaline solution is 2mol·L -1 ~4mol·L - 1 NaOH aqueous solution or KOH aqueous solution, the etching reaction is 160r·min -1 Stir and etch for 1 h.
9. β-cyclodextrin magnetically modified biochar prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the β-cyclodextrin magnetically modified biochar according to claim 9 as an adsorbent for removing estrogen from water, characterized in that: The amount of β-cyclodextrin magnetically modified biochar added to the water to be treated was 1 mg·L -1 ~10mg·L -1 .
Citation Information
Patent Citations
Preparation and application of novel functional magnetic graphene oxide composite material
CN106423088A
Preparation method of beta-cyclodextrin immobilizing charcoal for absorbing and enduring cadmium ions
CN107185503A
Treatment method of BPA-containing sewage and ball-milling modified magnetic biochar composite material
CN113233573A
Magnetic nano biochar with high adsorption performance as well as preparation method and application of magnetic nano biochar
CN114950356A
Use of functionalised nanosponges for the growth, conservation, protection and disinfection of vegetable organisms
WO2013046165A1