Catalyst for preparing trichlorosilane through silicon tetrachloride hydrogenation and preparation method thereof
The copper-nickel alloy catalyst is supported on the alumina support by sol-gel method, which solves the problems of uneven distribution of active components and unstable support in the cold hydrogenation catalyst, and achieves efficient preparation of trichlorosilicon, which is suitable for industrial applications.
Patent Information
- Application Number
- CN202411024713.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-19
AI Technical Summary
In the preparation of trichlorosilicon, existing cold hydrogenation catalysts have problems of uneven distribution of active components and unstable support, which affects the reaction efficiency and purification of products.
The sol-gel method is used to load the copper-nickel alloy catalyst in situ, doped with alkaline earth metal additives, and supported on an alumina support. The catalyst is prepared by the sol-gel method to ensure the uniform distribution of active components and the stability of the support.
It improves the stability and activity of the catalyst, realizes efficient conversion of the reaction of silicon tetrachloride and hydrogen, simplifies the preparation process, and is suitable for industrial applications.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cold hydrogenation catalysis, and specifically relates to a catalyst used for preparing trichlorosilane by hydrogenating silicon tetrachloride and a preparation method thereof. Background Art
[0002] Energy is the foundation of economic development and social progress. For a long time, due to the increasing depletion of traditional energy and the urgent need to solve environmental problems, finding new energy has become a research hotspot. my country is rich in silicon resources. Polysilicon is the key basic raw material for the electronic information industry and the photovoltaic industry. The polysilicon industry has broad market prospects and development space.
[0003] The main production processes of polysilicon include the modified Siemens process, the silane process and the fluidized bed process, among which the modified Siemens process is the main process for polysilicon production in my country. During the production process, 11-14kg of silicon tetrachloride (STC) will be produced as a by-product for every 1kg of polysilicon produced. The recycling of STC to trichlorosilane (TCS) not only solves the problem of by-products, but also realizes the atomic economy of green chemistry. It is a widely recognized and used treatment method.
[0004] At present, the industry uses two technical routes to hydrogenate STC to produce TCS: thermal hydrogenation and cold hydrogenation. The thermal hydrogenation process uses STC and hydrogen (H2) as raw materials at 1200-1400
[0005] The reaction takes place at 400-600℃ and 0.20-0.40MPa, with a single-pass conversion rate of 15%-20%. The reaction temperature is high and the energy consumption is high.
[0006] STC is hydrogenated to produce TCS at ℃ and 1-4MPa, with a single-pass conversion rate of 15%-35%. The reaction temperature is low, and the energy consumption of thermal hydrogenation is greatly reduced. Copper-based, nickel-based and precious metal catalysts are often used in this reaction process to improve the reaction activity. Commonly used carriers are silicon dioxide (SiO2) and aluminum oxide (Al2O3).
[0007] CN102909006B discloses a catalyst for preparing trichlorosilane by reacting silicon tetrachloride with hydrogen, wherein the active component of the catalyst is nano-platinum particles, and the carrier is self-made silicon dioxide, and the specific preparation method is as follows: first, a mixed reaction of ammonia ethanol mixed liquid and an ethanol solution of tetraethyl silicate is used to obtain a SiO2 carrier. Afterwards, the SiO2 carrier is dispersed in water, chloroplatinate is added, and the reaction is carried out under isopropanol and illumination conditions for more than 10 hours, and then the catalyst is obtained by separation, washing, drying and calcination. Although the catalyst can shorten the time for silicon tetrachloride to react with hydrogen to generate trichlorosilane, making the reaction conditions more gentle, the active component distribution of the catalyst prepared by the method is uneven, and the carrier is easily brought into the subsequent system, affecting the purification process of the subsequent product. Summary of the invention
[0008] The technical problem to be solved by the present invention is to provide a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride and a preparation method thereof in view of the above-mentioned deficiencies in the prior art, thereby overcoming the uneven distribution of active components and unstable carrier in the catalytic material prepared by the impregnation method, using the sol-gel method to in-situ load metal salts to prepare the copper-nickel alloy, and doping alkaline earth metal additives at the same time, so that the prepared catalyst is stable, highly active, and the active components are evenly distributed, thereby providing a preparation method of an efficient cold hydrogenation catalyst suitable for industrial application.
[0009] The technical solution adopted to solve the technical problem of the present invention is to provide a catalyst for preparing trichlorosilane by hydrogenation of silicon tetrachloride, whose molecular formula is Cu x Ni y ·M / Al2O3, where x is 0.2, y is 0.02-0.2 (x, y ratio is (1:1)-(10:1)), M is x Ni y Alkaline earth metal oxides doped in alloys, Cu x Ni y The alloy is loaded on the carrier Al2O3.
[0010] Preferably, the catalyst used for preparing trichlorosilane by hydrogenation of silicon tetrachloride has a specific surface area of 300 m 2 In the present invention, the specific surface area is measured by nitrogen physical adsorption-desorption experiment.
[0011] The present invention also provides a method for preparing a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride, comprising the following steps:
[0012] (1) dissolving a copper salt and a nickel salt in a first solvent to obtain a first solution;
[0013] (2) dissolving an aluminum salt and an alkaline earth metal salt in a second solvent to obtain a second solution;
[0014] (3) adding the second solution in step (2) to the first solution in step (1), adjusting the pH value, and stirring to obtain a sol;
[0015] (4) adding a gelling agent solution dropwise to the sol obtained in step (3), heating and stirring until a gel is formed;
[0016] (5) Drying, calcining and reducing the gel obtained in step (4) to finally obtain a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride, which is an alumina carrier-supported copper-nickel alloy doped with alkaline earth metal oxide.
[0017] Preferably, in step (1), the first solvent comprises water and ethanol, and the volume ratio of water to ethanol is (1-3): (1-2);
[0018] In the step (2), the second solvent includes water and ethanol, and the volume ratio of water to ethanol is (1-3): (1-2).
[0019] Preferably, the copper salt in step (1) is one or more of copper sulfate, copper nitrate, copper chloride, and copper acetate; more preferably, the copper salt in step (1) is copper nitrate;
[0020] The nickel salt in step (1) is one or more of nickel nitrate, nickel acetate, nickel chloride, and nickel sulfate. More preferably, the nickel salt in step (1) is nickel nitrate.
[0021] Preferably, the molar ratio of the copper salt to the nickel salt in step (1) is (1:1)-(10:1). More preferably, the molar ratio of the copper salt to the nickel salt in step (1) is (8:1)-(3:1).
[0022] Preferably, the aluminum salt in step (2) is an inorganic aluminum salt, and the aluminum salt is one or more of aluminum nitrate, aluminum chloride, and aluminum sulfate. More preferably, the aluminum salt in step (2) is an inorganic aluminum salt, and the aluminum salt is aluminum nitrate.
[0023] The alkaline earth metal salt in step (2) is one or more of magnesium nitrate, calcium nitrate, strontium nitrate and barium nitrate. More preferably, the alkaline earth metal salt in step (2) is barium nitrate.
[0024] Preferably, the molar ratio of the aluminum salt and the alkaline earth metal salt added in step (2) is (1:1)-(10:1). More preferably, the molar ratio of the aluminum salt and the alkaline earth metal salt added in step (2) is (1:1)-(3:1).
[0025] Preferably, the ratio of the sum of the amounts of the aluminum salt and the alkaline earth metal salt in step (2) to the sum of the amounts of the copper salt and the nickel salt in step (1) is (1-7):(1-6).
[0026] Preferably, the volume ratio of the first solution to the second solution is (1:1)-(1:4). More preferably, the volume ratio of the first solution to the second solution is (1:1)-(1:2).
[0027] Preferably, in step (3), the pH value range is 8-10, and the pH adjuster is one or more of ethylenediamine, ethanolamine, sodium hydroxide, sodium bicarbonate, and ammonia. More preferably, in step (3), the pH value range is 8.0, and the pH adjuster is ammonia.
[0028] Preferably, the gelling aid in step (4) is any one or more of modified cellulose, citric acid, propylene oxide, butylene oxide, and pentane oxide.
[0029] Preferably, the modified cellulose in step (4) is one or more of carboxymethyl cellulose, methyl cellulose, and cellulose acetate. More preferably, the modified cellulose in step (4) is carboxymethyl cellulose.
[0030] Preferably, the mass content of the gelling aid in the gelling aid solution in step (4) is 2 mas%-10 mas%. More preferably, the mass content of the gelling aid in the gelling aid solution in step (4) is 4 mas%.
[0031] Preferably, the heating temperature in step (4) is 70-100° C. More preferably, the heating temperature in step (4) is 80° C.
[0032] Preferably, the drying condition in step (5) is 60-150°C for 10-24 hours. More preferably, the drying condition in step (5) is 120°C for 12 hours.
[0033] Preferably, the calcination conditions in step (5) are first calcined at 100-200°C for 0.5-1.5h, then calcined at 500-1000°C for 2-5h. More preferably, the calcination conditions in step (5) are first calcined at 200°C for 0.5h, then calcined at 550°C for 2h.
[0034] Preferably, the catalyst particle size is 0.25-0.83 mm; more preferably, the catalyst particle size is 0.38-0.55 mm.
[0035] Preferably, the reduction condition in step (5) is at 400-600° C. in a hydrogen atmosphere for 1-5 h. More preferably, the reduction condition in step (5) is at 500° C. in a hydrogen atmosphere for 2 h.
[0036] The catalyst used for preparing trichlorosilane by hydrogenating silicon tetrachloride in the present invention and the preparation method thereof have the following advantages:
[0037] (1) Alumina is used as a catalyst carrier. Alumina with a large specific surface area has a developed pore structure, which can make the loaded active components highly dispersed, thereby improving the utilization rate of the metal.
[0038] (2) The copper-nickel alloy catalyst is prepared by in-situ loading of metal salts using the sol-gel method. The active component and the carrier are stably combined, and the molding of the carrier and the loading of the active component are integrated, which shortens the catalyst preparation process, simplifies the process flow, and is easy to implement.
[0039] (3) The copper atoms and nickel atoms in the catalyst can produce a synergistic effect, and the catalyst has good catalytic activity.
[0040] (4) During the calcination process, alkaline earth metals and active components form composite oxides, which prevent the migration of active components, inhibit the agglomeration of active components, and improve the dispersion of active components. DETAILED DESCRIPTION
[0041] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with specific implementation methods.
[0042] Example 1
[0043] This embodiment provides a catalyst for preparing trichlorosilane by hydrogenation of silicon tetrachloride, the molecular formula of which is Cu x Ni y ·M / Al2O3, where x is 0.2, y is 0.02-0.2 (x, y ratio is (1:1)-(10:1)), M is x Ni y Alkaline earth metal oxides doped in alloys, Cu x Ni y The alloy is loaded on the carrier Al2O3.
[0044] This embodiment also provides a method for preparing the catalyst used for preparing trichlorosilane by hydrogenating silicon tetrachloride, comprising the following steps:
[0045] (1) dissolving a copper salt and a nickel salt in a first solvent to obtain a first solution;
[0046] (2) dissolving an aluminum salt and an alkaline earth metal salt in a second solvent to obtain a second solution;
[0047] (3) adding the second solution in step (2) to the first solution in step (1), adjusting the pH value, and stirring to obtain a sol;
[0048] (4) adding a gelling agent solution dropwise to the sol obtained in step (3), heating and stirring until a gel is formed;
[0049] (5) Drying, calcining and reducing the gel obtained in step (4) to finally obtain a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride, which is an alkaline earth metal oxide doped with copper-nickel alloy supported by an alumina carrier.
[0050] The catalyst used for preparing trichlorosilane by hydrogenating silicon tetrachloride in this embodiment and its preparation method have the following advantages:
[0051] (1) Alumina is used as a catalyst carrier. Alumina with a large specific surface area has a developed pore structure, which can make the loaded active components highly dispersed, thereby improving the utilization rate of the metal.
[0052] (2) The copper-nickel alloy catalyst is prepared by in-situ loading of metal salts using the sol-gel method. The active component and the carrier are stably combined, and the molding of the carrier and the loading of the active component are integrated, which shortens the catalyst preparation process, simplifies the process flow, and is easy to implement.
[0053] (3) The copper atoms and nickel atoms in the catalyst can produce a synergistic effect, and the catalyst has good catalytic activity.
[0054] (4) During the calcination process, alkaline earth metals and active components form composite oxides, which prevent the migration of active components, inhibit the agglomeration of active components, and improve the dispersion of active components.
[0055] Example 2
[0056] This embodiment provides a catalyst for preparing trichlorosilane by hydrogenation of silicon tetrachloride, the molecular formula of which is Cu x Ni y ·M / Al2O3, where x is 0.2, y is 0.02-0.2 (x, y ratio is (1:1)-(10:1)), M is x Ni y Alkaline earth metal oxides doped in alloys, Cu x Ni y The alloy is loaded on the carrier Al2O3.
[0057] Preferably, the catalyst used for preparing trichlorosilane by hydrogenation of silicon tetrachloride has a specific surface area of 300 m 2In this embodiment, the specific surface area is measured by nitrogen physical adsorption-desorption experiment.
[0058] This embodiment also provides a method for preparing the catalyst used for preparing trichlorosilane by hydrogenating silicon tetrachloride, comprising the following steps:
[0059] (1) dissolving a copper salt and a nickel salt in a first solvent to obtain a first solution;
[0060] (2) dissolving an aluminum salt and an alkaline earth metal salt in a second solvent to obtain a second solution;
[0061] (3) adding the second solution in step (2) dropwise into the first solution in step (1), adjusting the pH value, and stirring at room temperature to obtain a sol;
[0062] (4) adding a gelling agent solution dropwise to the sol obtained in step (3), heating and stirring until a gel is formed;
[0063] (5) drying, calcining, screening and reducing the gel obtained in step (4), wherein the calcination process obtains an alumina carrier, and the reduction process obtains a copper-nickel alloy doped with an alkaline earth metal oxide, and finally obtains a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride, which is an alumina carrier loaded with a copper-nickel alloy doped with an alkaline earth metal oxide.
[0064] Preferably, in step (1), the first solvent comprises deionized water and anhydrous ethanol, and the volume ratio of deionized water to anhydrous ethanol is (1-3): (1-2);
[0065] In the step (2), the second solvent includes deionized water and anhydrous ethanol, and the volume ratio of deionized water to anhydrous ethanol is (1-3): (1-2).
[0066] Preferably, the copper salt in step (1) is one or more of copper sulfate, copper nitrate, copper chloride, and copper acetate; more preferably, the copper salt in step (1) is copper nitrate;
[0067] The nickel salt in step (1) is one or more of nickel nitrate, nickel acetate, nickel chloride, and nickel sulfate. More preferably, the nickel salt in step (1) is nickel nitrate.
[0068] Preferably, the molar ratio of the copper salt to the nickel salt in step (1) is (1:1)-(10:1). More preferably, the molar ratio of the copper salt to the nickel salt in step (1) is (8:1)-(3:1).
[0069] Preferably, the aluminum salt in step (2) is an inorganic aluminum salt, and the aluminum salt is one or more of aluminum nitrate, aluminum chloride, and aluminum sulfate. More preferably, the aluminum salt in step (2) is an inorganic aluminum salt, and the aluminum salt is aluminum nitrate.
[0070] The alkaline earth metal salt in step (2) is one or more of magnesium nitrate, calcium nitrate, strontium nitrate and barium nitrate. More preferably, the alkaline earth metal salt in step (2) is barium nitrate.
[0071] Preferably, the molar ratio of the aluminum salt and the alkaline earth metal salt added in step (2) is (1:1)-(10:1). More preferably, the molar ratio of the aluminum salt and the alkaline earth metal salt added in step (2) is (1:1)-(3:1).
[0072] Preferably, the ratio of the sum of the amounts of the aluminum salt and the alkaline earth metal salt in step (2) to the sum of the amounts of the copper salt and the nickel salt in step (1) is (1-7):(1-6).
[0073] Preferably, the volume ratio of the first solution to the second solution is (1:1)-(1:4). More preferably, the volume ratio of the first solution to the second solution is (1:1)-(1:2).
[0074] Preferably, in step (3), the pH value range is 8-10, and the pH adjuster is one or more of ethylenediamine, ethanolamine, sodium hydroxide, sodium bicarbonate, and ammonia. More preferably, in step (3), the pH value range is 8.0, and the pH adjuster is ammonia.
[0075] Preferably, the gelling aid in step (4) is any one or more of modified cellulose, citric acid, propylene oxide, butylene oxide, and pentane oxide.
[0076] Preferably, the modified cellulose in step (4) is one or more of carboxymethyl cellulose, methyl cellulose, and cellulose acetate. More preferably, the modified cellulose in step (4) is carboxymethyl cellulose.
[0077] Preferably, the mass content of the gelling aid in the gelling aid solution in step (4) is 2 mas%-10 mas%. More preferably, the mass content of the gelling aid in the gelling aid solution in step (4) is 4 mas%.
[0078] Preferably, the heating temperature in step (4) is 70-100° C. More preferably, the heating temperature in step (4) is 80° C.
[0079] Preferably, the drying condition in step (5) is 60-150°C for 10-24 hours. More preferably, the drying condition in step (5) is 120°C for 12 hours.
[0080] Preferably, the calcination conditions in step (5) are first calcined at 100-200°C for 0.5-1.5h, then calcined at 500-1000°C for 2-5h. More preferably, the calcination conditions in step (5) are first calcined at 200°C for 0.5h, then calcined at 550°C for 2h.
[0081] Preferably, the catalyst particle size is 0.25-0.83 mm; more preferably, the catalyst particle size is 0.38-0.55 mm.
[0082] Preferably, the reduction condition in step (5) is at 400-600° C. in a hydrogen atmosphere for 1-5 h. More preferably, the reduction condition in step (5) is at 500° C. in a hydrogen atmosphere for 2 h.
[0083] Specifically, this embodiment provides a method for preparing the catalyst used for preparing trichlorosilane by hydrogenating silicon tetrachloride, comprising the following steps:
[0084] (1) 60 mL of deionized water and 40 mL of anhydrous ethanol were uniformly mixed, and then 48.3 g of Cu(NO3)2·3H2O and 5.8 g of Ni(NO3)2·6H2O were weighed and dissolved in the mixed solution. The mixed solution was placed in a three-necked flask and stirred at room temperature for 0.5 h until the solution became clear and transparent.
[0085] (2) Weigh 64 g of Al(NO3)3·9H2O and 4.4 g of Ba(NO3)2 and dissolve them in a mixed solution of 60 mL of deionized water and 40 mL of anhydrous ethanol. Stir evenly at room temperature.
[0086] (3) Then, the mixture was added dropwise into the three-necked flask containing the metal salt solution while stirring, the pH of the solution was adjusted to 8.0 with aqueous ammonia, and stirred at room temperature for 4 h to form a sol.
[0087] (4) 100 mL of deionized water was placed in a beaker and heated to 80°C. Then, 2 g of carboxymethyl cellulose was added while stirring and waited for complete dispersion to obtain a carboxymethyl cellulose solution. Finally, 10 mL of the carboxymethyl cellulose solution was added dropwise to the three-necked flask while stirring. After the addition was completed, the solution was heated in an 80°C water bath with magnetic stirring until the solution gradually formed a gel, and then allowed to cool naturally.
[0088] (5) The obtained gel was placed in a constant temperature drying oven at 120°C for 12 hours, then ground into powder using an agate mortar, placed in a crucible and calcined in a muffle furnace: the temperature was raised to 200°C at a heating rate of 2°C / min, maintained for 0.5 hours, and then continued to be raised to 550°C at a heating rate of 2°C / min, maintained for 2 hours, and the calcination was completed. The catalyst was then tableted on a powder tablet press, crushed and sieved to screen out catalyst particles of 0.38-0.55 mm. After screening, 8 g of the catalyst was placed in a tube furnace and reduced at 500°C for 2 h in a H2 atmosphere to obtain the catalyst A of this embodiment. The XRD spectrum analysis of the catalyst A in this embodiment shows that the diffraction peaks at 2θ=43.3, 50.4 and 74.1° correspond to the Cu (111), (200) and (220) crystal planes, the diffraction peaks at 2θ=44.5, 51.8 and 76.4° correspond to the Ni (111), (200) and (220) crystal planes, and the diffraction peaks at 2θ=37.4, 45.8 and 67.3° correspond to the Al2O3 (311), (400), (440) crystal planes. The specific surface area of the catalyst is shown in Table 1, and the evaluation results of the catalyst are shown in Table 2.
[0089] The catalyst in this embodiment is stable and the active components are evenly distributed, which is crucial for the cold hydrogenation process.
[0090] The catalyst used for preparing trichlorosilane by hydrogenating silicon tetrachloride in this embodiment and its preparation method have the following advantages:
[0091] (1) Alumina is used as a catalyst carrier. Alumina with a large specific surface area has a developed pore structure, which can make the loaded active components highly dispersed, thereby improving the utilization rate of the metal.
[0092] (2) The copper-nickel alloy catalyst is prepared by in-situ loading of metal salts using the sol-gel method. The active component and the carrier are stably combined, and the molding of the carrier and the loading of the active component are integrated, which shortens the catalyst preparation process, simplifies the process flow, and is easy to implement.
[0093] (3) The copper atoms and nickel atoms in the catalyst can produce a synergistic effect, and the catalyst has good catalytic activity.
[0094] (4) The modified cellulose contains a large number of hydroxyl groups, which can form intermolecular hydrogen bonds with the hydrolysis product hydroxyaluminum oxide, thereby enhancing the interaction between the modified cellulose and the hydrolysis product and facilitating the formation of a stable gel network structure.
[0095] (5) During the calcination process, alkaline earth metals and active components form composite oxides, which prevent the migration of active components, inhibit the agglomeration of active components, and improve the dispersion of active components.
[0096] (6) The catalyst was heat treated by a staged calcination method to inhibit the sintering of catalyst particles.
[0097] Example 3
[0098] The preparation process is the same as in Example 1, except that the amount of Ni(NO3)2·6H2O added is changed to 7.3 g, the added Ba(NO3)2 is changed to Sr(NO3)2, the added amount is 3.6 g, the pH adjuster is ethylenediamine, and the pH is adjusted to 9.0 to prepare Catalyst B of this example. The specific surface area of the catalyst is shown in Table 1, and the evaluation results of the catalyst are shown in Table 2.
[0099] This embodiment also provides a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride, which is prepared by the above method.
[0100] Example 4
[0101] The preparation process is the same as in Example 1, except that the amount of Ni(NO3)2·6H2O added is changed to 9.7 g, the added Ba(NO3)2 is changed to Mg(NO3)2·6H2O, and the added amount is 5.4 g. The concentration of the carboxymethyl cellulose solution is changed to 4 mas%, and the pH adjuster is ethylenediamine, and the pH is adjusted to 10.0 to prepare Catalyst C of this example. The specific surface area of the catalyst is shown in Table 1, and the evaluation results of the catalyst are shown in Table 2.
[0102] This embodiment also provides a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride, which is prepared by the above method.
[0103] Example 5
[0104] The preparation process is the same as in Example 1, except that the added Cu(NO3)2·3H2O is changed to Cu(CH3COO)2·H2O, and the added amount is 39.9 g; the added Ni(NO3)2·6H2O is changed to Ni(CH3COO)2·4H2O, and the added amount is 8.3 g; the added Ba(NO3)2 is changed to Ca(NO3)2·4H2O, and the added amount is 5 g; the added carboxymethyl cellulose is changed to methyl cellulose, and the concentration is 6 mas%, to prepare Catalyst D of this example. The specific surface area of the catalyst is shown in Table 1, and the evaluation results of the catalyst are shown in Table 2.
[0105] This embodiment also provides a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride, which is prepared by the above method.
[0106] Example 6
[0107] The preparation process is the same as that in Example 1, except that the added Cu(NO3)2·3H2O is replaced by CuCl2·2H2O in an amount of 34.1 g, the added Ni(NO3)2·6H2O is replaced by NiCl2·6H2O in an amount of 15.8 g, the added carboxymethyl cellulose is replaced by cellulose acetate in a concentration of 6 mas%, and the calcination conditions of the catalyst are changed to heating the temperature to 150°C at a heating rate of 2°C / min, maintaining for 0.5 h, and then continuing to heating the temperature to 700°C at a heating rate of 2°C / min, maintaining for 4 h, to prepare Catalyst E of this example. The specific surface area of the catalyst is shown in Table 1, and the evaluation results of the catalyst are shown in Table 2.
[0108] This embodiment also provides a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride, which is prepared by the above method.
[0109] Example 7
[0110] The preparation process is the same as in Example 1, except that the added Al(NO3)3·9H2O is changed to AlCl3·6H2O, and the added amount is 41.0 g, the added amount of Ba(NO3)2 is changed to 7.4 g, the concentration of the carboxymethyl cellulose solution is changed to 10 mas%, and the roasting conditions are changed to heating the temperature to 100°C at a heating rate of 2°C / min, maintaining for 2 h, and then heating the temperature to 800°C at a heating rate of 2°C / min, maintaining for 5 h, to prepare Catalyst F of this example. The specific surface area of the catalyst is shown in Table 1, and the evaluation results of the catalyst are shown in Table 2.
[0111] This embodiment also provides a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride, which is prepared by the above method.
[0112] Example 8
[0113] The preparation process was the same as in Example 1, except that the screening range of the catalyst particles was changed to 0.25-0.27 mm to prepare Catalyst G of this Example. The specific surface area of the catalyst is shown in Table 1, and the evaluation results of the catalyst are shown in Table 2.
[0114] This embodiment also provides a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride, which is prepared by the above method.
[0115] Example 9
[0116] The preparation process was the same as in Example 1, except that the reduction condition was changed to reduction at 400° C. for 4 h to prepare Catalyst H of this Example. The specific surface area of the catalyst is shown in Table 1, and the evaluation results of the catalyst are shown in Table 2.
[0117] This embodiment also provides a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride, which is prepared by the above method.
[0118] Comparative Example 1
[0119] The preparation process was the same as in Example 1, except that no nickel salt was added during the preparation process to obtain comparative catalyst I. The specific surface area of the catalyst is shown in Table 1, and the catalyst evaluation results are shown in Table 2.
[0120] Comparative Example 2
[0121] Weigh 48.3g Cu(NO3)2·3H2O and 5.8g Ni(NO3)2·6H2O and dissolve them in 100mL of deionized water, then weigh 20g of alumina carrier and place it in the above mixed solution and stir evenly, and let it stand at room temperature for 12h. Then filter to obtain a solid, and place the solid in a constant temperature drying oven and dry it at 120°C for 12h. Then use an agate mortar to grind it into powder and place it in a crucible and roast it in a muffle furnace: heat it to 200°C at a heating rate of 2°C / min, keep it for 0.5h, continue to heat it to 550°C at a heating rate of 2°C / min, keep it for 2h, and the roasting is completed. Then, the catalyst is pressed on a powder tablet press, crushed and sieved, and catalyst particles of 0.38-0.55mm are screened out. After screening, take 8g of the catalyst and place it in a tubular furnace and reduce it at 500°C in a H2 atmosphere for 2h to obtain Catalyst J of this embodiment.
[0122] The specific surface areas of the catalysts in Examples 2 to 9 and Comparative Examples 1 to 2 are shown in Table 1, and the evaluation results of the catalysts are shown in Table 2.
[0123] Table 1 Specific surface area of catalyst
[0124] Catalyst No. catalyst <![CDATA[Specific surface area (m 2 / g)]]> A <![CDATA[Cu 0.2 It is 0.02 ·BaO / Al2O3]]> 341 B <h2 style=";text-align:left;direction:ltr"><![CDATA[Cu <h2 style=";text-align:left;direction:ltr"> 0.2 <h2 style=";text-align:left;direction:ltr"> Ni<h2 style=";text-align:left;direction:ltr"> 0.025 <h2 style=";text-align:left;direction:ltr"> SrO / Al2O3<h2 style=";text-align:left;direction:ltr"> 337 C <![CDATA[Cu 0.2 Be 0.033 ·MgO / Al2O3]]> 321 D <![CDATA[Cu 0.2 Ni 0.033 ·CaO / Al2O3]]> 320 E <![CDATA[Cu 0.2 It is 0.066 ·BaO / Al2O3]]> 317 F <![CDATA[Cu 0.2 It is 0.02 ·BaO / Al2O3]]> 323 G <![CDATA[Cu 0.2 It is 0.02 ·BaO / Al2O3]]> 341 H <![CDATA[Cu 0.2 It is 0.02 ·BaO / Al2O3]]> 327 I <![CDATA[Cu 0.2 ·BaO / Al2O3]]> 349 J <h2 style=";text-align:left;direction:ltr"><![CDATA[Cu <h2 style=";text-align:left;direction:ltr"> 0.2 <h2 style=";text-align:left;direction:ltr"> Ni<h2 style=";text-align:left;direction:ltr"> 0.02 <h2 style=";text-align:left;direction:ltr"> / Al2O3]]><h2 style=";text-align:left;direction:ltr"> 343
[0125] The activity of the catalyst was evaluated using a fixed bed evaluation device, with 8 g of catalyst and 80 g of silicon powder, a reaction pressure of 2.1 MPa, a H2 / SiC14 (molar ratio) of 20, and a gas hourly space velocity of 24000 h -1 The reaction temperature was 550°C, silicon tetrachloride was hydrogenated to prepare trichlorosilane, and the conversion rate of silicon tetrachloride to trichlorosilane was tested. The evaluation results are shown in Table 2.
[0126] Table 2 Evaluation results of catalysts
[0127] Catalyst No. A B C D E F G H I J Conversion rate (%) 30.8 31.4 31.8 31.7 32.6 31.2 30.9 29.9 28.1 24.3
[0128] Example 10
[0129] This embodiment provides a method for preparing a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride, which differs from the method in Example 2 in that:
[0130] In the step (1), the volume ratio of water to ethanol in the first solvent is 1:1;
[0131] In the step (2), the volume ratio of water to ethanol in the second solvent is 1:1.
[0132] The copper salts described in step (1) are copper sulfate and copper nitrate, with a mass ratio of 1:1.
[0133] The nickel salt in step (1) is nickel sulfate.
[0134] In step (1), the molar ratio of the copper salt to the nickel salt is 1:1.
[0135] The aluminum salt in step (2) is aluminum sulfate. The alkaline earth metal salt is strontium nitrate and barium nitrate.
[0136] The molar ratio of the aluminum salt and the alkaline earth metal salt added in step (2) is 1:1.
[0137] The ratio of the sum of the amounts of the aluminum salt and the alkaline earth metal salt in step (2) to the sum of the amounts of the copper salt and the nickel salt in step (1) is 7:3.
[0138] The volume ratio of the first solution to the second solution is 1:1.
[0139] The pH regulator in step (3) is ethanolamine.
[0140] In step (4), the gelling aids are cellulose acetate and methyl cellulose, and the mass ratio of the two is 4:1.
[0141] The heating temperature in step (4) is 70°C.
[0142] The drying condition in step (5) is drying at 60° C. for 24 hours.
[0143] The calcination conditions in step (5) are first calcining at 100° C. for 1.5 h and then calcining at 1000° C. for 5 h.
[0144] The reduction condition in step (5) is at 400° C. in a hydrogen atmosphere for 5 hours.
[0145] This embodiment also provides a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride, which is prepared by the above method.
[0146] Embodiment 11
[0147] This embodiment provides a method for preparing a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride, which differs from the method in Example 2 in that:
[0148] In the step (1), the volume ratio of water to ethanol in the first solvent is 2:1.5;
[0149] The volume ratio of water to ethanol in the second solvent in step (2) is 3:2.
[0150] The copper salt in step (1) is copper chloride.
[0151] The nickel salt in step (1) is nickel acetate and nickel chloride, and the mass ratio of the nickel salt and nickel chloride is 2:1.
[0152] In step (1), the molar ratio of copper salt to nickel salt is 5:1.
[0153] The aluminum salt in step (2) is aluminum sulfate and aluminum chloride, and the mass ratio of the two is 1:4. The alkaline earth metal salt is strontium nitrate.
[0154] The molar ratio of the aluminum salt and the alkaline earth metal salt added in step (2) is 10:1.
[0155] The ratio of the sum of the amounts of the aluminum salt and the alkaline earth metal salt in step (2) to the sum of the amounts of the copper salt and the nickel salt in step (1) is 1:6.
[0156] The volume ratio of the first solution to the second solution is 1:2.
[0157] The pH regulator in step (3) is sodium hydroxide.
[0158] In step (4), the gelling aid is citric acid.
[0159] The heating temperature in step (4) is 100°C.
[0160] The drying condition in step (5) is drying at 150° C. for 10 hours.
[0161] The calcination conditions in step (5) are first calcining at 150° C. for 2 h and then calcining at 500° C. for 3.5 h.
[0162] The reduction condition in step (5) is at 480° C. in a hydrogen atmosphere for 1 h.
[0163] This embodiment also provides a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride, which is prepared by the above method.
[0164] Example 12
[0165] This embodiment provides a method for preparing a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride, which differs from the method in Example 2 in that:
[0166] In the step (1), the volume ratio of water to ethanol in the first solvent is 3:2;
[0167] The volume ratio of water to ethanol in the second solvent in step (2) is 2:1.5.
[0168] The copper salts in step (1) are copper sulfate and copper acetate, and the mass ratio of the copper salts is 1:1.
[0170] The nickel salt in step (1) is nickel chloride.
[0171] In step (1), the molar ratio of copper salt to nickel salt is 10:1.
[0172] The aluminum salt in step (2) is aluminum chloride. The alkaline earth metal salt is magnesium nitrate.
[0173] The molar ratio of the aluminum salt and the alkaline earth metal salt added in step (2) is 3:1.
[0174] The ratio of the sum of the amounts of the aluminum salt and the alkaline earth metal salt in step (2) to the sum of the amounts of the copper salt and the nickel salt in step (1) is 3:1.
[0175] The volume ratio of the first solution to the second solution is 1:4.
[0176] In the step (3), the pH regulator is sodium hydroxide and sodium bicarbonate, and the mass ratio of the two is 3:1.
[0177] In step (4), the gelling aids are propylene oxide, butylene oxide and pentyl oxide, and the mass ratio of the three is 1:1:1.
[0178] The heating temperature in step (4) is 90°C.
[0179] The drying condition in step (5) is drying at 110° C. for 18 hours.
[0180] The calcination conditions in step (5) are first calcining at 200° C. for 0.5 h and then calcining at 800° C. for 2 h.
[0181] The reduction condition in step (5) is at 600° C. in a hydrogen atmosphere for 3 h.
[0182] This embodiment also provides a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride, which is prepared by the above method.
[0183] The specific surface areas of the catalysts in Examples 10 to 12 are shown in Table 3, and the evaluation results of the catalysts are shown in Table 4.
[0184] Table 3 Specific surface area of catalyst
[0185]
[0186] The activity of the catalyst was evaluated using a fixed bed evaluation device, with 8 g of catalyst and 80 g of silicon powder, a reaction pressure of 2.1 MPa, a H2 / SiC14 (molar ratio) of 20, and a gas hourly space velocity of 24000 h-1 The reaction temperature was 550°C, silicon tetrachloride was hydrogenated to prepare trichlorosilane, and the conversion rate of silicon tetrachloride to trichlorosilane was tested. The evaluation results are shown in Table 2.
[0187] Table 4 Evaluation results of catalysts
[0188] Catalyst No. Example 10 Embodiment 11 Example 12 Conversion rate (%) 32.0 31.5 30.6
[0189] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.
Claims
1. A catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride, characterized in that: Its molecular formula is Cu x Ni y ·M / Al2O3, where x is 0.2, y is 0.02-0.2, and M is x Ni y Alkaline earth metal oxides doped in alloys, Cu x Ni y The alloy is loaded on the carrier Al2O3.
2. The catalyst used for preparing trichlorosilane by hydrogenating silicon tetrachloride according to claim 1, characterized in that: Its specific surface area>300m 2 / g.
3. A method for preparing a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride according to any one of claims 1 to 2, characterized in that: The following steps are involved: (1) dissolving a copper salt and a nickel salt in a first solvent to obtain a first solution; (2) dissolving an aluminum salt and an alkaline earth metal salt in a second solvent to obtain a second solution; (3) adding the second solution in step (2) to the first solution in step (1), adjusting the pH value, and stirring to obtain a sol; (4) adding a gelling agent solution dropwise to the sol obtained in step (3), heating and stirring until a gel is formed; (5) Drying, calcining and reducing the gel obtained in step (4) to finally obtain a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride, which is an alkaline earth metal oxide doped with copper-nickel alloy supported by an alumina carrier.
4. The method for preparing a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride according to claim 3, characterized in that: In step (1), the first solvent includes water and ethanol, and the volume ratio of water to ethanol is (1-3): (1-2); In the step (2), the second solvent includes water and ethanol, and the volume ratio of water to ethanol is (1-3): (1-2).
5. The method for preparing a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride according to claim 3, characterized in that: The copper salt in step (1) is one or more of copper sulfate, copper nitrate, copper chloride and copper acetate; The nickel salt in step (1) is one or more of nickel nitrate, nickel acetate, nickel chloride and nickel sulfate.
6. The method for preparing a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride according to claim 3, characterized in that: In step (1), the molar ratio of copper salt to nickel salt is (1:1)-(10:1).
7. The method for preparing a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride according to claim 3, characterized in that: The aluminum salt in step (2) is an inorganic aluminum salt, and the aluminum salt is one or more of aluminum nitrate, aluminum chloride, and aluminum sulfate; The alkaline earth metal salt in step (2) is one or more of magnesium nitrate, calcium nitrate, strontium nitrate and barium nitrate.
8. The method for preparing a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride according to claim 3, characterized in that: The molar ratio of the aluminum salt and the alkaline earth metal salt added in step (2) is (1:1)-(10:1).
9. The method for preparing a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride according to claim 3, characterized in that: The ratio of the sum of the amounts of the aluminum salt and the alkaline earth metal salt in step (2) to the sum of the amounts of the copper salt and the nickel salt in step (1) is (1-7):(1-6).
10. The method for preparing a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride according to claim 3, characterized in that: In the step (3), the pH value range is 8-10, and the pH adjuster is one or more of ethylenediamine, ethanolamine, sodium hydroxide, sodium bicarbonate, and ammonia water.
11. The method for preparing a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride according to claim 3, characterized in that: In step (4), the gelling aid is any one or more of modified cellulose, citric acid, propylene oxide, butylene oxide and pentane oxide.
12. The method for preparing a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride according to claim 11, characterized in that: In step (4), the modified cellulose is one or more of carboxymethyl cellulose, methyl cellulose and cellulose acetate.
13. The method for preparing a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride according to claim 3, characterized in that: The mass content of the gelling agent in the gelling agent solution in step (4) is 2mas%-10mas%.
14. The method for preparing a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride according to claim 3, characterized in that: The heating temperature in step (4) is 70-100°C.
15. The method for preparing a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride according to any one of claims 3 to 14, characterized in that: The drying condition in step (5) is 60-150° C. for 10-24 hours.
16. The method for preparing a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride according to any one of claims 3 to 14, characterized in that: The calcination conditions in step (5) are first calcining at 100-200°C for 0.5-1.5h, and then calcining at 500-1000°C for 2-5h.
17. The method for preparing a catalyst for preparing trichlorosilane by hydrogenating silicon tetrachloride according to any one of claims 3 to 14, characterized in that: The reduction conditions in step (5) are at 400-600° C. in a hydrogen atmosphere for 1-5 hours.
Citation Information
Patent Citations
Method for preparing trichlorosilane by hydrogenating silicon tetrachloride
CN102633263A
Catalyst for preparation of trichlorosilicon by cold hydrogenation of silicon tetrachloride, and preparation method of catalyst
CN108855091A
Catalyst used for hydrogenation of silicon tetrachloride to prepare trichlorosilane and preparation method thereof
CN109718781A
Nickel-copper catalyst, preparation method thereof and method for preparing methyl isobutyl alcohol
CN112547069A
Method for synthesizing trichlorosilane from silicon tetrachloride
CN115845910A