Preparation method of ZnFe2O4 / TiO2 composite material and application of ZnFe2O4 / TiO2 composite material in degradation of patulin
The preparation of ZnFe2O4/TiO2 composite material by solvent thermal synthesis method solves the problems of nutrient loss and complex operation in penicillin removal, improves photocatalytic activity and recovery, and achieves efficient and safe penicillin degradation effect.
Patent Information
- Application Number
- CN202411233439.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-19
AI Technical Summary
The prior art has problems such as nutrient loss, complex operation, and inconsistent microbial detoxification effects when removing penicillin. The photocatalytic activity of TiO2 is insufficient and difficult to recover, which limits its industrial application.
The ZnFe2O4/TiO2 composite material was prepared by solvent thermal synthesis. By changing the proportion of a single material, the photocatalytic efficiency was improved, and the magnetic properties were used to facilitate recovery and removal.
It realizes efficient, safe and secondary pollution-free photocatalytic degradation of penicillin, improves photocatalytic activity and visible light utilization, simplifies the process flow, reduces costs, and solves the problem of difficulty in recycling nanomaterials.
Smart Images

Figure CN118976500A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of photocatalytic degradation of fungal toxins, and specifically relates to the preparation of a ZnFe2O4 / TiO2 composite material and the application of the composite material in the degradation of patulin. Background Art
[0002] Patulin is a genotoxic secondary metabolite produced by various fungi such as Penicillium expansum, Penicillium patulin, and Aspergillus. It is also called patulin and is a neurotoxin that has strong toxic effects on animal cells and tissues. Animal experiments and cell toxicology tests have shown that patulin has multiple hazards such as carcinogenicity, mutagenicity, immunotoxicity, embryotoxicity, and reproductive toxicity. It is classified as a Class III suspected carcinogen by the International Agency for Research on Cancer. Long-term consumption of products containing patulin can cause serious damage to human body functions and may cause symptoms such as vomiting, nausea, convulsions, and coma.
[0003] Patulin mainly contaminates fruits and their products, especially apples, hawthorns, pears, tomatoes, etc. At present, people have developed a variety of methods to remove patulin from food. Traditional methods include physical methods, chemical methods, and biological methods. Commonly used physical detoxification methods include heating, adsorption, washing, sorting, etc.; chemical methods refer to the use of chemical reagents to remove patulin; biological methods use the adsorption of microorganisms and animals or their metabolites to remove patulin. Although these three methods can achieve the detoxification effect of patulin, there are still certain defects. For example: the use of heating methods may cause the loss of nutrients in food; the use of chemical reagents has a complicated operation process and requires a high level of technical skills for operators; the use of biological methods has different detoxification effects for each microorganism, and it cannot be guaranteed that the fungal toxins are completely removed. Therefore, people urgently need to find a new, safer and more efficient detoxification method to meet people's needs.
[0004] In recent years, studies have found that photodegradation technology has the advantages of being green, safe, and efficient, and has gradually been applied to the degradation of mycotoxins. This technology is an environmentally friendly technology with mild reaction conditions, high efficiency, and high stability. Therefore, some researchers have applied photocatalytic technology to the degradation of mycotoxins and achieved good results. TiO2, as a nanomaterial with high oxidation efficiency, high stability, green environmental protection, and low cost, is widely used in the field of photocatalytic degradation. However, it has the disadvantages of low separation efficiency of photogenerated electron-hole pairs, low utilization rate of visible light, and difficulty in recycling, which limits the industrial application of TiO2. Therefore, it is necessary to modify it to improve its photocatalytic activity. Studies have found that combining TiO2 with metal semiconductor materials can improve its utilization rate of sunlight and inhibit the recombination of photogenerated electron-hole pairs.
[0005] As a magnetic material, ZnFe2O4 has attracted wide attention due to its high visible light utilization rate, small bandgap, and easy separation and recovery. The present invention uses a simple solvent thermal synthesis method to prepare a ZnFe2O4 / TiO2 composite photocatalytic material from nanomaterial TiO2 and metal semiconductor material ZnFe2O4, which can improve the photocatalytic efficiency, and the composite material has magnetism. In the food system, the photocatalytic material can be removed by magnetic adsorption, which solves the problem that nanomaterials are not easy to recycle, has no reagent residue, and is safer. The method of the present invention is expected to introduce a new method in the field of mycotoxin removal, and provide a partial basis and new ideas for the application of photocatalytic technology in the degradation of mycotoxin. Summary of the invention
[0006] The first object of the present invention is to provide a method for preparing a ZnFe2O4 / TiO2 composite material. The method adopts a solvent thermal synthesis method to prepare ZnFe2O4 / TiO2 composite materials with different mass ratios by changing the ratio of two single materials. The preparation method has the advantages of simple process, low cost, and suitability for large-scale production. The composite material has high photocatalytic performance, strong stability, easy recycling, and good reuse effect.
[0007] The second object of the present invention is to provide an application of a ZnFe2O4 / TiO2 composite material in the photocatalytic degradation of patulin. The method has the advantages of no secondary pollution, safety and stability, and has a good application prospect for the degradation of fungal toxins.
[0008] In order to achieve the above object, the present invention is implemented by the following technical solutions:
[0009] 1. A method for preparing a ZnFe2O4 / TiO2 composite material, comprising the following steps:
[0010] 1) Nano ZnFe2O4 material is prepared by a hydrothermal method;
[0011] 2) The above ZnFe2O4 nanomaterials and commercial TiO2 nanomaterials are mixed in anhydrous ethanol solution at different mass ratios, and are mixed evenly by ultrasonication for 2 hours; then the mixed solution is transferred to a hydrothermal kettle for hydrothermal reaction, and the reaction is cooled to room temperature after the reaction is completed, and the precipitate is collected by centrifugation, and the precipitate is washed alternately with anhydrous ethanol and distilled water for 3 times, placed in a vacuum drying oven at 60°C for 12 hours, and then ground after drying. After grinding, the ground precipitate is placed in a muffle furnace for calcination, and the mixture is taken out after natural cooling to room temperature, and ground into powder to obtain a ZnFe2O4 / TiO2 composite material.
[0012] Furthermore, in the step 2), the TiO2 nanomaterial is Degussa P25 material.
[0013] Furthermore, in the step 2), the hydrothermal temperature is 160° C. and the hydrothermal time is 8 hours.
[0014] Furthermore, in the step 2), the calcination temperature in the muffle furnace is 400° C., the calcination time is 2 h, and the heating rate is 5° C. / main.
[0015] Furthermore, in step 2), the mass fraction of ZnFe2O4 in the composite material is 5% to 25%, preferably 10%.
[0016] 2. Application of a ZnFe2O4 / TiO2 composite material in the degradation of patulin. The specific operation includes the following steps:
[0017] 1) adding the ZnFe2O4 / TiO2 composite material to acetic acidified water and ultrasonically treating the solution for 10 to 30 minutes, and then adding patulin to the solution;
[0018] 2) The mixed solution was stirred for 30 min in the dark to perform a dark reaction to reach an adsorption-degradation equilibrium. After the dark reaction, 1 mL of the sample was taken. The solution was then continuously irradiated under a 300 W xenon lamp, and samples were taken every 5 min. The degradation of patulin was recorded by high performance liquid chromatography.
[0019] Furthermore, the concentration of patulin in the solution is 250 to 1500 μg / kg.
[0020] Furthermore, the time for the solution to degrade under continuous irradiation with a xenon lamp is 10 to 30 minutes.
[0021] Furthermore, the addition amount of ZnFe2O4 / TiO2 composite material in the photocatalytic reaction system is 50-300 μg / mL.
[0022] In addition, it should be noted that, unless otherwise specified, any range described in the present invention includes the end values and any numerical values between the end values and any sub-range formed by the end values or any numerical values between the end values.
[0023] Beneficial effects of the present invention:
[0024] (1) The preparation method of the composite material of the present invention has a simple process, low cost, and low requirements on equipment. There is no need to prepare a titanium dioxide precursor. It only requires directly mixing the ZnFe2O4 material prepared by a simple solvent thermal method and the commercial Degussa P25 material. After hydrothermal treatment, washing, drying, and calcination, the composite material can be obtained. The composite material is suitable for industrial production and has high application prospects and practical value in the field of photocatalytic degradation of fungal toxins.
[0025] (2) The ZnFe2O4 / TiO2 composite material prepared by the present invention has magnetism and can be removed by magnetic adsorption and is easy to recycle, thus solving the problem of difficult recycling of nanomaterials.
[0026] (3) Compared with pure titanium dioxide, the ZnFe2O4 / TiO2 composite material prepared by the present invention has a higher utilization rate of visible light, a higher efficiency of electron and hole transfer, and a stronger photocatalytic performance.
[0027] (4) The ZnFe2O4 / TiO2 composite material prepared by the present invention has a low reaction dosage when photocatalytically degrading patulin, and only 10 mg of catalyst is needed in a 50 mL system, which can save costs;
[0028] (5) The ZnFe2O4 / TiO2 composite material prepared by the present invention has high photocatalytic efficiency, short sampling interval, sampling once every 5 minutes, short degradation time, and can completely degrade patulin within 20 minutes;
[0029] (6) The present invention has high safety in the process of photocatalytic degradation of patulin and no reagent residues. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 is the scanning electron microscope (SEM) image of the ZFT10 composite;
[0031] Figure 2 is the transmission electron microscopy (TEM) image of the ZFT10 composite material;
[0032] Figure 3 It is a comparison of the photoluminescence spectra (PL) of TiO2 and ZFT10 composites;
[0033] Figure 4 It is a comparison diagram of the hysteresis loop (VSM) of ZnFe2O4 and ZFT10 composite materials;
[0034] Figure 5 is the macroscopic magnetic adsorption image of ZFT10 composite material;
[0035] Figure 6 It is the photocatalytic degradation diagram of patulin by TiO2, ZnFe2O4, and ZnFe2O4 / TiO2 composite materials with different mass ratios; DETAILED DESCRIPTION
[0036] Example 1
[0037] 1) Preparation of ZnFe2O4
[0038] 5mmol Fe(NO3)3·9H2O and 2.5mmol Zn(NO3)2·6H2O were dissolved in 40mL distilled water, and then the pH of the solution was adjusted to 13 with 6M KOH, and then the mixed solution was transferred to a 50mL hydrothermal kettle, heated at 180°C for 6h to carry out a hydrothermal reaction, cooled to room temperature after the reaction, and the precipitate was collected by centrifugation. The precipitate was washed alternately with anhydrous ethanol and distilled water for 3 times, placed in a 60°C vacuum drying oven to dry for 12h, and ground after drying; after grinding, it was placed in a muffle furnace and calcined at 400°C for 2h, and the heating program was 5°C / min. After naturally cooling to room temperature, it was taken out and ground into powder to obtain ZnFe2O4 material;
[0039] 2) Preparation of ZnFe2O4 / TiO2 composite photocatalytic materials
[0040] The prepared 20mg ZnFe2O4 and 180mg TiO2 (Degussa P25) samples were mixed in 40mL anhydrous ethanol solution, and ultrasonicated for 2h to mix the two substances evenly; then the mixed solution was transferred to a 50mL hydrothermal kettle, heated at 180℃ for 8h, and the hydrothermal reaction was carried out; after the reaction was completed, the mixture was cooled to room temperature, and the precipitate was collected by centrifugation. The precipitate was washed alternately with anhydrous ethanol and distilled water for 3 times, placed in a 60℃ vacuum drying oven to dry for 12h, and then ground; after grinding, it was placed in a muffle furnace and calcined at 400℃ for 2h, with a heating program of 5℃ / min, and naturally cooled to room temperature. After that, it was taken out and ground into powder to obtain a ZnFe2O4 / TiO2 composite material. The mass ratio of ZnFe2O4 in the composite photocatalytic material is 10wt%, which is recorded as ZFT10.
[0041] like Figure 1 The SEM image of the ZFT10 composite material is shown. It can be seen from the figure that the prepared composite material has uniform particle size and smooth surface. ZnFe2O4 is attached to the composite TiO2 surface, achieving good interaction, which is beneficial to the separation of electron-hole pairs and improves the photocatalytic rate.
[0042] like Figure 2 The TEM image of the ZFT10 composite material is shown. From the image, it can be seen that the TiO2 (Degussa P25) in the prepared composite material has a spherical structure and the ZnFe2O4 has a cubic structure. The two materials are tightly combined together, the specific surface area of the composite material is increased, and the absorption and utilization rate of light are improved.
[0043] like Figure 3A comparison of the photoluminescence spectra (PL) of TiO2 and ZFT10 composites is shown. It can be seen from the figure that compared with pure TiO2, the fluorescence intensity of the ZFT10 composite is significantly reduced, indicating that in the photocatalytic reaction system of pure TiO2, photogenerated electrons and holes are easy to recombine quickly, while the modification of ZnFe2O4 can inhibit the recombination of the two. The prepared ZFT10 composite material has a higher separation and transfer rate of photogenerated electron-hole pairs, which is more conducive to the photocatalytic reaction.
[0044] like Figure 4 The comparison of the hysteresis loop (VSM) of ZnFe2O4 and ZFT10 is shown. It can be seen from the figure that the VSM curves of ZnFe2O4 and ZFT10 materials pass through the origin and no hysteresis phenomenon occurs, indicating that ZnFe2O4 and ZFT10 composite materials are magnetic and both are soft magnetic materials. And because TiO2 material is not magnetic, the magnetism of ZFT10 composite material comes entirely from ZnFe2O4.
[0045] Figure 5 This is a macroscopic magnetic adsorption diagram of the ZFT10 composite material. The diagram shows that the ZFT10 composite material can be attracted by a magnet in the presence of an external magnetic field, and can be quickly and conveniently separated and recovered from the photocatalytic solution system using the external magnetic field, with good separation and recovery performance, which is conducive to the recycling of the ZFT10 composite material.
[0046] Example 2
[0047] The ZnFe2O4 / TiO2 composite photocatalyst material was prepared in the same manner as in Example 1, except that the "20 mg ZnFe2O4 and 180 mg TiO2 (Degussa P25) sample" in step 2) of Example 1 was changed to "10 mg ZnFe2O4 and 190 mg TiO2 (Degussa P25) sample" to obtain ZFT5.
[0048] Example 3
[0049] The ZnFe2O4 / TiO2 composite photocatalytic material was prepared in the same manner as in Example 1, except that the "20 mg ZnFe2O4 and 180 mg TiO2 (Degussa P25) sample" in step 2) of Example 1 was changed to "30 mg ZnFe2O4 and 170 mg TiO2 (Degussa P25) sample" to obtain ZFT15.
[0050] Example 4
[0051] The ZnFe2O4 / TiO2 composite photocatalytic material was prepared in the same manner as in Example 1, except that the "20 mg ZnFe2O4 and 180 mg TiO2 (Degussa P25) sample" in step 2) of Example 1 was changed to "50 mg ZnFe2O4 and 150 mg TiO2 (Degussa P25) sample" to obtain ZFT25.
[0052] Example 5
[0053] Photocatalytic degradation of patulin by ZnFe2O4 / TiO2 composites with different mass ratios
[0054] Experimental group: 6 mg of ZnFe2O4 / TiO2 composite materials with different mass ratios were weighed and added to 30 mL of acetic acidified water for 10 minutes of ultrasonic treatment to make the composite materials dispersed evenly in the solution. Then, patulin was added to the solution to make the concentration of patulin in the solution system 500 μg / kg. The above solution system was stirred for 30 minutes under dark conditions to make ZnFe2O4 / TiO2 reach adsorption-desorption equilibrium for patulin. After the dark reaction, 1 mL of sample was taken, and then the solution was continuously irradiated with a 300W xenon lamp for 20 minutes, and samples were taken every 5 minutes, with a sampling volume of 1 mL. After the reaction was completed, the sample was centrifuged and the supernatant was filtered through a 0.22 μm water filter membrane and then detected by high performance liquid chromatography to record the degradation of patulin. The results showed that after 20 minutes of illumination, the degradation rate of patulin by ZFT10 reached 100%.
[0055] The ZnFe2O4 / TiO2 composite material is ZFT5, ZFT10, ZFT15, and ZFT25 prepared in Examples 1 to 4.
[0056] Control group 1: except that the "ZnFe2O4 / TiO2" in the experimental group was replaced by "TiO2 (Degussa P25)", the other procedures were the same as those of the experimental group. When the photodegradation time was 20 min, the degradation rate of patulin was 67.55%.
[0057] Control group 2: except that the "ZnFe2O4 / TiO2" in the experimental group was replaced by "ZnFe2O4 material", the rest was carried out in the same manner as the experimental group. When the photodegradation time was 20 min, the degradation rate of patulin was 12.76%.
[0058] Blank group: Prepare 30mL of 500μg / kg patulin in acetic acid-acidified water, sonicate for 10min, stir for 30min in dark conditions, take 1mL of sample after dark reaction, and irradiate the solution with a 300W xenon lamp for 20min, take samples every 5min, and take 1mL of sample. After the reaction, centrifuge the sample, take the supernatant through a 0.22μm water filter, and then detect it by high performance liquid chromatography to record the degradation of patulin. The results show that after 20min of illumination, patulin is not degraded.
[0059] Figure 6 The figure is the degradation diagram of patulin by different materials. The results show that the photocatalytic effect of the prepared ZnFe2O4 / TiO2 composite materials with different mass ratios on patulin is higher than that of ZnFe2O4 and TiO2, indicating that the ZnFe2O4 / TiO2 composite material has good migration and separation speed of electrons and holes, thereby improving the efficiency of photocatalytic degradation of patulin; with the increase of the mass fraction of ZnFe2O4 in the composite material, the degradation efficiency of the composite material on patulin shows a trend of first increasing and then decreasing. When the mass fraction of ZnFe2O4 in the ZnFe2O4 / TiO2 composite material is 10wt%, that is, the photocatalytic degradation activity of the ZFT10 composite material is the best, and patulin can be completely degraded after 20 minutes of illumination.
[0060] The above is an explanation of the present invention, not a limitation of the present invention. For those skilled in the art, other forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes derived from this are still within the scope of protection of the present invention.
Claims
1. A ZnFe2O4 / TiO2 composite material, characterized in that: The composite material is prepared by using nanometer materials ZnFe2O4 and TiO2 in different mass ratios through a solvent thermal synthesis method, and the material has a nanometer structure.
2. A method for preparing the composite material according to claim 1, characterized in that: Here are the steps: 1) Nano ZnFe2O4 material is prepared by a hydrothermal method; 2) The above ZnFe2O4 nanomaterials and commercial TiO2 nanomaterials are mixed in anhydrous ethanol solution at different mass ratios, and are mixed evenly by ultrasonication for 2 hours; then the mixed solution is transferred to a hydrothermal kettle for hydrothermal reaction, and the reaction is cooled to room temperature after the reaction is completed, and the precipitate is collected by centrifugation, and the precipitate is washed alternately with anhydrous ethanol and distilled water for 3 times, placed in a vacuum drying oven at 60°C for 12 hours, and then ground after drying. After grinding, the ground precipitate is placed in a muffle furnace for calcination, and the mixture is taken out after natural cooling to room temperature, and ground into powder to obtain a ZnFe2O4 / TiO2 composite material.
3. The ZnFe2O4 / TiO2 composite photocatalytic material according to claim 2, characterized in that: Step 2) The TiO2 nanomaterial is Degussa P25 material.
4. The ZnFe2O4 / TiO2 composite photocatalytic material according to claim 2 and the Degussa P25 material according to claim 3, characterized in that: The hydrothermal temperature in step 2) of claim 2 is 160° C. and the hydrothermal time is 8 hours.
5. The ZnFe2O4 / TiO2 composite photocatalytic material according to claim 2 and the Degussa P25 material according to claim 3, characterized in that: In step 2) of claim 2, the muffle furnace calcination temperature is 400°C, the calcination time is 2h, and the heating rate is 5°C / min.
6. The ZnFe2O4 / TiO2 composite photocatalytic material according to claim 2 and the Degussa P25 material according to claim 3, characterized in that: The mass fraction of ZnFe2O4 in the composite material in step 2) of claim 2 is 5% to 25%.
7. An application of the ZnFe2O4 / TiO2 composite material as claimed in claim 1, characterized in that: Its application in photocatalytic degradation of fungal toxins. The specific operation includes the following steps: 1) adding the ZnFe2O4 / TiO2 composite material to acetic acidified water and ultrasonically treating the solution for 10 to 30 minutes, and then adding patulin to the solution; 2) The mixed solution was stirred for 30 min in the dark for dark reaction, and 1 mL was sampled after the dark reaction. The solution was then continuously irradiated under a 300 W xenon lamp, and samples were taken every 5 min. The degradation of patulin was recorded by high performance liquid chromatography.
8. The use according to claim 7, characterized in that: The concentration of patulin in the solution is 250-1500 μg / kg.
9. The use according to claim 7, characterized in that: The time for the solution to degrade under continuous irradiation with a xenon lamp is 10 to 30 minutes.
Citation Information
Patent Citations
Preparation method of photocatalytic material by in-situ compositing zinc ferrite nano-rods with lamellar TiO2
CN108686665A
Preparation method of oxygen defect TiO2@ZnFe2O4 heterojunction photocatalytic material
CN109876814A
Preparation method of {001} crystal face TiO2@ZnFe2O4 heterojunction photocatalytic material
CN111389402A
Preparation method of heterojunction photocatalytic composite material
CN111659403A
Titanium dioxide-bismuth tungstate heterojunction photocatalyst and application thereof in degradation of patulin in fruit juice