Cu / MgO-M supported catalyst as well as preparation method and application thereof
Through Cu/MgO-M supported catalyst, the combination of copper and MgO and the doping of La2O3 is used to solve the heavy metal pollution and activity of CuCrOx catalyst, and the efficient and stable selective hydrogenation reaction of furfural is achieved, which improves the catalyst Number of cycles and reaction activity.
Patent Information
- Application Number
- CN202411101075.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-12
AI Technical Summary
The existing CuCrOx catalysts have problems such as heavy metal contamination and poor low-temperature activity, low high-temperature selectivity and poor cycle stability in the preparation of furfurfural alcohol, making it difficult to achieve efficient and stable selective hydrogenation reaction of furfural.
Cu/MgO-M supported catalyst is used, and La2O3 is introduced as the second support by introducing copper as the main metal and MgO as the main support, and adjusting the molar ratio and preparation method to form a stable catalyst, thereby improving the catalytic activity and the number of cycles.
It realizes efficient catalyzing of furfurfural preparation of furfurfural at room temperature. The metal of the catalyst is evenly dispersed, has strong hydrothermal stability, and can be recycled multiple times, which improves the reaction activity and selectivity and reduces the generation of by-products.
Smart Images

Figure CN118976504A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalysis and relates to a Cu / MgO-M supported catalyst and a preparation method thereof. Background Art
[0002] As the only renewable organic carbon source, biomass resources can effectively utilize CO2 released into the atmosphere by nature or human activities and convert it into chemicals and fuels with extremely high application value. Lignocellulose is the most promising raw material for biomass derivatives. The most important subsequent derivative operation is the hydrolysis reaction of cellulose and hemicellulose to obtain second-generation biofuels and intermediate compounds, such as glycerol, glucose, furfural, 5-hydroxymethylfurfural and levulinic acid. Among them, furfural is the intermediate link between biomass resources and the chemical industry.
[0003] Generally, furfural is produced by acid-catalyzed degradation of cellulose or hemicellulose in agricultural and forestry waste into xylose, which is then dehydrated to produce furfural. Due to the presence of C=O bonds, C=C bonds and furan rings in furfural, it can be used to prepare a variety of downstream derivatives through decarbonylation, hydrogenation, ring opening and other reactions. Furfuryl alcohol is an important fine chemical obtained by the selective hydrogenation of furfural, with high added value and wide application. In industry, CuCrO is mainly used. x The catalyst selectively hydrogenates the furfuryl alcohol, which can selectively hydrogenate the C=O double bond without affecting the C=C double bond, with a yield of up to 95%. However, catalysts containing heavy metal Cr cause increasingly serious environmental problems and cannot be mass-produced. In recent years, people have shown increasing interest in finding more environmentally friendly alternatives to replace CuCrO. x Cr component in the catalyst. In addition to Cr, many transition metals have extremely high reactivity for the production of furfuryl alcohol from furfural, such as Au, Cu, Co, Ir, Ni, Pd, Pt, Rh, and Ru. In particular, Cu-based catalysts have attracted much attention in the reaction of furfural to furfuryl alcohol. However, copper-based catalysts have problems such as poor low-temperature activity, low high-temperature selectivity, and poor cyclic stability. Therefore, it is imperative to develop efficient and stable copper-based catalysts to achieve efficient and selective hydrogenation of furfural to produce furfuryl alcohol. Summary of the invention
[0004] In view of this, the present invention provides a preparation method of a Cu / MgO-M supported catalyst and a method for catalyzing furfural to prepare furfuryl alcohol. The catalyst prepared by the preparation method has simple steps, easy operation, is prepared at room temperature, consumes less energy, and the metal of the supported catalyst is evenly dispersed, has strong hydrothermal stability, and can be recycled for multiple times.
[0005] It should be noted that the Cu catalyst often binds to the surface by adsorbing the C=O double bond of furfural, showing good selectivity for furfuryl alcohol. DFT calculations on the Cu surface show that furfural tends to η 1 (O)-aldehyde binding mode, the carbonyl in furfural is easily bound to the Cu surface through the lone pair of electrons of O, while the rest of the molecule is pushed away from the surface due to the net repulsion between C and Cu. Since the copper metal surface has a weak affinity for C=C bonds and a strong affinity for C=O bonds, this binding mode is more conducive to the hydrogenation of C=O bonds. Therefore, the present invention selects non-precious metal copper as the active main metal.
[0006] The study found that the product distribution and hydrogenation rate of furfural depend on the affinity of the reactant for the metal and the adsorption mode of the adsorbate on the specific part of the catalyst (vertical or flat adsorption). The reaction mechanism shows that the activation of the C=O double bond is crucial in the reaction of furfural hydrogenation to furfuryl alcohol. Although Cu has a high selectivity for furfuryl alcohol, its adsorption and activation ability for H2 is poor, which slows down the occurrence of the hydrogenation process. The catalytic activity can be improved by introducing a second metal / metal oxide or selecting a non-benign carrier to reasonably adjust the electronic structure of the metal. On the one hand, the interaction between metal nanoparticles and metal oxides changes the electron density of the metal, promoting the formation of nanoparticles and facilitating the availability of a large number of active sites. On the other hand, the oxide / metal interface can enhance the Lewis acidity and hydrogen activation ability, improve the anti-sintering performance of metal nanoparticles, and greatly improve the catalytic activity of the single metal catalyst. Therefore, in the reaction of catalyzing furfural to prepare furfuryl alcohol, it is necessary to dope a second carrier to change the metal properties, but it is still unknown what kind of second carrier should be selected to make the supported catalyst more conducive to catalyzing furfural to prepare furfuryl alcohol. Therefore, the present invention develops a novel supported catalyst Cu / MgO-M and a preparation method thereof, so that the catalyst can efficiently catalyze furfural to selectively prepare furfuryl alcohol.
[0007] Specifically, the present invention uses Cu as the main metal, MgO as the main carrier, and La2O3 as the second carrier. By changing the different molar ratios of the main carrier and the doping carrier, different active sites are effectively combined to maximize the synergistic effect while the reaction proceeds smoothly.
[0008] In order to achieve the above object, the present invention adopts the following technical solution:
[0009] The first technical purpose of the present invention is to provide a Cu / MgO-M supported catalyst, wherein the main active metal of the supported catalyst is copper, the carrier is the metal oxide MgO, the second carrier M is La2O3; and the molar ratio between Mg and M is 0.1-8.
[0010] The second technical purpose of the present invention is to provide a method for preparing the Cu / MgO-M supported catalyst as described above, which specifically comprises the following steps:
[0011] S1. Mixing a copper sulfate metal precursor with water, stirring until the solid is dissolved, adding two carriers in different molar ratios, ultrasonicating for a period of time, and stirring to obtain a corresponding mixed solution;
[0012] S2, stop the above stirring, let it stand overnight, and then put it in an oven to dry at a certain temperature;
[0013] S3. The dried product is calcined in air and reduced under the action of H2 to obtain the Cu / MgO-M supported catalyst.
[0014] Furthermore, in S1, the metal salt is CuSO4·5H2O, the carrier is selected from MgO, the second carrier (M) is selected from La2O3, and the molar ratio between Mg and M is 0.1-8. The excess impregnation method is adopted, the ultrasonic time is 10 to 30 minutes, and the stirring time is 10 to 12 hours.
[0015] Furthermore, in S2, the standing time is 8 to 12 hours, the drying temperature is 60 to 80°C, and the drying time is 6 to 8 hours.
[0016] Further, in S3, the dried product is subjected to air roasting in a muffle furnace and reduction under the action of H2 in a tubular furnace. The specific operation is as follows:
[0017] The heating rate of the muffle furnace is 1-5°C / min, and the temperature is maintained at 300-600°C for 1-4 hours; the heating rate of the tubular furnace is 1-5°C / min, and the temperature is maintained at 100-600°C for 1-5 hours.
[0018] The third technical purpose of the present invention is to provide the application of the Cu / MgO-M supported catalyst as described above in the field of catalysis.
[0019] Furthermore, the Cu / MgO-M supported catalyst is used in environmental governance and restoration.
[0020] Furthermore, the Cu / MgO-M supported catalyst catalyzes furfural to prepare furfuryl alcohol.
[0021] Specifically, a method for catalyzing furfural to prepare furfural alcohol, the method comprises using the Cu / MgO-M supported catalyst prepared by the method as described above to catalyze furfural to prepare furfural alcohol, and the operation is as follows:
[0022] The reaction of preparing furfuryl alcohol from furfural catalyzed by the Cu / MgO-M supported catalyst is carried out in a stainless steel high-pressure reactor. The air in the reactor is replaced by N2 for several times. After H2 is introduced for multiple replacements, the H2 pressure in the high-pressure reactor is maintained at a certain pressure, and the catalytic reaction is carried out by stable heating and stirring. After the reaction is completed, the product furfuryl alcohol is obtained by centrifugal separation, and the catalyst Cu / MgO-M is recovered at the same time, and the catalyst phase does not need to be post-treated and is directly recycled.
[0023] Furthermore, nitrogen is used to replace the air in the kettle for 2 to 5 times, and hydrogen is used to replace the air in the kettle for 1 to 3 times. The H2 pressure should be maintained at 1 to 4 MPa, the mass of Cu / MgO-M and furfural is 1:(0.5 to 4), the reaction temperature is 70 to 130°C, and the reaction time is 10 to 120 min.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The supported catalyst Cu / MgO-M prepared by the present invention uses copper as the active metal, MgO as the main carrier, and La2O3 as the secondary carrier. Compared with the prior art, La2O3 doping greatly increases the Cu 0 At the same time, the size of the metal particles is greatly reduced, which promotes the increase of the active surface area of the catalyst, thereby providing a larger active surface area that is conducive to the efficient adsorption of FAL and H2. The addition of La2O3 increases the strong alkaline sites of the catalyst, which can promote the dispersion of Cu metal on the one hand, and on the other hand, can effectively promote the adsorption of FAL, which is conducive to the hydrogenation reaction. At the same time, the strong alkaline sites have a weak adsorption effect on furfuryl alcohol, which promotes the desorption of the reaction products from the catalyst surface and prevents excessive hydrogenation and the formation of by-products.
[0026] Specifically, the present invention uses Cu as an active metal, MgO as a main carrier, and La2O3 as a second carrier, effectively combining the two active sites of Cu and La to maximize the synergistic effect, that is, La2O3 selectively adsorbs the terminal carbonyl group, and Cu decomposes H2 into hydrogen protons and then transfers them to La2O3, so that the C=O double bond is selectively hydrogenated to generate furfuryl alcohol, which greatly improves the reaction activity. After the catalytic reaction is completed, the catalyst and the product can be separated simply and efficiently by centrifugation. The catalyst phase does not need post-treatment and can be directly reused. After being reused for 5 times, the catalytic performance is not significantly reduced, and the recycling effect is good. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0028] Figure 1 It is a schematic diagram of the preparation mechanism of the Cu / MgO-M supported catalyst of the present invention.
[0029] Figure 2 These are TEM images of the Cu / MgO-M supported catalysts prepared by the present invention: (a) Cu / MgO-La2O3-2, (b) Cu / MgO-La2O3-4, (c) Cu / MgO-La2O3-6, (d) Cu / MgO-La2O3-8; (ef) HR-TEM of Cu / MgO-La2O3-6.
[0030] Figure 3 This is the EDS element mapping of Cu / MgO-La2O3-6.
[0031] Figure 4 It is the XRD spectrum of the Cu / MgO-M supported catalyst prepared by the present invention.
[0032] Figure 5 It is H2-TPR of MgO, La2O3, LA-0, LA-2, LA-4, LA-6 and LA-8 catalysts.
[0033] Figure 6 The catalytic effects of a series of different carriers of Cu-based catalysts on the selective hydrogenation of FAL under the same reaction conditions are compared; (a) catalysts with different doped carriers, (b) catalysts with different doping amounts.
[0034] Figure 7 (a) Cu 2p spectrum, (b) XAES spectrum corresponding to Cu LMM, (c) La 3d spectrum, (d) Mg 2s spectrum and (e) O 1s spectrum of LA-0, LA-2, LA-4, LA-6 and LA-8.
[0035] Figure 8 (a) NH3-TPD and (b) CO2-TPD of MgO, La2O3, LA-0, LA-2, LA-4, LA-6 and LA-8 catalysts. DETAILED DESCRIPTION
[0036] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.
[0038] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.
[0039] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.
[0040] Under the premise of no conflict, the technical features disclosed in the embodiments of the present application can be combined arbitrarily, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present application.
[0041] The invention discloses a method for preparing a Cu / MgO-M supported catalyst and catalyzing furfural to prepare furfuryl alcohol.
[0042] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.
[0043] Example 1
[0044] S1. Mix 0.31 g CuSO4·5H2O and 5.0 mL deionized water in a 10.0 mL beaker, stir until the solid is dissolved, add the oxide carrier, then add 0.5 g MgO and 1.01 g La2O3 carrier, ultrasonicate for 10 min, stir at room temperature, and keep for 8 h to obtain the corresponding mixed solution;
[0045] S2, stop the above stirring, let it stand overnight for 12 hours, and then place it in an oven at 80°C to dry for 6 hours;
[0046] S3, calcining the dried product in a muffle furnace, the calcination temperature is increased to 500°C at a rate of 2°C / min, the calcination time is 3h, the obtained solid product is placed in a tubular furnace for reduction, the reduction temperature is increased to 300°C at a rate of 2°C / min, the calcination time is 3h, and the product Cu / MgO-La2O3-2 is obtained;
[0047] S4, 0.05 mL furfural, 0.05 g Cu / MgO-La2O3-2, 5 mL isopropanol and a high temperature magnet are placed in a 75 mL high temperature and high pressure stainless steel reactor, the air in the reactor is replaced with nitrogen 3 times, and hydrogen is replaced 3 times, the pressure in the high pressure reactor is maintained at 2 MPa, and heated and stirred at 100°C for 40 min;
[0048] S5. After the reaction is completed, the mixture is allowed to stand and cool to room temperature. The product furfuryl alcohol is obtained by centrifugal separation, and the catalyst Cu / MgO-La2O3-2 is recovered. The catalyst phase is directly recycled without post-treatment. The furfural conversion rate is 66.4%, and the furfuryl alcohol yield is 49.1%.
[0049] The calculation formulas for furfural conversion and furfuryl alcohol yield are as follows:
[0050]
[0051] Y=S*X
[0052] Wherein, Y is the yield of furfural; X is the conversion rate of furfural; S is the selectivity of furfuryl alcohol; n initial is the molar amount of furfural added; n final is the remaining molar amount of furfuryl alcohol; m product is the molar mass of the product furfuryl alcohol.
[0053] Example 2
[0054] S1. Mix 0.21 g CuSO4·5H2O and 5.0 mL deionized water in a 10.0 mL beaker, stir until the solid is dissolved, add the oxide carrier, then add 0.5 g MgO and 0.5 g La2O3 carrier, ultrasonicate for 10 min, stir at room temperature, and keep for 8 h to obtain the corresponding mixed solution;
[0055] S2, stop the above stirring, let it stand overnight for 12 hours, and then place it in an oven at 80°C to dry for 6 hours;
[0056] S3, calcining the dried product in a muffle furnace, the calcination temperature is increased to 500°C at a rate of 2°C / min, the calcination time is 3h, the obtained solid product is placed in a tubular furnace for reduction, the reduction temperature is increased to 300°C at a rate of 2°C / min, the calcination time is 3h, and the product Cu / MgO-La2O3-4 is obtained;
[0057] S4, 0.05 mL furfural, 0.05 g Cu / MgO-La2O3-4, 5 mL isopropanol and a high temperature magnet are placed in a 75 mL high temperature and high pressure stainless steel reactor, the air in the reactor is replaced with nitrogen 3 times, and hydrogen is replaced 3 times, the pressure in the high pressure reactor is maintained at 2 MPa, and heated and stirred at 100°C for 40 min;
[0058] S5. After the reaction is completed, the mixture is allowed to stand and cool to room temperature. The product furfuryl alcohol is obtained by centrifugal separation, and the catalyst Cu / MgO-La2O3-4 is recovered. The catalyst phase is directly recycled without post-treatment. The furfural conversion rate is 70.5%, and the furfuryl alcohol yield is 56.8%.
[0059] Example 3
[0060] S1. Mix 0.21 g CuSO4·5H2O and 5.0 mL deionized water in a 10.0 mL beaker, stir until the solid is dissolved, add the oxide carrier, then add 0.5 g MgO and 0.34 g La2O3 carrier, ultrasonicate for 10 min, stir at room temperature, and keep for 8 h to obtain the corresponding mixed solution;
[0061] S2, stop the above stirring, let it stand overnight for 12 hours, and then place it in an oven at 80°C to dry for 6 hours;
[0062] S3, calcining the dried product in a muffle furnace, the calcination temperature is increased to 500°C at a rate of 2°C / min, the calcination time is 3h, the obtained solid product is placed in a tubular furnace for reduction, the reduction temperature is increased to 300°C at a rate of 2°C / min, the calcination time is 3h, and the product Cu / MgO-La2O3-6 is obtained;
[0063] S4, 0.05 mL furfural, 0.05 g Cu / MgO-La2O3-6, 5 mL isopropanol and a high temperature magnet are placed in a 75 mL high temperature and high pressure stainless steel reactor, the air in the reactor is replaced with nitrogen 3 times, and hydrogen is replaced 3 times, the pressure in the high pressure reactor is maintained at 2 MPa, and heated and stirred at 100°C for 40 min;
[0064] S5. After the reaction is completed, the mixture is allowed to stand and cool to room temperature. The product furfuryl alcohol is obtained by centrifugal separation, and the catalyst Cu / MgO-La2O3-6 is recovered. The catalyst phase is directly recycled without post-treatment. The furfural conversion rate is 93.6%, and the furfuryl alcohol yield is 88.1%.
[0065] Example 4
[0066] S1. Mix 0.21 g CuSO4·5H2O and 5.0 mL deionized water in a 10.0 mL beaker, stir until the solid is dissolved, add the oxide carrier, then add 0.5 g MgO and 0.25 g La2O3 carrier, ultrasonicate for 10 min, stir at room temperature, and keep for 8 h to obtain the corresponding mixed solution;
[0067] S2, stop the above stirring, let it stand overnight for 12 hours, and then place it in an oven at 80°C to dry for 6 hours;
[0068] S3, calcining the dried product in a muffle furnace, the calcination temperature is increased to 500°C at a rate of 2°C / min, the calcination time is 3h, the obtained solid product is placed in a tubular furnace for reduction, the reduction temperature is increased to 300°C at a rate of 2°C / min, the calcination time is 3h, and the product Cu / MgO-La2O3-8 is obtained;
[0069] S4, 0.05 mL furfural, 0.05 g Cu / MgO-La2O3-8, 5 mL isopropanol and a high temperature magnet are placed in a 75 mL high temperature and high pressure stainless steel reactor, the air in the reactor is replaced with nitrogen three times, and hydrogen is replaced three times, the pressure in the high pressure reactor is maintained at 2 MPa, and heated and stirred at 100°C for 40 min;
[0070] S5. After the reaction is completed, the mixture is allowed to stand and cool to room temperature. The product furfuryl alcohol is obtained by centrifugal separation, and the catalyst Cu / MgO-La2O3-8 is recovered. The catalyst phase is directly recycled without post-treatment. The furfural conversion rate is 82.6%, and the furfuryl alcohol yield is 74.9%.
[0071] Example 5
[0072] S1. Mix 0.21 g CuSO4·5H2O and 5.0 mL deionized water in a 10.0 mL beaker, stir until the solid is dissolved, add the oxide carrier, then add 0.5 g MgO and 0.34 g La2O3 carrier, ultrasonicate for 10 min, stir at room temperature, and keep for 8 h to obtain the corresponding mixed solution;
[0073] S2, stop the above stirring, let it stand overnight for 12 hours, and then place it in an oven at 80°C to dry for 6 hours;
[0074] S3, calcining the dried product in a muffle furnace, the calcination temperature is increased to 500°C at a rate of 2°C / min, the calcination time is 3h, the obtained solid product is placed in a tubular furnace for reduction, the reduction temperature is increased to 300°C at a rate of 2°C / min, the calcination time is 3h, and the product Cu / MgO-La2O3-6 is obtained;
[0075] S4, 0.05 mL furfural, 0.05 g Cu / MgO-La2O3-6, 5 mL isopropanol and a high temperature magnet are placed in a 75 mL high temperature and high pressure stainless steel reactor, the air in the reactor is replaced with nitrogen three times, and hydrogen is replaced three times, the pressure in the high pressure reactor is maintained at 2 MPa, and heated and stirred at 90°C for 70 min;
[0076] S5. After the reaction is completed, the mixture is allowed to stand and cool to room temperature. The product furfuryl alcohol is obtained by centrifugal separation, and the catalyst Cu / MgO-La2O3-6 is recovered. The catalyst phase is directly recycled without post-treatment. The furfural conversion rate is 100%, and the furfuryl alcohol yield is 99.9%.
[0077] Example 6
[0078] The experimental conditions and steps were the same as those in Example 5, except that the catalyst was replaced with the catalyst recovered in Example 5. The experiment was repeated five times. After five times of repeated use, the furfural conversion rate was 98.7% and the furfuryl alcohol yield was 97.6%.
[0079] Example 7
[0080] S1. Mix 0.21 g CuSO4·5H2O and 5.0 mL deionized water in a 10.0 mL beaker, stir until the solid is dissolved, add the oxide support, then add 0.5 g MgO and 1.01 g La2O3, ultrasonicate for 10 min, stir at room temperature, and keep for 8 h to obtain the corresponding mixed solution;
[0081] S2, stop the above stirring, let it stand overnight for 12 hours, and then place it in an oven at 80°C to dry for 6 hours;
[0082] S3, calcining the dried product in a muffle furnace, the calcination temperature is increased to 500°C at a rate of 2°C / min, the calcination time is 3h, the obtained solid product is placed in a tubular furnace for reduction, the reduction temperature is increased to 350°C at a rate of 2°C / min, the calcination time is 3h, and the product Cu / MgO-La2O3-2 is obtained;
[0083] S4, 0.05 mL furfural, 0.05 g Cu / MgO-La2O3-2, 5 mL isopropanol and a high temperature magnet are placed in a 75 mL high temperature and high pressure stainless steel reactor, the air in the reactor is replaced with nitrogen 3 times, and hydrogen is replaced 3 times, the pressure in the high pressure reactor is maintained at 2 MPa, and heated and stirred at 100°C for 60 min;
[0084] S5. After the reaction is completed, the mixture is allowed to stand and cool to room temperature. The product furfuryl alcohol is obtained by centrifugal separation, and the catalyst Cu / MgO-La2O3-2 is recovered. The catalyst phase is directly recycled without post-treatment. The furfural conversion rate is 66.9%, and the furfuryl alcohol yield is 52.4%.
[0085] In order to further demonstrate the beneficial effects of the present invention and to better understand the present invention, the following comparative examples and test examples are used to further illustrate the technical features of the supported catalyst Cu / MgO-M and its application disclosed in the present invention, but they should not be understood as limitations of the present invention. Other improvements made by those skilled in the art based on the above invention content without inventive work are also considered to fall within the scope of protection of the present invention.
[0086] Comparative Example:
[0087] Comparative Example 1
[0088] S1. Mix 0.21 g CuSO4·5H2O and 5.0 mL deionized water in a 10.0 mL beaker, stir until the solid is dissolved, add the oxide support, then add 0.5 g MgO and 0.34 g neutral Al2O3, ultrasonicate for 10 min, stir at room temperature, and keep for 8 h to obtain the corresponding mixed solution;
[0089] S2, stop the above stirring, let it stand overnight for 12 hours, and then place it in an oven at 80°C to dry for 6 hours;
[0090] S3, the dried product was calcined in a muffle furnace, the calcination temperature was increased to 500°C at a rate of 2°C / min, the calcination time was 3h, the obtained solid product was placed in a tubular furnace for reduction, the reduction temperature was increased to 350°C at a rate of 2°C / min, the calcination time was 3h, and the product Cu / MgO-Al2O3-2 (medium) was obtained;
[0091] S4, 0.05 mL furfural, 0.05 g Cu / MgO-Al2O3-2 (medium), 5 mL isopropanol and a high temperature magnet are placed in a 75 mL high temperature and high pressure stainless steel reactor, the air in the reactor is replaced with nitrogen 3 times, and hydrogen is replaced 3 times, the pressure in the high pressure reactor is maintained at 2 MPa, and heated and stirred at 100°C for 60 min;
[0092] S5. After the reaction is completed, the mixture is allowed to stand and cool to room temperature. The product furfuryl alcohol is obtained by centrifugal separation, and the catalyst Cu / MgO-Al2O3-2 (middle) is recovered. The catalyst phase is directly recycled without post-treatment. The furfural conversion rate is 30.1%, and the furfuryl alcohol yield is 10.7%.
[0093] Comparative Example 2
[0094] S1. Mix 0.21 g CuSO4·5H2O and 5.0 mL deionized water in a 10.0 mL beaker, stir until the solid is dissolved, add the oxide support, then add 0.5 g MgO and 0.34 g alkaline Al2O3, ultrasonicate for 10 min, stir at room temperature, and keep for 8 h to obtain the corresponding mixed solution;
[0095] S2, stop the above stirring, let it stand overnight for 12 hours, and then place it in an oven at 80°C to dry for 6 hours;
[0096] S3, the dried product was calcined in a muffle furnace, the calcination temperature was increased to 500°C at a rate of 2°C / min, the calcination time was 3h, the obtained solid product was placed in a tubular furnace for reduction, the reduction temperature was increased to 350°C at a rate of 2°C / min, the calcination time was 3h, and the product Cu / MgO-Al2O3-2 (alkali) was obtained;
[0097] S4, 0.05 mL furfural, 0.05 g Cu / MgO-Al2O3-2 (base), 5 mL isopropanol and a high temperature magnet are placed in a 75 mL high temperature and high pressure stainless steel reactor, the air in the reactor is replaced with nitrogen 3 times, and hydrogen is replaced 3 times, the pressure in the high pressure reactor is maintained at 2 MPa, and heated and stirred at 100°C for 60 min;
[0098] S5. After the reaction is completed, the mixture is allowed to stand and cool to room temperature. The product furfuryl alcohol is obtained by centrifugal separation, and the catalyst Cu / MgO-Al2O3-2 (base) is recovered. The catalyst phase is directly recycled without post-treatment. The furfural conversion rate is 43.8%, and the furfuryl alcohol yield is 32.8%.
[0099] Comparative Example 3
[0100] S1. Mix 0.21 g CuSO4·5H2O and 5.0 mL deionized water in a 10.0 mL beaker, stir until the solid is dissolved, add the oxide support, then add 0.5 g MgO and 0.34 g acidic Al2O3, ultrasonicate for 10 min, stir at room temperature, and keep for 8 h to obtain the corresponding mixed solution;
[0101] S2, stop the above stirring, let it stand overnight for 12 hours, and then place it in an oven at 80°C to dry for 6 hours;
[0102] S3, the dried product was calcined in a muffle furnace, the calcination temperature was increased to 500°C at a rate of 2°C / min, the calcination time was 3h, the obtained solid product was placed in a tubular furnace for reduction, the reduction temperature was increased to 350°C at a rate of 2°C / min, the calcination time was 3h, and the product Cu / MgO-Al2O3-2 (acid) was obtained;
[0103] S4, 0.05 mL furfural, 0.05 g Cu / MgO-Al2O3-2 (acid), 5 mL isopropanol and a high temperature magnet are placed in a 75 mL high temperature and high pressure stainless steel reactor, the air in the reactor is replaced with nitrogen 3 times, and hydrogen is replaced 3 times, the pressure in the high pressure reactor is maintained at 2 MPa, and heated and stirred at 100°C for 60 min;
[0104] S5. After the reaction is completed, the mixture is allowed to stand and cool to room temperature. The product furfuryl alcohol is obtained by centrifugal separation, and the catalyst Cu / MgO-Al2O3-2 (acid) is recovered. The catalyst phase is directly recycled without post-treatment. The furfural conversion rate is 29.9%, and the furfuryl alcohol yield is 6.9%.
[0105] Comparative Example 4
[0106] S1. Mix 0.21 g CuSO4·5H2O and 5.0 mL deionized water in a 10.0 mL beaker, stir until the solid is dissolved, add the oxide support, then add 0.5 g MgO and 0.5 g ZnO, ultrasonicate for 10 min, stir at room temperature, and keep for 8 h to obtain the corresponding mixed solution;
[0107] S2, stop the above stirring, let it stand overnight for 12 hours, and then place it in an oven at 80°C to dry for 6 hours;
[0108] S3, calcining the dried product in a muffle furnace, the calcination temperature is increased to 500°C at a rate of 2°C / min, the calcination time is 3h, the obtained solid product is placed in a tubular furnace for reduction, the reduction temperature is increased to 350°C at a rate of 2°C / min, the calcination time is 3h, and the product Cu / MgO-ZnO-2 is obtained;
[0109] S4, 0.05 mL furfural, 0.05 g Cu / MgO-ZnO-2, 5 mL isopropanol and a high temperature magnet are placed in a 75 mL high temperature and high pressure stainless steel reactor, the air in the reactor is replaced with nitrogen 3 times, and hydrogen is replaced 3 times, the pressure in the high pressure reactor is maintained at 2 MPa, and heated and stirred at 100 ° C for 60 min;
[0110] S5. After the reaction is completed, the mixture is allowed to stand and cool to room temperature. The product furfuryl alcohol is obtained by centrifugal separation, and the catalyst Cu / MgO-ZnO-2 is recovered. The catalyst phase is directly recycled without post-treatment. The furfural conversion rate is 43.8%, and the furfuryl alcohol yield is 9.9%.
[0111] Comparative Example 5
[0112] S1. Mix 0.21 g CuSO4·5H2O and 5.0 mL deionized water in a 10.0 mL beaker, stir until the solid is dissolved, add the oxide support, then add 0.5 g MgO and 0.54 g MnO2, ultrasonicate for 10 min, stir at room temperature, and keep for 8 h to obtain the corresponding mixed solution;
[0113] S2, stop the above stirring, let it stand overnight for 12 hours, and then place it in an oven at 80°C to dry for 6 hours;
[0114] S3, calcining the dried product in a muffle furnace, the calcination temperature is increased to 500°C at a rate of 2°C / min, the calcination time is 3h, the obtained solid product is placed in a tubular furnace for reduction, the reduction temperature is increased to 350°C at a rate of 2°C / min, the calcination time is 3h, and the product Cu / MgO-MnO2-2 is obtained;
[0115] S4, 0.05 mL furfural, 0.05 g Cu / MgO-MnO2-2, 5 mL isopropanol and a high temperature magnet are placed in a 75 mL high temperature and high pressure stainless steel reactor, the air in the reactor is replaced with nitrogen 3 times, and hydrogen is replaced 3 times, the pressure in the high pressure reactor is maintained at 2 MPa, and heated and stirred at 100 ° C for 60 min;
[0116] S5. After the reaction is completed, the mixture is allowed to stand and cool to room temperature. The product furfuryl alcohol is obtained by centrifugal separation, and the catalyst Cu / MgO-MnO2-2 is recovered. The catalyst phase is directly recycled without post-treatment. The furfural conversion rate is 39.2%, and the furfuryl alcohol yield is 5.8%.
[0117] Comparative Example 6
[0118] S1. Mix 0.21 g CuSO4·5H2O and 5.0 mL deionized water in a 10.0 mL beaker, stir until the solid is dissolved, add the oxide support, then add 0.5 g MgO and 0.5 g TiO2, ultrasonicate for 10 min, stir at room temperature, and keep for 8 h to obtain the corresponding mixed solution;
[0119] S2, stop the above stirring, let it stand overnight for 12 hours, and then place it in an oven at 80°C to dry for 6 hours;
[0120] S3, calcining the dried product in a muffle furnace, the calcination temperature is increased to 500°C at a rate of 2°C / min, the calcination time is 3h, the obtained solid product is placed in a tubular furnace for reduction, the reduction temperature is increased to 350°C at a rate of 2°C / min, the calcination time is 3h, and the product Cu / MgO-TiO2-2 is obtained;
[0121] S4, 0.05 mL furfural, 0.05 g Cu / MgO-TiO2-2, 5 mL isopropanol and a high temperature magnet are placed in a 75 mL high temperature and high pressure stainless steel reactor, the air in the reactor is replaced with nitrogen 3 times, and hydrogen is replaced 3 times, the pressure in the high pressure reactor is maintained at 2 MPa, and heated and stirred at 100 ° C for 60 min;
[0122] S5. After the reaction is completed, the mixture is allowed to stand and cool to room temperature. The product furfuryl alcohol is obtained by centrifugal separation, and the catalyst Cu / MgO-TiO2-2 is recovered. The catalyst phase is directly recycled without post-treatment. The furfural conversion rate is 32.4%, and the furfuryl alcohol yield is 0.3%.
[0123] Comparative Example 7
[0124] S1. Mix 0.21 g CuSO4·5H2O and 5.0 mL deionized water in a 10.0 mL beaker, stir until the solid is dissolved, add the oxide support, then add 0.5 g MgO and 1.1 g CeO2, ultrasonicate for 10 min, stir at room temperature, and keep for 8 h to obtain the corresponding mixed solution;
[0125] S2, stop the above stirring, let it stand overnight for 12 hours, and then place it in an oven at 80°C to dry for 6 hours;
[0126] S3, calcining the dried product in a muffle furnace, the calcination temperature is increased to 500°C at a rate of 2°C / min, the calcination time is 3h, the obtained solid product is placed in a tubular furnace for reduction, the reduction temperature is increased to 300°C at a rate of 2°C / min, the calcination time is 3h, and the product Cu / MgO-CeO2-2 is obtained;
[0127] S4, 0.05 mL furfural, 0.05 g Cu / MgO-CeO2-2, 5 mL isopropanol and a high temperature magnet are placed in a 75 mL high temperature and high pressure stainless steel reactor, the air in the reactor is replaced with nitrogen 3 times, and hydrogen is replaced 3 times, the pressure in the high pressure reactor is maintained at 2 MPa, and heated and stirred at 100 ° C for 60 min;
[0128] S5. After the reaction is completed, the mixture is allowed to stand and cool to room temperature. The product furfuryl alcohol is obtained by centrifugal separation, and the catalyst Cu / MgO-CeO2-2 is recovered. The catalyst phase is directly recycled without post-treatment. The furfural conversion rate is 34.5%, and the furfuryl alcohol yield is 3.8%.
[0129] Comparative Example 8
[0130] S1. Mix 0.21 g CuSO4·5H2O and 5.0 mL deionized water in a 10.0 mL beaker, stir until the solid is dissolved, add the oxide support, then add 0.5 g MgO and 0.47 g CoO, ultrasonicate for 10 min, stir at room temperature, and keep for 8 h to obtain the corresponding mixed solution;
[0131] S2, stop the above stirring, let it stand overnight for 12 hours, and then place it in an oven at 80°C to dry for 6 hours;
[0132] S3, calcining the dried product in a muffle furnace, the calcination temperature is increased to 500°C at a rate of 2°C / min, the calcination time is 3h, the obtained solid product is placed in a tubular furnace for reduction, the reduction temperature is increased to 350°C at a rate of 2°C / min, the calcination time is 3h, and the product Cu / MgO-CoO-2 is obtained;
[0133] S4, 0.05 mL furfural, 0.05 g Cu / MgO-CoO-2, 5 mL isopropanol and a high temperature magnet are placed in a 75 mL high temperature and high pressure stainless steel reactor, the air in the reactor is replaced with nitrogen 3 times, and hydrogen is replaced 3 times, the pressure in the high pressure reactor is maintained at 2 MPa, and heated and stirred at 100 ° C for 60 min;
[0134] S5. After the reaction is completed, the mixture is allowed to stand and cool to room temperature. The product furfuryl alcohol is obtained by centrifugal separation, and the catalyst Cu / MgO-CoO-2 is recovered. The catalyst phase is directly recycled without post-treatment. The furfural conversion rate is 55.5%, and the furfuryl alcohol yield is 21.4%.
[0135] Comparative Example 9
[0136] S1. Mix 0.21 g CuSO4·5H2O and 5.0 mL deionized water in a 10.0 mL beaker, stir until the solid is dissolved, add the oxide support, then add 0.5 g MgO and 0.82 g Nb2O5, ultrasonicate for 10 min, stir at room temperature, and keep for 8 h to obtain the corresponding mixed solution;
[0137] S2, stop the above stirring, let it stand overnight for 12 hours, and then place it in an oven at 80°C to dry for 6 hours;
[0138] S3, calcining the dried product in a muffle furnace, the calcination temperature is increased to 500°C at a rate of 2°C / min, the calcination time is 3h, the obtained solid product is placed in a tubular furnace for reduction, the reduction temperature is increased to 350°C at a rate of 2°C / min, the calcination time is 3h, and the product Cu / MgO-Nb2O5-2 is obtained;
[0139] S4, 0.05 mL furfural, 0.05 g Cu / MgO-Nb2O5-2, 5 mL isopropanol and high temperature magnetron were placed in a 75 mL high temperature and high pressure stainless steel reactor, the air in the reactor was replaced with nitrogen 3 times, and hydrogen was replaced 3 times, the pressure in the high pressure reactor was maintained at 2 MPa, and heated and stirred at 100 ° C for 60 min;
[0140] S5. After the reaction is completed, the mixture is allowed to stand and cool to room temperature. The product furfuryl alcohol is obtained by centrifugal separation, and the catalyst Cu / MgO-Nb2O5-2 is recovered. The catalyst phase is directly recycled without post-treatment. The furfural conversion rate is 44.5%, and the furfuryl alcohol yield is 15.4%.
[0141] Comparative Example 10
[0142] S1. Mix 0.21 g CuSO4·5H2O and 5.0 mL deionized water in a 10.0 mL beaker, stir until the solid is dissolved, add the oxide support, then add 0.5 g MgO, ultrasonicate for 10 min, stir at room temperature, and keep for 8 h to obtain the corresponding mixed solution;
[0143] S2, stop the above stirring, let it stand overnight for 12 hours, and then place it in an oven at 80°C to dry for 6 hours;
[0144] S3, calcining the dried product in a muffle furnace, the calcination temperature is increased to 500° C. at a rate of 2° C. / min, the calcination time is 3 h, the obtained solid product is placed in a tubular furnace for reduction, the reduction temperature is increased to 300° C. at a rate of 2° C. / min, the calcination time is 3 h, and the product Cu / MgO is obtained;
[0145] S4, 0.05 mL furfural, 0.05 g Cu / MgO, 5 mL isopropanol and a high temperature magnet are placed in a 75 mL high temperature and high pressure stainless steel reactor, the air in the reactor is replaced with nitrogen three times, and hydrogen is replaced three times, the pressure in the high pressure reactor is maintained at 2 MPa, and heated and stirred at 100 ° C for 40 min;
[0146] S5. After the reaction is completed, the mixture is allowed to stand and cool to room temperature. The product furfuryl alcohol is obtained by centrifugal separation, and the catalyst Cu / MgO is recovered. The catalyst phase is directly recycled without post-treatment. The furfural conversion rate is 56.2%, and the furfuryl alcohol yield is 36.8%.
[0147] Test example:
[0148] Attached Figure 1 The preparation steps of Cu / MgO-La2O3-X supported catalyst are as follows: a certain amount of copper precursor is dissolved in deionized water, and then magnesium oxide support and lanthanum oxide (X = n Mg :n La =2, 4, 6, 8); ultrasonically treating the mixture, stirring, standing, and drying in an oven; grinding the obtained mixture solid into powder and calcining it in a muffle furnace; transferring the obtained target product solid powder to a tube furnace for reduction, and finally obtaining the target product Cu / MgO-La2O3-X.
[0149] Attached Figure 2 The TEM images of Cu / MgO-La2O3-2, Cu / MgO-La2O3-4, Cu / MgO-La2O3-6 and Cu / MgO-La2O3-8 catalysts shown in Figure 2 have metal NPs size distributions of 3.75±0.35nm, 2.75±0.065nm, 2.25±0.11nm and 2.75±0.26nm, respectively. It can be concluded that the metal dispersion of Cu / MgO-La2O3-6 catalyst is the best.
[0150] The HR-TEM image of Cu / MgO-La2O3-6 shows lattice fringes with a lattice spacing of 0.209 nm, confirming the presence of the typical lattice spacing of metallic Cu(111). At the same time, the characteristic lattice spacing of MgO and La2O3 was observed, with lattice spacings of 0.149 nm and 0.338 nm, respectively, confirming that no new MgLaO was generated in the Cu / MgO-La2O3-X catalyst. x Mutually.
[0151] In addition, EDS characterization shows that the distribution of Cu, Mg, O and La on the surface of Cu / MgO-La2O3-6 catalyst ( Figure 3 ). The smaller range of La element indicates that La is most likely concentrated on the surface of the support MgO, while Cu is more evenly distributed throughout the catalyst.
[0152] Attached Figure 4X-ray diffraction analysis of Cu / MgO, Cu / MgO-La2O3-2, Cu / MgO-La2O3-4, Cu / MgO-La2O3-6 and Cu / MgO-La2O3-8 shown in the figure determined the physical phase and crystal properties of the prepared catalysts. The strong reflection peaks at 2θ=36.86°, 42.82°, 62.16°, 74.51° and 78.44° correspond to the (111), (200), (220), (311) and (222) crystal planes of MgO, respectively (JCPDS71-1176). With the increase of Mg / La molar ratio, the intensity of MgO diffraction peak gradually increases, which indicates that La has good dispersion on the MgO surface. At the same time, no new MgLaOx phase exists in Cu / MgO-La2O3-X catalyst.
[0153] In order to further confirm that La plays a positive role in the reduction of Cu species in Cu / MgO-La2O3-X samples, H2-TPR test results were performed on them. Figure 5 Compared with Cu / MgO, the Cu / MgO-La2O3-X catalyst has 2+ The reduction peak of CuO shifts from 320°C to 250°C. Therefore, the introduction of La weakens the interaction between CuO and MgO, making it easier for CuO to be reduced to Cu 0 Combined with the TEM analysis results, it was determined that the structure of the Cu / MgO-La2O3-X catalyst is composed of MgO loaded with La2O3 as the carrier, and some uniformly dispersed metal Cu particles on its surface. In addition, the catalyst mainly contains MgO, and some Cu is distributed at the interface between La2O3 and MgO. 0 Therefore, the three different forms of Cu 0 The reduction peak of Cu / MgO-La2O3-X at around 450℃ may be due to the presence of Cu hidden at the interface between La2O3 and MgO. 2+ The reduction of can only be reduced at a higher temperature due to its strong interaction with the support. This is also confirmed by XPS analysis ( Figure 7 ) in the catalyst, when it was reduced at 300 °C, some Cu 2+ However, the reduction peaks near 550 °C and 700 °C correspond to the CO2 desorption peaks generated by the decomposition of La2O3 in the support.
[0154] Application testing:
[0155] Catalytic Performance of Cu / MgO-La2O3-X Supported Catalysts for Furfural Hydrogenation
[0156] First, a series of different Cu-based catalyst supports were used to test the catalytic performance of FAL selective hydrogenation under the same reaction conditions (e.g. Figure 6 a). Compared with other Cu-based catalysts doped with different carrier properties (acidic, basic, neutral), Cu / MgO-La2O3 has a conversion of 66.9% for FAL and a selectivity of 78.4% for FOL. Therefore, La2O3 carrier was used as the doping carrier for the next study.
[0157] In order to further optimize the catalytic performance of Cu / MgO-La2O3 catalyst, the effect of Mg:La ratio on the selective hydrogenation reaction of FAL was studied (e.g. Figure 6 b) The Cu loading was fixed at 5% to prepare the catalyst Cu / MgO-La2O3-X (X = n Mg :n La =2, 4, 6, 8), as in Example 1 to Example 4. When the Mg / La molar ratio is increased from 1:1 to 6:1, the conversion of FAL is increased from 66.4% to 93.6%, and the yield of FOL is increased from 73.9% to 94.1%. When the Mg / La molar ratio is further increased to 8, the conversion of FAL decreases slightly (82.6%), and the yield of FOL is only 90.7%.
[0158] The results show that the increase of Mg / La ratio is beneficial to the formation of product FOL. However, excessive La leads to a decrease in FOL selectivity. Therefore, the effect of Mg / La ratio on the structure of Cu / MgO-La2O3-X catalysts needs to be further studied to determine its effect on the selective hydrogenation reaction of FAL.
[0159] Cu / MgO-La2O3-X is a bifunctional catalyst mainly composed of metal nanoparticles and alkaline carriers. The former can dissociate H2 molecules into H atoms for subsequent hydrogenation reactions, and the latter provides a site for the selective adsorption of reactants. Therefore, the properties of the active components and the carrier play a decisive role in the product distribution of the selective hydrogenation of furfural. According to the analysis of multiple characterization data, the reason why LA-6 has excellent catalytic activity is mainly attributed to the fact that the addition of La is beneficial to improve the dispersion of Cu and promote the reduction of metallic Cu. According to the XPS and H2-TPR results (such as Figure 7 and Figure 5 As shown), La doping greatly increases Cu 0 The ratio is more than twice that of LA-0. At the same time, the size of the metal particles is greatly reduced, which promotes the increase of the active surface area of the catalyst, thereby providing a larger active surface area that is conducive to the strong adsorption of FAL and H2. CO2-TPD characterization ( Figure 8 ) also confirmed that the addition of La increases the strong base sites of the catalyst and promotes the dispersion of Cu metal.
[0160] In summary, La2O3 as a strong alkaline support is the main adsorption site on the FAL catalyst, while the highly dispersed Cu nanoparticles are beneficial to improving the catalyst activity and the selectivity of FOL.
[0161] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A Cu / MgO-M supported catalyst, characterized in that: The main active metal of the supported catalyst is copper, the carrier is the metal oxide MgO, the second carrier M is La2O3; and the molar ratio between Mg and M is 0.1-8.
2. A method for preparing the Cu / MgO-M supported catalyst as claimed in claim 1, characterized in that: The following steps are involved: S1, mixing the metal salt with water, stirring until the solid is dissolved, then adding the oxide carriers MgO and M, ultrasonicating, and stirring to obtain a mixed solution; S2, stop stirring, let stand overnight, and place the mixed solution in an oven to dry; S3. The dried product is calcined in air and reduced under the action of H2 to obtain the Cu / MgO-M supported catalyst.
3. The method for preparing the Cu / MgO-M supported catalyst according to claim 2, characterized in that: In S1, the metal salt is CuSO4·5H2O, the carrier is MgO, the second carrier M is La2O3, and the molar ratio of Mg to M is 0.1-8. The equal volume impregnation method is adopted, the ultrasonic time is 10-30 minutes, and the stirring time is 10-12 hours.
4. The method for preparing the Cu / MgO-M supported catalyst according to claim 2, characterized in that: In S2, the standing time is 8 to 12 hours, the drying temperature is 60 to 80° C., and the drying time is 6 to 8 hours.
5. The method for preparing the Cu / MgO-M supported catalyst according to claim 2, characterized in that: In S3, the dried product is calcined in a muffle furnace with air and reduced in a tube furnace with H2. The specific operation is as follows: The heating rate of the muffle furnace is 1-5°C / min, and the temperature is maintained at 300-600°C for 1-4 hours; the heating rate of the tubular furnace is 1-5°C / min, and the temperature is maintained at 100-600°C for 1-5 hours.
6. Use of the Cu / MgO-M supported catalyst as claimed in claim 1 or the Cu / MgO-M supported catalyst prepared by the method as claimed in claim 2 in the field of catalysis.
7. The use according to claim 6, characterized in that: Application of the Cu / MgO-M supported catalyst in environmental governance and restoration.
8. The use according to claim 7, characterized in that: The Cu / MgO-M supported catalyst catalyzes furfural to prepare furfuryl alcohol.
Citation Information
Patent Citations
Catalyst used in furfuryl alcohol preparation by furfural gas phase hydrogenation and preparation method thereof
CN101423505A
Foam-structure catalyst used in reaction for preparing benzyl alcohol from benzaldehyde through hydrogenation and preparation thereof
CN107442149A
Cu / MxOy / Al2O3 catalyst, preparation method and application thereof in preparing benzyl alcohol
CN109569602A
Application of Cu-based catalyst in preparation of pentanediol by hydrogenolysis of furfuryl alcohol
CN113908841A
Synthesis method of high-dispersity supported catalyst and method for preparing furfuryl alcohol by catalyzing furfural through high-dispersity supported catalyst
CN117019147A