Cobalt hexacyanocobaltate-loaded Co-N-C structure ceramic catalytic membrane and preparation method thereof
Through the Co-N-C structure ceramic catalytic film supported by cobalt hexacyanocobaltate, the problems of low mineralization efficiency and poor stability of the catalytic film are solved, and efficient degradation and mineralization capabilities are achieved, which are suitable for pollutant treatment in actual water bodies.
Patent Information
- Application Number
- CN202411050742.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
The existing catalytic films have low mineralization efficiency, poor stability and catalyst dissolution problems limit their application, making it difficult to effectively treat pollutant-rich wastewater.
The modified ceramic film is formed by using a Co-N-C structured ceramic catalytic film supported by cobalt hexacyanocobaltate through ultrasonic treatment, hydrothermal carbonization reaction and hexacyanocobaltate precipitation. The process is simple and the cost is low, and the catalytic film obtained has high catalytic Activity and stability.
100% removal and 80% mineralization of parachlorobenzoic acid are achieved, with excellent degradation and mineralization capabilities, and can efficiently degrade pollutants under actual water conditions and maintain a removal efficiency of more than 90% during continuous operation.
Smart Images

Figure CN118976537A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of environmental catalytic materials, and in particular relates to a Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate and a preparation method thereof. Background Art
[0002] Anthropogenic organic pollutants are discharged from domestic and industrial wastewater into natural waters, which has caused widespread concern about ecosystem health and human health worldwide. Due to their complex characteristics, these pollutants cannot be effectively removed by traditional wastewater biological treatment processes. At the same time, although some advanced physical and chemical treatment processes (such as adsorption and membrane filtration) can help us enrich and separate these pollutants from wastewater, this also creates another problem: how to treat these pollutant-rich solids and concentrated waste pollutants so that they can be permanently removed from the environment, which is exactly the new challenge we need to face and solve.
[0003] To address this problem, advanced oxidation processes (AOPs) can utilize hydroxyl radicals ( · OH) or sulfate radical (SO4 ·- ) and other active free radicals to efficiently degrade pollutants, and are suitable for a variety of water quality environments. Advanced oxidation technology that uses ceramic catalytic membranes to activate permonosulfate (PMS) to produce active oxygen is considered to be a promising wastewater treatment technology. Membrane catalytic technology effectively avoids the problem of catalyst powder separation and recovery, greatly improving work efficiency; in addition, the membrane treatment method provides a microreactor, which helps to reduce the concentration boundary layer of pollutants and effectively improves the utilization rate of active oxygen species to achieve more efficient wastewater treatment. (Wu, Hong, et al. "Manganese oxide integrated catalytic ceramic membrane for degradation of organic pollutants using sulfate radicals." Water research 167 (2019): 115110). However, the problems of catalyst dissolution or low mineralization efficiency of existing catalytic membranes limit their application. Therefore, it is urgent to develop a ceramic catalytic membrane that has strong stability enhancement and high mineralization efficiency. Summary of the invention
[0004] The purpose of the present invention is to solve the problems of low mineralization efficiency, poor stability and catalyst dissolution of the current catalytic membrane, and to provide a Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate and a preparation method thereof. The preparation method is simple in process and low in cost, and the obtained ceramic catalytic membrane has good catalytic stability and high catalytic activity.
[0005] The specific technical solutions adopted by the present invention are as follows:
[0006] In a first aspect, the present invention provides a method for preparing a Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate, the specific steps of which are as follows:
[0007] S1: immersing the cleaned ceramic membrane in a mixed solution containing a carbon source and a cobalt salt and performing ultrasonic treatment;
[0008] S2: subjecting the ceramic membrane obtained in step S1 and the mixed solution to a hydrothermal carbonization reaction, whereby a cobalt-rich hydrothermal carbon layer is generated on the surface of the ceramic membrane;
[0009] S3: immersing the ceramic membrane with a hydrothermal carbon layer on the surface obtained in step S2 into a hexacyanocobaltate solution, wherein the cobalt ions in the hydrothermal carbon layer react to form cobalt hexacyanocobaltate crystal precipitation, thereby obtaining a modified ceramic membrane;
[0010] S4: washing and calcining the modified ceramic membrane obtained in step S3 to obtain a Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate.
[0011] Preferably, the ceramic membrane in step S1 is a microfiltration ceramic membrane whose matrix is zirconium dioxide and titanium dioxide.
[0012] Preferably, the carbon source in step S1 is glucose, sucrose or starch, and the cobalt salt is cobalt nitrate hexahydrate, cobalt chloride or cobalt acetate.
[0013] Preferably, the mass concentration of glucose in the mixed solution in step S1 is 90-100 mg / mL, and the mass concentration of cobalt nitrate hexahydrate is 45-50 mg / mL.
[0014] Preferably, the hydrothermal carbonization reaction in step S2 is carried out in a high-pressure reactor, the reaction temperature in the high-pressure reactor is 250° C. to 280° C., and the reaction time is 12 to 48 hours.
[0015] Preferably, the hexacyanocobaltate solution in step S3 is a potassium hexacyanocobaltate solution or a sodium hexacyanocobaltate solution.
[0016] Preferably, the mass concentration of the hexacyanocobaltate solution in step S3 is 60-70 mg / mL; and the ceramic membrane having a hydrothermal carbon layer on its surface is immersed in the hexacyanocobaltate solution for 8-12 hours.
[0017] Preferably, in step S4, the modified ceramic membrane is soaked in an ethanol-water solution for at least 3 hours and then repeatedly rinsed with deionized water.
[0018] Preferably, the modified ceramic membrane in step S4 is washed and then calcined in a muffle furnace at a calcination temperature of 300 to 350° C. for a calcination time of 2.5 to 3 hours.
[0019] In a second aspect, the present invention provides a Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate obtained by the preparation method described in the first aspect.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] (1) The method for preparing the Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate provided by the present invention has a simple process, does not require expensive equipment, has low cost, and can be applied to large-scale industrial production.
[0022] (2) The Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate obtained by the preparation method provided by the present invention has atomically dispersed, unsaturated Co II -NC catalytic sites, these rich special structures, make it have better catalytic activity with the reaction substrate during reaction.
[0023] (3) The Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate obtained by the preparation method provided by the present invention can degrade 4-chlorobenzoic acid at 4000 L m -2 h -1 Under high water flux conditions, 100% removal of p-chlorobenzoic acid was achieved, while the conventional TiO2 commercial catalyst could only achieve 20% removal under the same conditions, indicating that the catalytic membrane has excellent degradation ability. -2 h -1 At a flow rate of , 80% of p-chlorobenzoic acid can be completely mineralized into harmless water and carbon dioxide, indicating that the catalytic membrane has excellent mineralization ability.
[0024] (4) The Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate obtained by the preparation method provided by the present invention can achieve efficient degradation of p-chlorobenzoic acid under actual water conditions. The presence of humus, chloride ions and bicarbonate ions has little effect on the degradation efficiency, indicating that it has greater application potential in actual water bodies.
[0025] (5) The Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate obtained by the preparation method provided by the present invention can operate continuously for two weeks and maintain a pollutant removal efficiency of more than 90%, and has the characteristics of high catalytic stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The scanning electron microscope image of the Co-NC structured ceramic catalytic membrane prepared in Example 1 and the corresponding element distribution energy spectrum diagram.
[0027] Figure 2The X-ray diffraction patterns of two ceramic catalyst membrane surface-supported materials include cobalt hexacyanocobaltate (Co-HCC) in Example 1 and a cobalt-carbon mixture (CoC) in the control group.
[0028] Figure 3 This is the X-ray photoelectron spectrum of cobalt hexacyanocobaltate (Co-HCC) on the surface of the Co-NC structure ceramic catalyst membrane prepared in Example 1. Figure a is the full spectrum analysis of Co-HCC, and Figure b is the cobalt element spectrum analysis of Co-HCC.
[0029] Figure 4 This is a diagram showing the effect of using the Co-NC structured ceramic catalytic membrane prepared in Example 1 to degrade p-chlorobenzoic acid in advanced oxidation technology.
[0030] Figure 5 The difference in activation efficiency of peroxymonosulfate of the Co-NC structured ceramic catalytic membrane prepared in Example 1 at different water flux rates.
[0031] Figure 6 This is a diagram showing the effect of the Co-NC structured ceramic catalytic membrane prepared in Example 1 on the mineralization of p-chlorobenzoic acid at different water flux rates.
[0032] Figure 7 The difference in degradation of p-chlorobenzoic acid between the Co-NC structured ceramic catalytic membrane prepared in Example 1 and other different ceramic catalytic membranes in Comparative Example 1 at different water flux flow rates.
[0033] Figure 8 This is a diagram showing the effect of the Co-NC structured ceramic catalytic membrane in Example 2 being used to treat p-chlorobenzoic acid in simulated actual wastewater.
[0034] Fig. 9 The stability of the ceramic catalytic membrane (M_Co-HCC) in removing p-chlorobenzoic acid for two consecutive weeks in Example 3. DETAILED DESCRIPTION
[0035] The present invention is further described and illustrated below in conjunction with the accompanying drawings and specific embodiments. The technical features of each embodiment of the present invention can be combined accordingly without conflicting with each other.
[0036] Example 1
[0037] This embodiment provides a method for preparing a Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate, wherein the specific steps are as follows:
[0038] (1) The ceramic membrane was immersed in a 70% ethanol solution, ultrasonically cleaned for 10 minutes, and rinsed with deionized water. 1.4 g of glucose and 0.7 g of cobalt nitrate hexahydrate were added to 15 mL of deionized water to prepare a mixed solution. The cleaned ceramic membrane was immersed in the above mixed solution and ultrasonically treated for 10 minutes to accelerate the diffusion of glucose and cobalt nitrate hexahydrate in the solution into the pores of the ceramic membrane.
[0039] In this embodiment, the ceramic membrane adopts a microfiltration ceramic membrane whose matrix is zirconium dioxide and titanium dioxide.
[0040] (2) The ceramic membrane and the mixed solution obtained in step (1) were transferred to a 50 mL stainless steel autoclave lined with para-polyphenylene, and then the temperature was raised to 260° C. and a hydrothermal carbonization reaction was carried out under autogenous pressure for 15 h to generate a cobalt-rich hydrothermal carbon layer on the surface of the ceramic membrane.
[0041] (3) The ceramic membrane having a hydrothermal carbon layer on its surface obtained in step (2) is placed in 15 mL of a potassium hexacyanocobaltate solution having a mass concentration of 66.7 mg / L, the ceramic membrane is immersed, and the reaction is carried out for 10 hours, so that the hexacyanocobaltate ions in the solution react and crystallize with the cobalt ions in the pores of the ceramic membrane to form a cobalt hexacyanocobaltate precipitate, thereby obtaining a modified ceramic membrane.
[0042] (4) The modified ceramic membrane obtained in step (3) was immersed in a 70% ethanol solution for 3 h and rinsed with deionized water for 3 times, then placed in a muffle furnace and calcined at 300° C. for 3 h to finally obtain a Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate.
[0043] After the preparation, the Co-NC structure ceramic catalyst membrane prepared in Example 1 was characterized by morphology, and the test analysis results obtained were as follows: Figure 1 to Figure 3 shown.
[0044] Figure 1 The scanning electron microscope image and the corresponding element distribution energy spectrum of the Co-NC structure ceramic catalytic membrane prepared in Example 1 show that cobalt, nitrogen and carbon elements are evenly distributed inside the pores of the ceramic membrane, which means that the synthesized catalyst is very evenly loaded.
[0045] Figure 2 The X-ray diffraction pattern of the cobalt hexacyanocobaltate catalyst on the surface of the Co-NC structure ceramic catalytic membrane prepared in Example 1 has the same characteristic peaks as Co3[Co(CN)6]2, indicating that cobalt hexacyanocobaltate is successfully loaded on the surface of the membrane, indicating that there is a Co-N / C coordination structure on the catalyst surface, in which Co II The site binds to N, Co III The site combines with C to form Co II -N≡C-Co IIIThe X-ray diffraction peak of the crystal plane (200) (I 200 / I220 =1.13) is much smaller than the reference value (I 200 / I 220 =2.35), indicating that there are coordination-unsaturated Co centers on the surface of the supported cobalt hexacyanocobaltate.
[0046] Figure 3 The X-ray photoelectron spectrum of the cobalt hexacyanocobaltate catalyst on the surface of the Co-NC structure ceramic catalytic film prepared in Example 1 shows that nitrogen and two valence states of cobalt (Co 2+) exist on the surface of cobalt hexacyanocobaltate. II ,Co III ), these elements can serve as reactive sites to enhance the activation performance of peroxymonosulfate (PMS).
[0047] Next, the Co-NC structured ceramic catalytic membrane prepared in Example 1 was applied to an advanced oxidation reaction to perform a chlorobenzoic acid degradation test as follows:
[0048] The Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate was used to treat a p-chlorobenzoic acid solution containing PMS, wherein the loading amount of cobalt hexacyanocobaltate catalyst on the ceramic catalytic membrane surface was 12 mg, the p-chlorobenzoic acid concentration was 25 μM, and the PMS concentrations were 0.1, 0.5, 1.0 and 2.5 mM, respectively, at 100, 500, 1000, 2000 and 4000 L / (m 2 h) and take samples at the water flux to determine the concentration of p-chlorobenzoic acid.
[0049] The results are as follows Figure 4 As shown in Figure 2, when the PMS concentration is 2.5 mM, even if the water flux increases to 4000 L / (m 2 h), the Co-NC structured ceramic catalytic membrane can still achieve a removal rate of more than 90% of p-chlorobenzoic acid. This means that the Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate can almost completely remove p-chlorobenzoic acid within 0.64s in advanced oxidation applications.
[0050] The PMS residue in the water treated by Co-NC structured ceramic catalytic membrane at different water fluxes was further compared. Figure 5 As shown, the water flux is 10 / (m 2 h), the Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate can activate more than 80% of PMS, and the utilization efficiency of PMS is very high.
[0051] The total organic carbon (TOC) in the treated water was further measured to evaluate the mineralization efficiency of the Co-NC structured ceramic catalytic membrane. Figure 6As shown, when the water flux is 10 / (m 2 h), the Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate can completely degrade about 80% of p-chlorobenzoic acid into CO2, and the required reaction residence time is only 255 seconds. Further results show that when the water flux is reduced to 5LMH, a 90% mineralization rate of p-chlorobenzoic acid can be achieved. Through fitting, its first-order reaction kinetics is about 0.005s -1 .
[0052] Comparative Example 1
[0053] The comparative examples used other different ceramic catalytic membranes, including the ceramic membrane M0 in the initial state before modification, the ceramic membrane M_CoC loaded with cobalt carbon catalyst commonly used in the literature, and the ceramic membrane M_Co-HCC of the Co-NC structured ceramic catalytic membrane (M_Co-HCC) prepared in Example 1 before calcination. pre .
[0054] The Co-NC structured ceramic catalytic membrane prepared in Example 1 and other ceramic catalytic membranes in the comparative example were respectively applied to the advanced oxidation reaction to carry out the degradation test of p-chlorobenzoic acid, as follows:
[0055] Different ceramic catalytic membranes were used to treat p-chlorobenzoic acid solution containing PMS. The loading amount of cobalt hexacyanocobaltate catalyst on the ceramic catalytic membrane was 12 mg, the p-chlorobenzoic acid concentration was 25 μM, and the PMS concentrations were 0.1, 0.5, 1.0 and 2.5 mM, respectively. The reaction conditions were 100, 500, 1000, 2000 and 4000 L / (m 2 h) and take samples at the water flux to determine the concentration of p-chlorobenzoic acid.
[0056] The results are as follows Figure 7 As shown, compared with other different ceramic catalytic membranes in the comparative examples, the Co-NC structured ceramic catalytic membrane (M_Co-HCC) loaded with cobalt hexacyanocobaltate prepared in Example 1 has significant advantages in degrading p-chlorobenzoic acid at various water fluxes. In contrast, the unmodified ceramic membrane and other ceramic membranes loaded with carbon-based cobalt materials failed to effectively remove p-chlorobenzoic acid.
[0057] Example 2
[0058] This example uses the Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate prepared in Example 1 to treat p-chlorobenzoic acid in simulated actual wastewater. The experimental setup is as follows:
[0059] Prepare a mixed solution containing 500 mg / L sodium chloride, 25 μM p-chlorobenzoic acid and 2.5 mM PMS, denoted as pCBA+Cl -A mixed solution containing 50 mg / L humic acid, 25 μM p-chlorobenzoic acid and 2.5 mM PMS was prepared, which was recorded as pCBA+NOM. A mixed solution containing 100 mg / L sodium bicarbonate, 5 μM p-chlorobenzoic acid and 2.5 mM PMS was prepared, which was recorded as pCBA+HCO3 - The Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate was used to treat the above mixed solutions. The experimental results are shown in Figure 8 shown.
[0060] The results show that the concentrations of natural organic matter, chloride ions and bicarbonate in real water have little effect on the degradation of chlorobenzoic acid by the Co-NC structured ceramic catalytic membrane prepared in this embodiment. The Co-NC structured ceramic catalytic membrane can still achieve a 95.4±2.2% removal rate of chlorobenzoic acid in chlorine-containing wastewater, a 90.2±1.9% removal rate of chlorobenzoic acid in wastewater containing humic acid, and a 95.4±2.1% removal rate of chlorobenzoic acid in wastewater containing bicarbonate. This shows that the Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate shows good tolerance to wastewater containing chloride ions and natural organic matter in practical applications.
[0061] Example 3
[0062] In this example, the Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate prepared in Example 1 was used to conduct a performance stability test. The experimental settings are as follows: the catalyst loading on the membrane surface is 12 mg, the concentration of p-chlorobenzoic acid is 25 μM, the concentration of PMS is 2.5 mM, and the water flux is 10 L / (m 2 h), the membrane catalytic device was operated for two consecutive weeks to detect the concentration of p-chlorobenzoic acid in the treated water to verify the stability of the Co-NC structure ceramic catalytic membrane. The experimental results are as follows Fig. 9 As shown, the Co-NC structured ceramic catalytic membrane can operate stably for two weeks, maintaining a p-chlorobenzoic acid removal rate of more than 90%. This shows that the Co-NC structured ceramic catalytic membrane prepared in Example 1 has good stability and high catalytic performance.
[0063] The above-described embodiment is only a preferred solution of the present invention, but it is not intended to limit the present invention. A person skilled in the relevant technical field may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, any technical solution obtained by equivalent replacement or equivalent transformation falls within the protection scope of the present invention.
Claims
1. A method for preparing a Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate, characterized in that: The specific steps are as follows: S1: immersing the cleaned ceramic membrane in a mixed solution containing a carbon source and a cobalt salt and performing ultrasonic treatment; S2: subjecting the ceramic membrane obtained in step S1 and the mixed solution to a hydrothermal carbonization reaction, whereby a cobalt-rich hydrothermal carbon layer is generated on the surface of the ceramic membrane; S3: immersing the ceramic membrane with a hydrothermal carbon layer on the surface obtained in step S2 into a hexacyanocobaltate solution, wherein the cobalt ions in the hydrothermal carbon layer react to form cobalt hexacyanocobaltate crystal precipitation, thereby obtaining a modified ceramic membrane; S4: washing and calcining the modified ceramic membrane obtained in step S3 to obtain a Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate.
2. The method for preparing the Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate according to claim 1, characterized in that: The ceramic membrane in step S1 is a microfiltration ceramic membrane whose matrix is zirconium dioxide and titanium dioxide.
3. The method for preparing the Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate according to claim 1, characterized in that: In step S1, the carbon source is glucose, sucrose or starch, and the cobalt salt is cobalt nitrate hexahydrate, cobalt chloride or cobalt acetate.
4. The method for preparing the Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate according to claim 1, characterized in that: The mass concentration of glucose in the mixed solution in step S1 is 90-100 mg / mL, and the mass concentration of cobalt nitrate hexahydrate is 45-50 mg / mL.
5. The method for preparing the Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate according to claim 1, characterized in that: The hydrothermal carbonization reaction described in step S2 is carried out in a high-pressure reactor, the reaction temperature in the high-pressure reactor is 250° C. to 280° C., and the reaction time is 12 to 48 hours.
6. The method for preparing the Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate according to claim 1, characterized in that: The hexacyanocobaltate solution in step S3 is a potassium hexacyanocobaltate solution or a sodium hexacyanocobaltate solution.
7. The method for preparing the Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate according to claim 1, characterized in that: The mass concentration of the hexacyanocobaltate solution in step S3 is 60-70 mg / mL; the ceramic membrane having a hydrothermal carbon layer on its surface is immersed in the hexacyanocobaltate solution for 8-12 hours.
8. The method for preparing the Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate according to claim 1, characterized in that: In step S4, the modified ceramic membrane is soaked in an ethanol aqueous solution for at least 3 hours and then repeatedly rinsed with deionized water.
9. The method for preparing the Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate according to claim 1, characterized in that: The modified ceramic membrane in step S4 is washed and then placed in a muffle furnace for calcination at a temperature of 300 to 350° C. for a calcination time of 2.5 to 3 hours.
10. A Co-NC structured ceramic catalytic membrane loaded with cobalt hexacyanocobaltate obtained by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Cobalt ferrite-supported graphene aerogel catalyst and preparation method thereof
CN110102303A
Simple preparation method of Co / CM ceramic catalytic membrane
CN113289666A
Preparation method of nano cobalt hexacyanocobaltate / nitrogen-doped porous carbon composite material
CN113548679A
Preparation method and application of photocatalytic ceramic membrane and water treatment method
CN115193469A
Cited By
Method for selectively removing lead ions in perovskite solar cell leachate
CN122254626A