Preparation method of non-stick pan coating

By roughening the surface of the pot with sandblasting and electrochemical nickel plating, combined with spraying a mixed solution of specific components, the problems of insufficient temperature resistance, corrosion resistance and hardness of non-stick pot coatings are solved, and the uniformity and durability of the coating are improved.

CN118976681AInactive Publication Date: 2024-11-19ZHAOQING HONGWANG METAL IND
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411127344.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing non-stick cookware coatings suffer from insufficient temperature resistance, chemical resistance, corrosion resistance, and hardness, and the coating thickness is uneven, affecting service life and quality.

Method used

After roughening and sandblasting the surface of the pot, electrochemical nickel plating is performed to ensure a smooth surface. Then, a mixed solution of components such as organosilicon resin, modified silicon carbide, and nano-calcium carbonate is prepared, sprayed, and dried to form a non-stick coating.

Benefits of technology

It improves the heat resistance, corrosion resistance and hardness of the non-stick coating, ensures coating uniformity, extends service life and enhances the user experience.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976681A_ABST
    Figure CN118976681A_ABST
Patent Text Reader

Abstract

The invention discloses a non-stick pan coating preparation method which comprises the following steps: step 1, selecting and cleaning a base material, selecting a proper pan body, removing dirt on the surface of the pan body, and performing roughening sand blasting treatment on the surface of the pan body by adopting silicon carbide ceramic; the non-stick pan coating has the beneficial effects that a layer of nickel is electroplated on the surface of the pan body in advance before spraying, so that the surface of the pan body is flat and smooth before being coated with the non-stick pan coating, meanwhile, the adhesion force of the non-stick pan coating after coating can be increased, the non-stick pan coating is prevented from easily falling off after coating, and the service life of the non-stick pan coating is prolonged. Meanwhile, organic silicon resin, modified silicon carbide, nano calcium carbonate and other components are mixed according to a specific proportion, so that the defects of the organic silicon resin are overcome after the non-stick pan coating is coated, the prepared non-stick pan coating has good high-temperature resistance and corrosion resistance, meanwhile, the non-stick pan coating further has good hardness and wear resistance, and the service life of the non-stick pan coating is prolonged. Therefore, the service life of the non-stick pan coating is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of non-stick pan coating preparation, and in particular to a method for preparing a non-stick pan coating. Background Art

[0002] Metal pots have long been the most commonly used food cooking tools. They are prone to causing food to stick to the pot, burn, and other problems, which are harmful to human health. Since the 1960s, non-stick pans have begun to enter family life. The main principle is: spray a layer of non-stick coating with polytetrafluoroethylene as the main raw material on the surface of the pot body, and sinter at a high temperature of 420°C to make the non-stick coating tightly bonded to the substrate. The strong chemical inertness of the non-stick coating is used to separate the food and the pot body, thereby achieving a non-stick effect. However, PFOA is used as a raw material in the production process of polytetrafluoroethylene, which may be harmful to the human body and the environment, and once caused panic among consumers. For this reason, it is necessary to research and develop green and environmentally friendly non-stick cookware coatings that are harmless to the human body and the environment.

[0003] Among the many types of non-stick pan coatings, silicone resin non-stick pan coatings are the most environmentally friendly. Since this type of coating does not contain fluorine, it avoids the disadvantage that fluorine-containing coatings cannot be used in acidic environments. However, although silicone resin has excellent thermal oxidation stability, electrical insulation performance and non-stick properties, pure silicone resin also has some disadvantages, such as poor temperature resistance, chemical resistance, corrosion resistance and low hardness. In addition, although polyester-modified silicone resin can improve some of the shortcomings of silicone resin, new problems will arise. For example, the hardness of silicone resin after modification is not improved much, the heat resistance is very poor when the silicone resin content is low, and the cost of high-performance modified resins is still very high. At the same time, silicone resin non-stick pan coatings are prone to uneven coating thickness at various parts of the pan surface after coating due to the uneven surface of the pan body during coating, which makes the quality of the non-stick pan coating after spraying preparation poor. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a non-stick pan coating in order to solve the above-mentioned problem.

[0005] The present invention achieves the above-mentioned purpose through the following technical solutions:

[0006] A method for preparing a non-stick pan coating comprises the following steps:

[0007] Step 1: Select and clean the base material, choose a suitable pot body, remove the dirt on the surface of the pot body, and use silicon carbide ceramics to roughen the surface of the pot body by sandblasting;

[0008] Step 2: Smooth the surface of the substrate and place the pot body in a nickel plating solution for electrochemical nickel plating to ensure that the surface of the substrate is evenly coated with a layer of nickel;

[0009] Step 3: Preparation of non-stick pan solution: putting silicone resin, modified silicon carbide, nano calcium carbonate, mica powder, amino resin, dispersant and solvent into a mixer in sequence for mixing and stirring to obtain a non-stick pan mixed solution;

[0010] Step 4: Place the substrate treated in step 2 in a spraying room and spray for 15-25 minutes at 220-260°C to prepare the non-stick coating on the pan body.

[0011] Furthermore, the roughening sandblasting treatment in step 1 can further remove the oxide scale on the surface of the pot body. While removing the oxide scale, a microscopic concave-convex structure can be formed on the surface of the pot body to ensure the adhesion strength of the subsequent nickel layer.

[0012] Furthermore, the purpose of nickel plating in step 2 is to ensure that the surface of the pan body is flat, thereby ensuring that the thickness of the subsequent non-stick pan coating is consistent after spraying.

[0013] Furthermore, the contents of the components in the nickel plating solution in step 2 are as follows: 220-240 parts of nickel sulfate, 50-55 parts of sodium citrate, 55-70 parts of ammonium chloride, 70-85 parts of sodium hyposulfite, and 100-300 parts of deionized water.

[0014] Furthermore, the preferred content of each component in the nickel plating solution in step 2 is as follows: 220 parts of nickel sulfate, 52 parts of sodium citrate, 60 parts of ammonium chloride, 75 parts of sodium hyposulfite, and 250 parts of deionized water. By strictly controlling the content of each component in the nickel plating solution, the uniformity and completeness of the thickness of the nickel layer on the surface of the pot body can be ensured.

[0015] Furthermore, the contents of the components in the non-stick pan solution in step 3 are as follows: 120-180 parts of silicone resin, 130-160 parts of modified silicon carbide, 60-80 parts of nano calcium carbonate, 40-50 parts of mica powder, 12-25 parts of amino resin, 2-4 parts of dispersant, and 25-45 parts of solvent.

[0016] Furthermore, the preferred content of each component in the non-stick pan solution in step 3 is as follows: 150 parts of silicone resin, 135 parts of modified silicon carbide, 70 parts of nano calcium carbonate, 45 parts of mica powder, 20 parts of amino resin, 3 parts of dispersant, and 35 parts of solvent. By strictly controlling the content of each component in the non-stick pan solution, the heat resistance, corrosion resistance and thermal conductivity of the coating after coating can be ensured without using polytetrafluoroethylene materials.

[0017] Furthermore, in step 3, the modified silicon carbide is prepared by mixing carbon nanoparticles with silicon powder, placing the mixed materials in a vacuum tank and sealing them, and grinding and configuring them after introducing argon gas.

[0018] Furthermore, the preferred spraying temperature in step 4 is 240° C., and the preferred drying time is 20 minutes. By strictly controlling the drying temperature and time, the efficiency of coating preparation can be accelerated while ensuring that the coating is completely dried.

[0019] The beneficial effects of the present invention are:

[0020] The present invention pre-plates a layer of nickel on the surface of the pot body before spraying, so that the surface of the pot body is smooth and clean before the non-stick coating is applied, and at the same time, the adhesion strength of the non-stick coating after application is increased to prevent the non-stick coating from falling off easily after application. At the same time, by mixing organic silicone resin with modified silicon carbide and nano calcium carbonate and other components in a specific proportion, the non-stick coating overcomes the disadvantages of the organic silicone resin after application, so that the non-stick coating has good high temperature resistance and corrosion resistance after preparation, and also has good hardness and wear resistance, is not easy to be damaged, and the service life of the non-stick coating is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The present invention is a flow chart of a method for preparing a non-stick pan coating. DETAILED DESCRIPTION

[0022] A method for preparing a non-stick pan coating comprises the following steps:

[0023] Step 1: Select and clean the base material, choose a suitable pot body, remove the dirt on the surface of the pot body, and use silicon carbide ceramics to roughen the surface of the pot body by sandblasting;

[0024] Step 2: Smooth the surface of the substrate and place the pot body in a nickel plating solution for electrochemical nickel plating to ensure that the surface of the substrate is evenly coated with a layer of nickel;

[0025] Step 3: Preparation of non-stick pan solution: putting silicone resin, modified silicon carbide, nano calcium carbonate, mica powder, amino resin, dispersant and solvent into a mixer in sequence for mixing and stirring to obtain a non-stick pan mixed solution;

[0026] Step 4: Place the substrate treated in step 2 in a spraying room and spray for 15-25 minutes at 220-260°C to prepare the non-stick coating on the pan body.

[0027] In this embodiment, the roughening sandblasting treatment in step 1 can further remove the oxide scale on the surface of the pot body. While removing the oxide scale, a microscopic concave-convex structure can be formed on the surface of the pot body to ensure the adhesion strength of the subsequent nickel layer.

[0028] In this embodiment, the purpose of nickel plating in step 2 is to ensure that the surface of the pan body is flat, thereby ensuring that the thickness of the subsequent non-stick pan coating is consistent after spraying.

[0029] In this embodiment, the contents of the components in the nickel plating solution in step 2 are as follows: 220-240 parts of nickel sulfate, 50-55 parts of sodium citrate, 55-70 parts of ammonium chloride, 70-85 parts of sodium hyposulfite, and 100-300 parts of deionized water.

[0030] In this embodiment, the preferred content of each component in the nickel plating solution in step 2 is as follows: 220 parts of nickel sulfate, 52 parts of sodium citrate, 60 parts of ammonium chloride, 75 parts of sodium hyposulfite, and 250 parts of deionized water. By strictly controlling the content of each component in the nickel plating solution, the uniformity and completeness of the thickness of the nickel layer on the surface of the pot body can be ensured.

[0031] In this embodiment, the contents of the components in the non-stick pan solution in step 3 are as follows: 120-180 parts of silicone resin, 130-160 parts of modified silicon carbide, 60-80 parts of nano calcium carbonate, 40-50 parts of mica powder, 12-25 parts of amino resin, 2-4 parts of dispersant, and 25-45 parts of solvent.

[0032] In this embodiment, the preferred content of each component in the non-stick pan solution in step 3 is as follows: 150 parts of silicone resin, 135 parts of modified silicon carbide, 70 parts of nano calcium carbonate, 45 parts of mica powder, 20 parts of amino resin, 3 parts of dispersant, and 35 parts of solvent. By strictly controlling the content of each component in the non-stick pan solution, the heat resistance, corrosion resistance and thermal conductivity of the coating after coating can be ensured without using polytetrafluoroethylene materials.

[0033] In this embodiment, the modified silicon carbide in step 3 is to mix carbon nanoparticles with silicon powder, seal the mixed materials in a vacuum tank, and grind and configure after introducing argon gas.

[0034] In this embodiment, the preferred spraying temperature in step 4 is 240° C., and the preferred drying time is 20 minutes. By strictly controlling the drying temperature and time, the efficiency of coating preparation can be accelerated while ensuring that the coating is completely dried.

[0035] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a non-stick pan coating, characterized in that: It includes the following steps: Step 1: Select and clean the base material, choose a suitable pot body, remove the dirt on the surface of the pot body, and use silicon carbide ceramics to roughen the surface of the pot body by sandblasting; Step 2: Smooth the surface of the substrate and place the pot body in a nickel plating solution for electrochemical nickel plating to ensure that the surface of the substrate is evenly coated with a layer of nickel; Step 3: Preparation of non-stick pan solution: putting silicone resin, modified silicon carbide, nano calcium carbonate, mica powder, amino resin, dispersant and solvent into a mixer in sequence for mixing and stirring to obtain a non-stick pan mixed solution; Step 4: Place the substrate treated in step 2 in a spraying room and spray for 15-25 minutes at 220-260°C to prepare the non-stick coating on the pan body.

2. The method for preparing a non-stick pan coating according to claim 1, characterized in that: The roughening sandblasting treatment in step 1 can further remove the oxide scale on the surface of the pot body.

3. The method for preparing a non-stick pan coating according to claim 1, characterized in that: The purpose of nickel plating in step 2 is to ensure that the surface of the pan body is flat, thereby ensuring that the thickness of the subsequent non-stick pan coating is consistent after spraying.

4. The method for preparing a non-stick pan coating according to claim 1, characterized in that: The contents of the components in the nickel plating solution in step 2 are as follows: 220-240 parts of nickel sulfate, 50-55 parts of sodium citrate, 55-70 parts of ammonium chloride, 70-85 parts of sodium hyposulfite, and 100-300 parts of deionized water.

5. The method for preparing a non-stick pan coating according to claim 4, characterized in that: The preferred contents of the components in the nickel plating solution in step 2 are as follows: 220 parts of nickel sulfate, 52 parts of sodium citrate, 60 parts of ammonium chloride, 75 parts of sodium hyposulfite, and 250 parts of deionized water.

6. The method for preparing a non-stick pan coating according to claim 1, characterized in that: The contents of the components in the non-stick pan solution in step 3 are as follows: 120-180 parts of silicone resin, 130-160 parts of modified silicon carbide, 60-80 parts of nano calcium carbonate, 40-50 parts of mica powder, 12-25 parts of amino resin, 2-4 parts of dispersant, and 25-45 parts of solvent.

7. The method for preparing a non-stick pan coating according to claim 6, characterized in that: The preferred contents of the components in the non-stick pan solution in step 3 are as follows: 150 parts of silicone resin, 135 parts of modified silicon carbide, 70 parts of nano calcium carbonate, 45 parts of mica powder, 20 parts of amino resin, 3 parts of dispersant, and 35 parts of solvent.

8. The method for preparing a non-stick pan coating according to claim 1, characterized in that: In step 3, the modified silicon carbide is prepared by mixing carbon nanoparticles with silicon powder, placing the mixed materials in a vacuum tank and sealing them, and grinding and configuring them after introducing argon gas.

9. The method for preparing a non-stick pan coating according to claim 1, characterized in that: The preferred spraying temperature in step 4 is 240° C., and the preferred drying time is 20 min.

Citation Information

Patent Citations

  • High-temperature-resistant abrasion-resistant non-stick pan coating, preparation method and non-stick pan with same

    CN105567066A

  • Nonstick pan coating layer, and production method and nonstick pan thereof

    CN105925176A