Preparation method and application of low-cost high-performance metal powder core wire

By adding binder and annealing treatment to the filler of the powder core wire material, combined with multi-pass isothermal rolling, the high cost and uncontrollable composition problems in the existing powder core wire material preparation methods are solved, and low cost is achieved , high-performance metal powder core wire preparation, suitable for a variety of materials and processes.

CN118976796AInactive Publication Date: 2024-11-19XIAN RARE METAL MATERIALS RES INST CO LTD

Patent Information

Application Number
CN202411455500.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-18
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing preparation methods for powder core wire materials have high costs and limitations in material types. The non-spherical powder mixed powder has uncontrollable components and non-uniformity due to differences in fluidity, which cannot meet the preparation needs of high hardness and brittle materials.

Method used

Add binder to the filler of the metal powder core wire material, and obtain a semi-solid mixture through refining and mixing to ensure fluidity and uniformity. Combined with annealing treatment and multi-pass isothermal rolling, reducing the morphology of the metal powder and particle size requirements to improve moldability.

Benefits of technology

It reduces powder costs, solves the composition and uniformity problems, is suitable for the preparation of a variety of materials, improves the performance and moldability of wire materials, and is suitable for welding, high-energy beam cladding or additive manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976796A_ABST
    Figure CN118976796A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a low-cost and high-performance metal powder core wire, which comprises the following steps: 1, selecting a metal belt as the outer skin of the metal powder core wire, and filling materials comprise metal powder and a binding agent; 2, metal powder and a binder are subjected to banburying and uniform mixing, and a semi-solid mixture is obtained; thirdly, the metal belt is annealed and then rolled into a U-shaped groove, then the semi-solid mixture is fed into the U-shaped groove, and a thick wire is obtained through rolling and closing of a roller; and fourthly, the thick wire is subjected to multi-pass isothermal rolling so that the diameter can be gradually reduced, and the metal powder core wire is obtained. The binder is added into the filler, so that the mixing uniformity of the metal powder and the mobility of the filler are guaranteed, the filling effect of the filler is improved, the performance of the metal powder core wire is further guaranteed, the requirements for the morphology, the particle size and the material of the metal powder are reduced, the powder cost is greatly reduced, and the service life of the metal powder core wire is prolonged. And the obtained metal powder core wire is suitable for welding, high-energy beam cladding or additive manufacturing, the application range is wide, and the practical value is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of new materials, and in particular to a preparation method of a low-cost and high-performance metal powder core wire and application thereof. Background Art

[0002] With the rapid development of manufacturing industries such as navigation, weapons, and oil extraction, the requirements for the service environment and performance of key parts are becoming more and more stringent. Traditional metal materials can no longer meet the use requirements. There is an urgent need to develop new materials with higher hardness, wear resistance, high temperature resistance, oxidation resistance, corrosion resistance, and fatigue resistance. The research mainly focuses on the use of welding or high-energy beam heat sources (laser / electron beam / arc / plasma arc) to prepare coatings with special properties on the surface of traditional metals, and even directly use high-energy beam heat sources to prepare parts with wire additive manufacturing. Welding and wire additive manufacturing both require welding wire, but the traditional solid welding wire has a long processing cycle and is difficult to adjust the composition. Some high-hardness materials have high hardness and high brittleness, causing their metal strips to crack during processing, making it impossible to prepare welding wire. Therefore, many researchers focus on the study of powder core wire.

[0003] At present, the preparation method of powder core wire is mainly to feed the pre-alloyed powder or mixed powder into a metal belt with a U-shaped groove through a conveyor belt, and then prepare it into welding wire after multiple rolling or drawing. In order to ensure the smooth transportation of powder on the conveyor belt, the pre-alloyed powder generally uses spherical powder of 120μm~250μm with good fluidity, but the preparation cost of spherical powder is high; and some materials with high hardness or large brittleness cannot prepare spherical powder, which makes it impossible for many materials with excellent performance to be prepared into welding wire, which seriously limits the preparation and application of wire parts. Some researchers have tried to use non-spherical powder as powder core, but due to the poor fluidity of non-spherical powder, especially when reinforcing particles, other alloy powders or elements are added to the pre-alloyed powder to prepare mixed powder, the difference in fluidity of different components in the mixed powder will further cause the mixed powder to be unable to be fed into the metal belt according to the preset composition and content, so that the actual composition of the welding wire cannot be guaranteed to be consistent with the preset composition, and the uniformity of its composition cannot be guaranteed. Therefore, it is urgent to develop a new method for preparing powder core wire to adapt to the preparation of more materials and reduce costs. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a method for preparing a low-cost, high-performance metal powder core wire in view of the deficiencies of the above-mentioned prior art. The method ensures the uniformity of metal powder mixing and the fluidity of the filler by adding a binder to the filler, improves the filling effect of the filler, and thus ensures the performance of the metal powder core wire, reduces the requirements for the morphology, particle size and material of the metal powder, thereby greatly reducing the powder cost, and solves the problem that the non-spherical powder mixture cannot be fed into the metal strip according to the preset composition and content due to the difference in fluidity, resulting in uncontrollable and non-uniform composition of the welding wire, and breaks through the limitations of the existing powder core wire forming technology in terms of powder morphology, particle size and material.

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a low-cost and high-performance metal powder core wire, characterized in that the method comprises the following steps: Step 1: Material selection: The outer skin of the metal powder core wire is made of metal strip, and the filler includes metal powder and binder; Step 2: Preparation of filler: placing the metal powder and binder selected in step 1 in an internal mixer for internal mixing to obtain a semi-solid mixture; Step 3, forming thick wire: annealing, cleaning and drying the metal strip selected in step 1, rolling it into a U-shaped groove by rollers, and then feeding the semi-solid mixture prepared in step 2 into the U-shaped groove through a conveying pipeline, and then rolling the U-shaped groove by rollers to obtain thick wire; Step 4: reducing the diameter: the thick wire obtained in step 3 is subjected to multiple isothermal rolling to reduce the diameter gradually to obtain a metal powder core wire.

[0006] The metal powder core wire of the present invention is composed of an outer metal strip and an inner filler, and the filler has a binder added thereto in addition to the metal powder. First, the metal powder and the binder are mixed by internal kneading to obtain a semi-solid mixture as the filler. By adding the binder to the filler, the fluidity and uniformity of the metal powder during internal kneading are ensured, and the fluidity of the semi-solid mixture is also ensured, thereby having a better filling effect, which not only solves the high cost and material type limitations of using spherical powder to prepare powder core wires, but also solves the problem that the mixed powder of non-spherical powder cannot be fed into the metal strip according to the preset composition and content due to the difference in fluidity; then, the metal strip with a certain width and thickness is annealed. After being processed, cleaned and dried, the wire is rolled into a U-shaped groove, a semi-solid mixture is fed in and the U-shaped groove is closed by rolling to obtain a thick wire. The stress of the metal strip is eliminated and softened by annealing, which promotes its deformation during rolling, reduces the wear layer of the rolling die, and improves the service life of the rolling die. Finally, the thick wire is subjected to multiple isothermal rolling to reduce the diameter gradually. The isothermal rolling not only ensures that the semi-solid mixture of the filler has a certain fluidity, but also softens the metal strip, thereby promoting the deformation of the filler and the metal strip at the same time, improving the formability of the wire, and avoiding the cracking of the metal strip during rolling.

[0007] The above-mentioned method for preparing a low-cost, high-performance metal powder core wire is characterized in that the particle size of the metal powder in step 1 is less than 0.5 mm, and the binder in step 1 is derived from a wax-based, polymer-based thermoplastic, water-soluble binder. By limiting the particle size of the metal powder and the type of the binder, it is ensured that during the later processing, the semi-solid mixture formed by the metal powder and the binder has suitable fluidity, which facilitates the smooth progress of the processing technology.

[0008] The above-mentioned method for preparing a low-cost, high-performance metal powder core wire is characterized in that the volume proportion of the binder in the metal powder and the binder in step 2 is 30% to 40%, the banburying chamber is a vacuum environment during banburying and mixing, the banburying temperature is 120°C to 180°C, and the mixture is first mixed at a low speed of 4rpm to 8rpm for 7min to 15min, and then mixed at a high speed of 38rpm to 43rpm for 50min to 80min. By adopting a vacuum environment during banburying and mixing, oxidation of the metal powder is prevented, and the banburying temperature is controlled to avoid decomposition of the binder, and the uniformity of banburying and mixing is improved by first mixing at a low speed and then mixing at a high speed.

[0009] The above-mentioned method for preparing a low-cost, high-performance metal powder core wire is characterized in that the filling rate of the semi-solid mixture fed into the U-shaped groove in step 3 is 14% to 35% by mass. By controlling the filling rate of the semi-solid mixture, it is ensured that during subsequent processing, the semi-solid mixture is filled as densely as possible inside the wire without forming internal gaps or flowing out from the joints.

[0010] The above-mentioned method for preparing a low-cost, high-performance metal powder core wire is characterized in that the temperature of the multiple isothermal rolling in step 4 is 120° C. to 200° C. By controlling the temperature of the multiple isothermal rolling, the decomposition of the binder is avoided while ensuring that the semi-solid mixture inside the thick wire has fluidity during the rolling process.

[0011] At the same time, the present invention also discloses an application of the metal powder core wire prepared by the above method, characterized in that it is used in welding, high-energy beam cladding or additive manufacturing.

[0012] Compared with the prior art, the present invention has the following advantages: 1. The present invention adds a binder to the filler of the metal powder core wire, thereby ensuring the mixing uniformity of the metal powder and avoiding the oxidation of the metal powder during conventional ball milling and mixing, and also ensuring the fluidity of the filler, so that it has an excellent filling effect, thereby ensuring the performance of the metal powder core wire, solving the problem that the mixed powder of non-spherical powder cannot be fed into the metal belt according to the preset composition and content due to the difference in fluidity, and reducing the preparation cost.

[0013] 2. The preparation method of the present invention has no requirements on the type and shape of metal powder, and the particle size selection range is relatively large (<0.5mm). The metal powder can be hydrogenated dehydrogenated powder, one-time or even multiple-time recycled powder. The powder selection has a large degree of freedom, a wide source, and low cost. This not only greatly reduces the cost of the powder, but also solves the limitations of the existing powder core wire forming technology in terms of powder morphology (spherical), particle size (120μm~250μm) and material (high hardness, brittleness) and so on.

[0014] 3. The present invention performs vacuum kneading on the metal powder and the binder, and prepares a semi-solid mixture by first mixing them into agglomerates at a low speed and then stirring and mixing them at a high speed, which not only avoids oxidation of the powder during mixing, but also promotes the uniformity of the semi-solid mixture.

[0015] 4. The present invention performs annealing treatment before rolling the outer metal strip into a U-shaped groove, so that the metal strip is softened, which promotes the deformation of the metal strip during rolling, reduces the number of rolling deformation passes, reduces the degree of wear on the rolling mold, and increases the service life of the rolling mold, thereby reducing the cost of using the mold.

[0016] 5. The present invention performs multiple isothermal rolling on the thick wire and controls the temperature to ensure the fluidity of the semi-solid mixture of the filler and further soften the metal strip, thereby promoting the simultaneous deformation of the two, avoiding cracking of the metal strip and improving the formability of the wire.

[0017] 6. The present invention improves the filling effect of the filler by adding a binder to the filler, reduces the requirements for the morphology, particle size and material of the metal powder, combines annealing and softening of the metal strip to reduce its rolling passes, and isothermal rolling of the coarse wire to improve the wire formability and reduce the isothermal rolling passes, thereby shortening the process flow, effectively reducing the raw material cost and preparation cost, and improving the yield rate.

[0018] 7. The metal powder core wire preparation method of the present invention is applicable to all kinds of metals and powders, and has low production cost and high efficiency, and is suitable for industrial mass production; at the same time, the prepared metal powder core wire is suitable for welding, high-energy beam cladding or additive manufacturing, with a wide range of applications and high practical value.

[0019] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a SEM image of the hydrogenated and dehydrogenated non-spherical Ti6Al4V powder used in Example 1 of the present invention.

[0021] Figure 2 This is a diagram of the internal kneading and mixing of the hydrogenated and dehydrogenated non-spherical Ti6Al4V powder and the binder in Example 1 of the present invention.

[0022] Figure 3 This is a physical picture of the metal powder core wire prepared in Example 1 of the present invention.

[0023] Figure 4 This is a physical picture of a titanium alloy block obtained by electron beam additive manufacturing of the metal powder core wire prepared in Example 1 of the present invention.

[0024] Figure 5 This is a microstructure diagram of a titanium alloy block obtained by electron beam additive manufacturing of the metal powder core wire prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0025] Example 1 The preparation method of the metal powder core wire of this embodiment comprises the following steps: Step 1: Material selection: The outer skin of the metal powder core wire is made of CP-Ti tape with a thickness and width of 0.4mm×10mm. The fillers include Figure 1 The hydrogenated dehydrogenated non-spherical Ti6Al4V powder with a particle size not exceeding 30 μm and a binder, and the binder is a thermoplastic, water-soluble polymer-based binder made of the following components by mass: polyethylene glycol PEG 72%, polyoxymethylene POM 23%, polymethyl methacrylate PMMA 2%, stearic acid SA 2%, dioctyl phthalate DOP 1%; Step 2: Preparation of filler: Place the hydrogenated dehydrogenated non-spherical Ti6Al4V powder and water-soluble binder selected in step 1 in an internal mixer for mixing. Figure 2 As shown, the volume proportion of the water-soluble binder in the Ti6Al4V hydrogenated dehydrogenated non-spherical powder and the water-soluble binder is 35%, the mixing chamber is a vacuum environment during the mixing, the mixing temperature is 180°C, and the mixing is first performed at a low speed of 5 rpm for 8 minutes, and then at a high speed of 40 rpm for 50 minutes to obtain a semi-solid mixture; Step 3, thick wire forming: the CP-Ti strip selected in step 1 is subjected to annealing treatment at 600°C / 4h and cleaned and dried, and then rolled into a U-shaped groove by a roller, and then the semi-solid mixture prepared in step 2 is fed into the U-shaped groove through a conveying pipeline with a filling rate of 30% by mass, and then the U-shaped groove is closed by rolling with a roller to obtain a thick wire with a diameter of φ3mm; Step 4: Reducing the diameter: The thick wire obtained in step 3 is subjected to 9 passes of isothermal rolling at 200°C to reduce the diameter gradually, and a metal powder core wire with a diameter of φ2 mm is obtained, such as Figure 3 shown.

[0026] After testing, it was found that the metal powder core wire prepared in this embodiment had a smooth surface and was free of oxidation, and the wire was continuous and uniform in size.

[0027] The application process of the metal powder core wire in this embodiment is: the metal powder core wire is subjected to electron beam additive manufacturing, and the process parameters are: power 5kW, wire feeding speed 2400mm / min, deposition speed 800mm / min, overlap rate 50%, to obtain titanium alloy blocks (sample 1 and sample 2).

[0028] After testing, the metal powder core wire of this embodiment is used in the electron beam additive manufacturing process to feed the wire continuously and stably, and the interlayer bonding is good. Figure 4 As shown, the yield strength of the printed titanium alloy block obtained is 498.7 MPa, the tensile strength is 649.6 MPa, and the elongation is 15.2%.

[0029] Figure 5 The microstructure of the titanium alloy block obtained by electron beam additive manufacturing of the metal powder core wire prepared in Example 1 of the present invention is shown in FIG. Figure 5 It can be seen that there are no obvious defects such as pores and cracks in the microstructure of the titanium alloy block.

[0030] The metal powder core wire of this embodiment is further applied to electron beam welding of sample 1 and sample 2, and the welding parameters are: voltage 150 kV, welding current 354 mA, base current 39 mA, welding speed 800 mm / min, to obtain welded parts.

[0031] After testing, it was found that the weld in the welded part of this embodiment was well bonded to the base material, the yield strength of the welded joint was 522.3 MPa, the tensile strength was 682.5 MPa, and the elongation was 14.4%.

[0032] Comparative Example 1 The preparation method of the metal powder core wire of this comparative example comprises the following steps: Step 1: Material selection: The outer skin of the metal powder core wire is made of CP-Ti tape with a thickness and width of 0.4mm×10mm, and the filler is Ti6Al4V spherical powder with a particle size of 120μm~250μm; Step 2, thick wire forming: the CP-Ti belt selected in step 1 is cleaned and dried, and rolled into a U-shaped groove by a roller, and then the Ti6Al4V spherical powder selected in step 1 is fed into the U-shaped groove through a conveying pipeline with a filling rate of 25.3% by mass, and then the U-shaped groove is closed by rolling with a roller to obtain a thick wire with a diameter of φ3mm; Step 3: Reducing the diameter: The thick wire obtained in step 2 is rolled 15 times to reduce the diameter gradually, and a metal powder core wire with a diameter of φ2 mm is obtained.

[0033] After testing, it was found that the metal powder core wire prepared in this comparative example had microcracks and oxidation on the surface, and the wire size was uneven and the length was limited.

[0034] The application process of the metal powder core wire in this comparative example is: the metal powder core wire is subjected to electron beam additive manufacturing, and the process parameters are: power 5kW, wire feeding speed 2400mm / min, deposition speed 800mm / min, overlap rate 50%, to obtain titanium alloy blocks (sample 1 and sample 2).

[0035] After testing, it was found that the metal powder core wire of this comparative example had fluctuations in wire feeding during electron beam additive manufacturing, good interlayer bonding, and the yield strength of the obtained printed titanium alloy block was 472.3 MPa, the tensile strength was 617.6 MPa, and the elongation was 13.6%.

[0036] The metal powder core wire of this comparative example was further applied to electron beam welding of sample 1 and sample 2, and the welding parameters were: voltage 150 kV, welding current 354 mA, base current 39 mA, welding speed 800 mm / min, to obtain welded parts.

[0037] According to the test, the yield strength of the welded joint in the welded part of this comparative example is 501.7 MPa, the tensile strength is 638.4 MPa, and the elongation is 11.6%.

[0038] By comparing Example 1 of the present invention with Comparative Example 1, it can be seen that the cost of Example 1 is reduced to about 45% of that of Comparative Example 1, and it is a low-cost metal powder core wire. At the same time, whether the metal powder core wire prepared in Example 1 is used for electron beam additive manufacturing or electron beam welding, the mechanical properties of the obtained product are better than those of Comparative Example 1, and it is a high-performance metal powder core wire.

[0039] Example 2 The preparation method of the metal powder core wire of this embodiment comprises the following steps: Step 1, material selection: The outer skin of the metal powder core wire is made of low-carbon steel strip with a thickness and width of 0.5mm×12mm. The filler includes metal powder and a binder. The metal powder includes irregular Cr powder with a particle size of 0.25mm~0.5mm, hydrogenated dehydrogenated non-spherical Ni powder, Mo powder, Mn powder and Cu powder with a particle size of 53μm~104μm, and irregular Si powder with a particle size of 200nm. The mass ratio of Ni:Cr:Mo:Mn:Cu:Si is 37:59:8:6:0.15:1.9. The binder is a thermoplastic, water-soluble polyoxymethylene-based binder made of the following mass contents: polyoxymethylene POM 35%, low-density polyethylene LDPE 18.6%, ethylene vinyl acetate copolymer EVA 1.4%, polyethylene wax PW 42%, stearic acid SA 3%; Step 2, preparation of filler: placing the metal powder and polyoxymethylene-based binder selected in step 1 in an internal mixer for internal mixing, wherein the volume proportion of the polyoxymethylene-based binder in the metal powder and the polyoxymethylene-based binder is 30%, the internal mixing chamber is a vacuum environment during the internal mixing, the internal mixing temperature is 150°C, and the mixture is first mixed at a low speed of 4rpm for 15min, and then mixed at a high speed of 43rpm for 60min to obtain a semi-solid mixture; Step 3, forming thick wire: the low carbon steel strip selected in step 1 is subjected to annealing treatment at 550°C / 6h and cleaned and dried, and then rolled into a U-shaped groove by a roller, and then the semi-solid mixture prepared in step 2 is fed into the U-shaped groove via a conveying pipeline with a filling rate of 35% by mass, and then the U-shaped groove is closed by rolling with a roller to obtain a thick wire with a diameter of φ3.5mm; Step 4: Reducing the diameter: The thick wire obtained in step 3 is subjected to 8 passes of isothermal rolling at 160° C. to reduce the diameter gradually, and a metal powder core wire with a diameter of φ1.6 mm is obtained.

[0040] After testing, it was found that the metal powder core wire prepared in this embodiment had a smooth surface and was free of oxidation, and the wire was continuous and uniform in size.

[0041] The application process of the metal powder core wire in this embodiment is: the metal powder core wire is subjected to laser additive manufacturing, and the process parameters are: power 3.5kW, wire feeding speed 2400mm / min, scanning speed 720mm / min, overlap rate 50%, and stainless steel blocks (sample 1 and sample 2) are obtained.

[0042] After testing, the metal powder core wire of this embodiment is used in the electron beam additive manufacturing process, the wire feeding is continuous and stable, the interlayer bonding is good, and the yield strength of the printed stainless steel block obtained is 441.6 MPa, the tensile strength is 635.4 MPa, and the elongation is 51.3%.

[0043] The metal powder core wire of this embodiment is further applied to the laser welding of Sample 1 and Sample 2, and the welding parameters are: laser power 1.35 kW, welding speed 0.8 m / min, defocus amount 0 mm, to obtain a welded part.

[0044] After testing, it was found that the weld in the welded part of this embodiment was well bonded to the base material, the yield strength of the welded joint was 453.1 MPa, the tensile strength was 655.9 MPa, and the elongation was 42.7%.

[0045] Comparative Example 2 The preparation method of the metal powder core wire of this comparative example comprises the following steps: Step 1, material selection: The outer skin of the metal powder core wire is made of low-carbon steel strip with a thickness and width of 0.5mm×12mm. The filler includes metal powder, and the metal powder includes spherical Ni powder, Cr powder, Mo powder, Mn powder and Cu powder with a particle size of 120μm~250μm, and irregular Si powder with a particle size of 200nm. The mass ratio is Ni:Cr:Mo:Mn:Cu:Si=37:59:8:6:0.15:1.9; Step 2, forming thick wire: the low carbon steel strip selected in step 1 is cleaned and dried, and rolled into a U-shaped groove by a roller, and then the metal powder selected in step 1 is fed into the U-shaped groove through a conveying pipeline with a filling rate of 32.2% by mass, and then the U-shaped groove is closed by rolling with a roller to obtain a thick wire with a diameter of φ3.5 mm; Step 3: Reducing the diameter: The thick wire obtained in step 3 is rolled 13 times to reduce the diameter gradually, and a metal powder core wire with a diameter of φ1.6 mm is obtained.

[0046] After testing, it was found that the metal powder core wire prepared in this embodiment had a smooth surface and was free of oxidation, and the wire was continuous and uniform in size.

[0047] The application process of the metal powder core wire in this comparative example is: the metal powder core wire is subjected to laser additive manufacturing, and the process parameters are: laser power 3.5kW, wire feeding speed 2400mm / min, scanning speed 720mm / min, overlap rate 50%, and stainless steel blocks (sample 1 and sample 2) are obtained.

[0048] After testing, the yield strength of the stainless steel block obtained by applying the metal powder core wire of this comparative example to laser beam additive manufacturing is 438.5 MPa, the tensile strength is 647.2 MPa, and the elongation is 47.1%.

[0049] The metal powder core wire of this comparative example was further applied to the laser welding of sample 1 and sample 2, and the welding parameters were: laser power 1.35 kW, welding speed 0.8 m / min, defocus amount 0 mm, to obtain a welded part.

[0050] According to the test, the yield strength of the welded joint in the welded part of this comparative example is 446.3 MPa, the tensile strength is 659.1 MPa, and the elongation is 39.8%.

[0051] By comparing Example 2 of the present invention with Comparative Example 2, it can be seen that the cost of Example 2 is reduced to about 41% of that of Comparative Example 2, and it is a low-cost metal powder core wire. At the same time, whether the metal powder core wire prepared in Example 2 is used for laser additive manufacturing or laser welding, the mechanical properties of the obtained product are equivalent to those of Comparative Example 2, but the plasticity is better, and it is a high-performance metal powder core wire.

[0052] Example 3 The preparation method of the metal powder core wire of this embodiment comprises the following steps: Step 1, material selection: The outer skin of the metal powder core wire is made of aluminum strip with a thickness and width of 0.8mm×16mm. The filler includes metal powder and a binder. The metal powder includes hydrogenated dehydrogenated non-spherical Cu powder, Mn powder, Fe powder, Zr powder with a particle size of 15μm~53μm and irregular Si powder with a particle size of 200nm. The mass ratio is Cu:Mn:Si:Fe:Zr=68:3.2:2.1:3.2:2.1. The binder is a thermoplastic, water-soluble wax-based binder made of the following mass contents: palm purlin wax CW 62%, high-density polyethylene HDPE 35%, stearic acid SA 3%; Step 2, preparation of filler: placing the metal powder and binder selected in step 1 in an internal mixer for internal mixing, wherein the volume proportion of the binder in the metal powder and the binder is 40%, the internal mixing chamber is a vacuum environment during internal mixing, the internal mixing temperature is 120°C, and the mixture is first mixed at a low speed of 8 rpm for 7 minutes, and then at a high speed of 38 rpm for 80 minutes to obtain a semi-solid mixture; Step 3, forming thick wire: the aluminum strip selected in step 1 is subjected to annealing treatment at 300°C / 4h and cleaned and dried, and then rolled into a U-shaped groove by a roller, and then the semi-solid mixture prepared in step 2 is fed into the U-shaped groove via a conveying pipeline with a filling rate of 14% by mass, and then the U-shaped groove is closed by rolling with a roller to obtain a thick wire with a diameter of φ5mm; Step 4: reducing the diameter: the thick wire obtained in step 3 is subjected to 6 passes of isothermal rolling at 120° C. to gradually reduce the diameter to obtain a metal powder core wire with a diameter of φ1.2 mm.

[0053] After testing, it was found that the metal powder core wire prepared in this embodiment had a smooth surface and was free of oxidation, and the wire was continuous and uniform in size.

[0054] The application process of the metal powder core wire in this embodiment is: the metal powder core wire is subjected to arc additive manufacturing, and the process parameters are: AC power supply frequency 50 Hz, wire feeding speed 2000 mm / min, scanning speed 300 mm / min, peak current 150 A, base current 100 A, to obtain aluminum alloy blocks (sample 1 and sample 2).

[0055] After testing, the metal powder core wire of this embodiment is used in the arc additive manufacturing process, the wire feeding is continuous and stable, the interlayer bonding is good, and the obtained printed aluminum alloy block has a yield strength of 128.3 MPa, a tensile strength of 262.6 MPa, and an elongation of 16.3%.

[0056] The metal powder core wire of this embodiment is further applied to arc welding of Sample 1 and Sample 2, and the welding parameters are: wire feeding speed 1800 mm / min, scanning speed 280 mm / min, peak current 200 A, base current 100 A, to obtain welded parts.

[0057] After testing, it was found that the weld in the welded part of this embodiment was well bonded to the base material, the yield strength of the welded joint was 137.8 MPa, the tensile strength was 274.6 MPa, and the elongation was 13.5%.

[0058] Comparative Example 3 The preparation method of the metal powder core wire of this comparative example comprises the following steps: Step 1, material selection: The outer skin of the metal powder core wire is made of aluminum strip with a thickness and width of 0.8mm×16mm. The filler includes metal powder, and the metal powder includes spherical Cu powder, Mn powder, Fe powder, Zr powder with a particle size of 120μm~150μm and irregular Si powder with a particle size of 200nm. The mass ratio is Cu:Mn:Si:Fe:Zr=68:3.2:2.1:3.2:2.1; Step 2, forming thick wire: the aluminum strip selected in step 1 is cleaned and dried, and rolled into a U-shaped groove by a roller, and then the metal powder selected in step 1 is fed into the U-shaped groove through a conveying pipeline with a filling rate of 9.5% by mass, and then the U-shaped groove is closed by rolling with a roller to obtain a thick wire with a diameter of φ3.5 mm; Step 4: Reducing the diameter: The thick wire obtained in step 3 is rolled 10 times to reduce the diameter gradually, and a metal powder core wire with a diameter of φ1.6 mm is obtained.

[0059] The application process of the metal powder core wire in this comparative example is: the metal powder core wire is subjected to arc additive manufacturing, and the process parameters are: AC power supply frequency 50 Hz, wire feeding speed 2000 mm / min, scanning speed 300 mm / min, peak current 150 A, base current 100 A, to obtain aluminum alloy blocks (sample 1 and sample 2).

[0060] After testing, it was found that the metal powder core wire of this embodiment had fluctuations in wire feeding during arc additive manufacturing, good interlayer bonding, and the obtained printed aluminum alloy block had a yield strength of 109.4 MPa, a tensile strength of 242.5 MPa, and an elongation of 14.7%.

[0061] The metal powder core wire of this embodiment is further applied to arc welding of Sample 1 and Sample 2, and the welding parameters are: wire feeding speed 1800 mm / min, scanning speed 280 mm / min, peak current 200 A, base current 100 A, to obtain welded parts.

[0062] According to the test, the yield strength of the welded joint in the welded part of this comparative example is 117.3 MPa, the tensile strength is 251.3 MPa, and the elongation is 12.3%.

[0063] By comparing Example 3 of the present invention with Comparative Example 3, it can be seen that the cost of Example 3 is reduced to about 38% of that of Comparative Example 3, and it is a low-cost metal powder core wire. At the same time, whether the metal powder core wire prepared by Example 3 is used for arc additive manufacturing or arc welding, the mechanical properties of the obtained product are better than those of Comparative Example 3, and it is a high-performance metal powder core wire.

[0064] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing low-cost high-performance metal powder core wire, characterized in that: The method comprises the following steps: Step 1: Material selection: The outer skin of the metal powder core wire is made of metal strip, and the filler includes metal powder and binder; Step 2: Preparation of filler: placing the metal powder and binder selected in step 1 in an internal mixer for internal mixing to obtain a semi-solid mixture; Step 3, forming thick wire: annealing, cleaning and drying the metal strip selected in step 1, rolling it into a U-shaped groove by rollers, and then feeding the semi-solid mixture prepared in step 2 into the U-shaped groove through a conveying pipeline, and then rolling the U-shaped groove by rollers to obtain thick wire; Step 4: reducing the diameter: the thick wire obtained in step 3 is subjected to multiple isothermal rolling to reduce the diameter gradually to obtain a metal powder core wire.

2. The method for preparing a low-cost, high-performance metal powder core wire according to claim 1, characterized in that: The particle size of the metal powder in step one is less than 0.5 mm, and the binder in step one is derived from a wax-based or polymer-based thermoplastic, water-soluble binder.

3. The method for preparing a low-cost, high-performance metal powder core wire according to claim 1, characterized in that: The volume proportion of the binder in the metal powder and the binder in step 2 is 30% to 40%. The mixing chamber is in a vacuum environment during the mixing, the mixing temperature is 120°C to 180°C, and the mixture is first mixed at a low speed of 4rpm to 8rpm for 7min to 15min, and then mixed at a high speed of 38rpm to 43rpm for 50min to 80min.

4. The method for preparing a low-cost, high-performance metal powder core wire according to claim 1, characterized in that: The filling rate of the semi-solid mixture fed into the U-shaped groove in step 3 is 14% to 35% by mass.

5. The method for preparing a low-cost, high-performance metal powder core wire according to claim 1, characterized in that: The temperature of the multiple isothermal rolling in step 4 is 120°C to 200°C.

6. An application of a metal powder core wire prepared by the method according to any one of claims 1 to 5, characterized in that: Applications in welding, high energy beam cladding or additive manufacturing.

Citation Information

Patent Citations

  • High-performance arc spraying Zn-Al powder core wire and preparation method thereof

    CN102839344A

  • Composite aluminum-base brazing wire for continuously brazing aluminum alloy and method for manufacturing composite aluminum-base brazing wire

    CN103203560A

  • Groove type aluminum alloy combined welding wire for arc welding and brazing and manufacturing method thereof

    CN103831545A

  • Titanium carbide type self-protective wear-resistant bead weld flux-cored wire and preparation method thereof

    CN104708226A

  • Continuous brazing composite aluminum-based brazing wire applying nanometer aluminum trioxide and preparation method of continuous brazing composite aluminum-based brazing wire applying nanometer aluminum trioxide

    CN105834609A

Cited By

  • High-strength titanium alloy flux-cored wire for additive manufacturing and preparation method and application of high-strength titanium alloy flux-cored wire

    CN121468012A

  • High-strength titanium alloy flux-cored wire for additive manufacturing and preparation method and application thereof

    CN121468012B

  • High-strength titanium alloy powder core wire material special for additive manufacturing and preparation method of component of high-strength titanium alloy powder core wire material

    CN121669957A