Welding method for seal welding of magnesium alloy
By brazing aluminum alloy on magnesium alloy and using laser sealing technology, the oxidation, reflection and thermal stress problems during laser sealing and welding of magnesium alloy are solved, and high-quality magnesium alloy and aluminum alloy are achieved, improving welding quality and sealing.
Patent Information
- Application Number
- CN202411151627.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-19
AI Technical Summary
During the laser sealing and welding process, magnesium alloys have oxidation reactions, high reflectivity, thermal stress problems and grain formation, resulting in poor welding quality and the inability to directly carry out laser sealing and welding.
Brazing a layer of aluminum alloy on the magnesium alloy, and welding the cover plate to the cavity through laser sealing welding, including surface treatment, preheating, brazing and laser sealing steps, controlling the welding temperature and speed, using appropriate brazing materials and laser parameters to ensure welding quality.
It improves the welding quality of magnesium alloy and aluminum alloy connectors, reduces deformation and residual stress, enhances sealing and service life, and meets the product's appearance and dimensional accuracy requirements.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum alloy sealing and welding, and in particular to a welding method for magnesium alloy sealing and welding. Background Art
[0002] As the lightest metal structural material, magnesium alloy has the characteristics of low density, high strength, good heat dissipation and strong impact resistance, and is widely used in aerospace, automobile manufacturing and other fields. Aluminum alloy, with its good corrosion resistance, machinability and conductivity, occupies an important position in electronic equipment, construction, transportation and other fields. The combination of the two materials can give full play to their respective advantages and achieve lighter and higher performance product design.
[0003] However, there are indeed some difficulties and challenges in the laser welding process, which makes it impossible to directly perform laser welding in some cases.
[0004] There are several main reasons why magnesium alloys cannot be laser sealed: Active chemical properties of magnesium alloys: The chemical properties of magnesium, the main element in magnesium alloys, are relatively active. Under high temperature conditions, magnesium alloys are prone to oxidation reactions, and the resulting magnesium oxide (MgO) is not easy to melt, forming granular slag inclusions, which directly affects the welding quality. At the same time, this oxidation process will also consume a lot of laser energy and reduce welding efficiency.
[0005] High reflectivity: Magnesium alloy has a relatively high reflectivity, which makes the laser beam easily reflected and scattered on the surface of magnesium alloy during welding, resulting in the inability to effectively concentrate the laser energy and act on the welding area, thus affecting the welding effect.
[0006] Thermal stress problem: Magnesium alloy has a high thermal expansion coefficient, about twice that of steel. During the welding process, magnesium alloy is prone to thermal stress due to uneven temperature distribution. This thermal stress may cause defects such as deformation and cracking of the workpiece, seriously affecting the quality of the welded joint.
[0007] Grain problem: Magnesium alloy has a relatively low melting point and strong thermal conductivity. During laser welding, due to the high power of the welding heat source, larger grains are easily formed at the weld. These grains will affect the mechanical properties of magnesium alloy and reduce its use value.
[0008] Poor welding stability: The ionization energy of magnesium alloy is low, and liquid magnesium has good fluidity and low surface tension, which leads to defects such as undercut and discontinuous welds during laser welding, reducing the quality of the welded joint. Summary of the invention
[0009] The purpose of the present invention is to provide a welding method for sealing magnesium alloys to solve the problem that magnesium alloys cannot be laser sealed in the prior art. At the same time, the sealing of the cavity is improved. By brazing a layer of aluminum alloy on the magnesium alloy, and then using laser sealing to weld the cover plate to the cavity, efficient and high-quality welding of the magnesium alloy is achieved.
[0010] To achieve the above object, the present invention provides the following technical solutions: The present invention provides a magnesium alloy sealing welding method, comprising the following steps: (1) Surface treatment: Clean and polish the welding areas of magnesium alloy and aluminum alloy to remove oil stains and oxide film impurities; (2) Preheating treatment: preheat the brazing material and alloy at 150-250℃ for 5-15min; (3) Brazing: Place the brazing material at the joint of the magnesium alloy and the aluminum alloy, and control the temperature at 550°C to 620°C for brazing; (4) Post-processing: After welding, let the welding area cool down naturally to room temperature, clean and polish the weld, and perform surface treatment on the aluminum alloy; (5) Laser sealing welding: Place the processed aluminum alloy material on the welding platform, ensure that the weld position is accurate and tight, start the laser welding equipment, and perform welding according to the preset parameters.
[0011] Furthermore, in the surface treatment in (1) and (4), acetone or a special cleaning agent is used to thoroughly clean the surface of the aluminum alloy to remove oil stains and oxide impurities, and a wire brush or sandpaper tool is used to polish the welding area until the metallic luster is exposed.
[0012] Furthermore, the brazing filler metal is Al-Si, Al-Si-Mg alloy, or zinc-based alloy. Al-Si, Al-Si-Mg and other alloy brazing fillers are selected to ensure good chemical compatibility with magnesium alloy and 6061 aluminum alloy, and to avoid the generation of a large amount of MgAl intermetallic compounds during the welding process.
[0013] Furthermore, the Al-Si composition is: Si: 9.3%~11.7%, Cu: 3.3%~4.7%, Zn: ≤0.2%, Al: balance; melting point: 585°C; the zinc-based alloy is ZnAl 10-5 Its composition is: Zn: 85%, Al: 10%, Cu: 5%; melting point: 385℃~460℃.
[0014] Furthermore, the preheating temperature is 150-250°C to reduce the temperature gradient during welding, reduce welding deformation and residual stress; the preheating time is 5-15 minutes to ensure that the material is fully preheated and the temperature distribution is uniform.
[0015] The welding speed directly affects the quality and performance of the welded joint. Under the premise of ensuring that the solder fully wets the base material, the welding speed should be increased as much as possible to reduce welding deformation and residual stress. Too fast a welding speed may result in incomplete penetration of the weld, while too slow a welding speed may result in overheating and deformation.
[0016] Furthermore, the alloy is a 6061 aluminum alloy plate with a thickness of 1.0 to 3.0 mm, the laser power during laser welding is 1500 W, the welding speed during laser welding is 50 mm / min, and the focusing diameter during laser welding is 0.2 to 0.4 mm. The focusing diameter determines the energy density of the laser beam on the surface of the workpiece. A focusing diameter that is too small may cause excessive concentration of energy, resulting in burn-through of the workpiece; a focusing diameter that is too large may reduce welding efficiency.
[0017] Furthermore, after the laser welding process (5) is completed, it is ensured that there are no cracks or pores, and heat treatment or mechanical correction is also performed to eliminate residual stress and deformation.
[0018] Based on the above technical solution, the embodiments of the present invention can at least produce the following technical effects: (1) Improving product appearance quality: The magnesium alloy and aluminum alloy connectors welded by the method of the present invention have flat and smooth welds without obvious welding defects. This helps to improve the product appearance quality and meet the user's requirements for product aesthetics.
[0019] (2) Reduce the degree of deformation. By optimizing the brazing and laser sealing process parameters, the present invention can reduce welding deformation and residual stress. This is of great significance for improving the dimensional accuracy and stability of the product.
[0020] (3) Increase product life: The solder material and laser sealing technology used in the present invention can ensure the sealing inside the product. This helps to improve the reliability and durability of the product and increase the product life. DETAILED DESCRIPTION
[0021] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0022] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0023] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0024] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0025] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0026] Example 1 The main components of magnesium alloy metal ZK61M-T5 are: Cu: 0.15%~0.4%, Si: 0.4%~08%, Fe: ≤0.7%, Mn: 0.15%~0.50%, Mg: balance, Zn: 0.25%~0.50%, Mn: 0.15%~0.50%, Cr: 0.04%~0.35%, Ti0.15%; The aluminum alloy is 1.0-3.0 mm 6061 aluminum alloy plate; Brazing material: Al-Si composition: Si: 9.3%~11.7%, Cu: 3.3%~4.7%, Zn: ≤0.2%, Al: balance; Melting point: 585℃; (1) Surface treatment: Use acetone to clean and polish the welding area of magnesium alloy and aluminum alloy to remove oil stains and oxide film impurities. Use wire brushes, sandpaper and other tools to polish the welding area until the metallic luster is exposed. (2) Preheating treatment: preheat the brazing material and alloy at 150-250℃ for 5-15min; (3) Brazing: Place the brazing material at the joint of the magnesium alloy and the aluminum alloy, and control the temperature at 550°C to 620°C for brazing; (4) Post-processing: After welding, let the welding area cool down naturally to room temperature, clean and polish the weld, and perform surface treatment on the aluminum alloy; (5) Laser welding: Place the processed aluminum alloy material on the welding platform to ensure that the weld position is accurate and tight, start the laser welding equipment, and perform welding in a helium atmosphere at a temperature controlled between 550°C and 620°C; the laser power is 1500W, the welding speed is 50mm / min, and the focus diameter is selected to be 0.2~0.4mm for welding.
[0027] After welding, the weld is visually inspected to ensure that there are no defects such as cracks and pores. If necessary, heat treatment or mechanical correction is performed to eliminate residual stress and deformation.
[0028] Example 2 The aluminum alloy is 1.0-3.0 mm 6061 aluminum alloy plate; Brazing material: zinc-based alloy is ZnAl 10-5 Its composition is: Zn: 85%, Al: 10%, Cu: 5%; melting point: 385℃~460℃; (1) Surface treatment: Use acetone to clean and polish the welding area of magnesium alloy and aluminum alloy to remove oil stains and oxide film impurities. Use wire brushes, sandpaper and other tools to polish the welding area until the metallic luster is exposed. (2) Preheating treatment: preheat the brazing material and alloy at 150-250℃ for 5-15min; (3) Brazing: Place the brazing material at the joint of the magnesium alloy and the aluminum alloy, and control the temperature at 550°C to 620°C for brazing; (4) Post-processing: After welding, let the welding area cool down naturally to room temperature, clean and polish the weld, and perform surface treatment on the aluminum alloy; (5) Laser welding: Place the processed aluminum alloy material on the welding platform to ensure that the weld position is accurate and tight, start the laser welding equipment, and perform welding in a helium atmosphere at a temperature controlled between 550°C and 620°C; the laser power is 1500W, the welding speed is 50mm / min, and the focus diameter is selected to be 0.2~0.4mm for welding.
[0029] After welding, the weld is visually inspected to ensure that there are no defects such as cracks and pores. If necessary, heat treatment or mechanical correction is performed to eliminate residual stress and deformation.
[0030] Finally, it should be noted that: The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that the technical solutions described in the above embodiments may still be modified, or some or all of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A welding method for magnesium alloy sealing, It is characterized in that The following steps are involved: (1) Surface treatment: Clean and polish the welding areas of magnesium alloy and aluminum alloy to remove oil stains and oxide film impurities; (2) Preheating treatment: preheat the brazing material and alloy at 150-250℃ for 5-15min; (3) Brazing: Place the brazing material at the joint of the magnesium alloy and the aluminum alloy, and control the temperature at 550°C to 620°C for brazing; (4) Post-processing: After welding, let the welding area cool down naturally to room temperature, clean and polish the weld, and perform surface treatment on the aluminum alloy; (5) Laser sealing welding: Place the processed aluminum alloy material on the welding platform, ensure that the weld position is accurate and tight, start the laser welding equipment, and perform welding according to the set parameters.
2. The magnesium alloy sealing welding method according to claim 1, It is characterized in that In the surface treatment of (1) and (4), acetone or a special cleaning agent is used to thoroughly clean the surface of the aluminum alloy to remove oil stains and oxide impurities, and a wire brush or sandpaper tool is used to polish the welding area until the metallic luster is exposed.
3. The magnesium alloy sealing welding method according to claim 1, It is characterized in that The solder is Al-Si, Al-Si-Mg alloy or zinc-based alloy.
4. The magnesium alloy sealing welding method according to claim 1, It is characterized in that The alloy is a 6061 aluminum alloy plate with a thickness of 1.0 to 3.0 mm, the laser power during laser welding is 1500 W, the welding speed during laser welding is 50 mm / min, and the focusing diameter during laser welding is 0.2 to 0.4 mm.
5. The magnesium alloy sealing welding method according to claim 1, It is characterized in that After the laser welding process (5) is completed, it is ensured that there are no cracks or pores, and heat treatment or mechanical correction is also performed to eliminate residual stress and deformation.