Production method of high-heat-resistance alloyed oxygen-free copper strip

By increasing the proportion of manganese raw materials in copper tape production and adopting melting, semi-continuous casting, sawing, hot rolling, annealing, bending straightening and shearing steps, the problem of insufficient heat resistance of existing copper tapes is solved. It significantly improves the heat resistance and service life of the copper belt.

CN118977061AInactive Publication Date: 2024-11-19ANHUI CHUJIANG HIGH PRECISION COPPER STRIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411060565.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing copper tape has a low lifespan in equipment with high heat resistance and cannot meet people's work needs.

Method used

Adopt high heat resistance alloyed oxygen-free copper tape production methods, including melting, semi-continuous casting, sawing, hot rolling, annealing, bending and straightening and shearing steps, and improve heat resistance by increasing the proportion of manganese raw materials .

Benefits of technology

It effectively improves the heat resistance of alloyed oxygen-free copper tape, extends the service life, and meets the high heat resistance needs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a high-heat-resistance alloying oxygen-free copper strip production method which comprises the following steps: (1) melting: putting alloy raw materials into melting equipment for melting processing, and condensing molten steel into a blank through a crystallizer; (2) semi-continuous casting: carrying out semi-continuous casting work on the blank-formed copper material through a blank drawing machine; (3) sawing: sawing the copper material subjected to semi-continuous casting through a sawing machine; (4) hot rolling: carrying out hot rolling work on the sawed copper material through hot rolling equipment; and (5) annealing: annealing the hot-rolled copper material through annealing equipment. According to the production method of the high-heat-resistance alloyed oxygen-free copper strip, a large amount of manganese is added into the raw materials according to the proportion, so that the heat-resistant effect after alloying is effectively improved, the problem of poor heat resistance is solved, the working requirements of people are met, and the production method is worthy of popularization and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of copper strip processing, in particular to a method for producing a highly heat-resistant alloyed oxygen-free copper strip. Background Art

[0002] Copper strip is a metal component, which is mainly used to produce electrical components, lamp holders, battery caps, buttons, seals, connectors, and is mainly used as conductive, heat-conductive, and corrosion-resistant equipment, such as electrical components, switches, washers, gaskets, vacuum devices, radiators, conductive base materials, and various parts such as automobile water tanks, heat sinks, and cylinder plates.

[0003] The existing copper strips have poor heat resistance during production and processing, resulting in a low lifespan when used in equipment with high heat resistance requirements. Therefore, the existing copper strip processing technology cannot meet people's work needs and brings inconvenience to people's use. Summary of the invention

[0004] The object of the present invention is to provide a method for producing a highly heat-resistant alloyed oxygen-free copper strip, so as to solve the above-mentioned problems of the method for producing a highly heat-resistant alloyed oxygen-free copper strip on the current market.

[0005] To achieve the above object, the present invention provides the following technical solution: a method for producing a highly heat-resistant alloyed oxygen-free copper strip, comprising the following steps:

[0006] (1) Melting: The alloy raw materials are put into the melting equipment for melting processing, and the melted molten steel is condensed into embryos through the crystallizer;

[0007] (ii) Semi-continuous casting: The copper material is semi-continuously cast through a casting machine;

[0008] (3) Sawing: The copper material after semi-continuous casting is sawed by a sawing machine;

[0009] (iv) Hot rolling: The sawn copper material is hot rolled through hot rolling equipment;

[0010] (V) Annealing: The hot-rolled copper material is annealed through an annealing device;

[0011] (VI) Bending and straightening: The annealed copper material is passed through the straightening equipment for bending and straightening;

[0012] (VII) Shearing: The copper material after bending and straightening is sheared by shearing equipment to obtain a formed copper strip.

[0013] Furthermore, during the melting process of step (i), the alloy raw material ratio is 92-97% copper, 0.25-0.4% nickel, 0.01-0.1.5% iron, 0.3-1.5% tin, 0.03-0.08% beryllium, 0.1-0.15% manganese, 0.08-0.2% rare earth metal elements, and the balance is zinc and unavoidable impurities.

[0014] Furthermore, the annealing process in step (V) includes intermediate annealing and finished product annealing.

[0015] Furthermore, the intermediate annealing process in the step also includes an intermediate cleaning process.

[0016] Furthermore, the steps of intermediate cleaning and finished product annealing also include finishing rolling.

[0017] Furthermore, the finished product annealing process also includes finished product cleaning.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] (1) The method for producing highly heat-resistant alloyed oxygen-free copper strip effectively increases the heat resistance after alloying by adding a large amount of manganese to the raw material ratio, solves the problem of poor heat resistance, and thus meets people's work needs, and is worthy of promotion and use. DETAILED DESCRIPTION

[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Embodiment 1:

[0022] A method for producing a highly heat-resistant alloyed oxygen-free copper strip. The production and application thereof are described in detail below:

[0023] (1) Melting: The alloy raw materials are put into the melting equipment for melting processing, and the melted molten steel is condensed into embryos through the crystallizer;

[0024] (ii) Semi-continuous casting: The copper material is semi-continuously cast through a casting machine;

[0025] (3) Sawing: The copper material after semi-continuous casting is sawed by a sawing machine;

[0026] (iv) Hot rolling: The sawn copper material is hot rolled through hot rolling equipment;

[0027] (V) Annealing: The hot-rolled copper material is annealed through an annealing device;

[0028] (VI) Bending and straightening: The annealed copper material is passed through the straightening equipment for bending and straightening;

[0029] (VII) Shearing: The copper material after bending and straightening is sheared by shearing equipment to obtain a formed copper strip.

[0030] Furthermore, during the melting process of step (i), the alloy raw material ratio is 92% copper, 0.4% nickel, 0.1.5% iron, 1.5% tin, 0.08% beryllium, 0.15% manganese, 0.2% rare earth metal element, and the balance is zinc and unavoidable impurities.

[0031] Furthermore, the annealing process in step (V) includes intermediate annealing and finished product annealing.

[0032] Furthermore, the intermediate annealing process in the step also includes an intermediate cleaning process.

[0033] Furthermore, the steps of intermediate cleaning and finished product annealing also include finishing rolling.

[0034] Furthermore, the finished product annealing process also includes finished product cleaning.

[0035] Embodiment 2:

[0036] A method for producing a highly heat-resistant alloyed oxygen-free copper strip. The production and application thereof are described in detail below:

[0037] (1) Melting: The alloy raw materials are put into the melting equipment for melting processing, and the melted molten steel is condensed into embryos through the crystallizer;

[0038] (ii) Semi-continuous casting: The copper material is semi-continuously cast through a casting machine;

[0039] (3) Sawing: The copper material after semi-continuous casting is sawed by a sawing machine;

[0040] (iv) Hot rolling: The sawn copper material is hot rolled through hot rolling equipment;

[0041] (V) Annealing: The hot-rolled copper material is annealed through an annealing device;

[0042] (VI) Bending and straightening: The annealed copper material is passed through the straightening equipment for bending and straightening;

[0043] (VII) Shearing: The copper material after bending and straightening is sheared by shearing equipment to obtain a formed copper strip.

[0044] Furthermore, during the melting process of step (i), the alloy raw material ratio is 97% copper, 0.25% nickel, 0.01% iron, 0.3% tin, 0.03% beryllium, 0.1% manganese, 0.08% rare earth metal element, and the balance is zinc and unavoidable impurities.

[0045] Furthermore, the annealing process in step (V) includes intermediate annealing and finished product annealing.

[0046] Furthermore, the intermediate annealing process in the step also includes an intermediate cleaning process.

[0047] Furthermore, the steps of intermediate cleaning and finished product annealing also include finishing rolling.

[0048] Furthermore, the finished product annealing process also includes finished product cleaning.

[0049] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, commodity or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, commodity or device. In the absence of more restrictions, the elements defined by the sentence "comprises a ..." do not exclude the existence of other identical elements in the process, method, commodity or device including the elements.

[0050] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for producing a highly heat-resistant alloyed oxygen-free copper strip, characterized in that: The following steps are involved: (1) Melting: The alloy raw materials are put into the melting equipment for melting processing, and the melted molten steel is condensed into embryos through the crystallizer; (ii) Semi-continuous casting: The copper material is semi-continuously cast through a casting machine; (3) Sawing: The copper material after semi-continuous casting is sawed by a sawing machine; (iv) Hot rolling: The sawn copper material is hot rolled through hot rolling equipment; (V) Annealing: The hot-rolled copper material is annealed through an annealing device; (VI) Bending and straightening: The annealed copper material is passed through the straightening equipment for bending and straightening; (VII) Shearing: The copper material after bending and straightening is sheared by shearing equipment to obtain a formed copper strip.

2. The method for producing a highly heat-resistant alloyed oxygen-free copper strip according to claim 1, characterized in that: During the melting process of step (i), the alloy raw material ratio is 92-97% copper, 0.25-0.4% nickel, 0.01-0.1.5% iron, 0.3-1.5% tin, 0.03-0.08% beryllium, 0.1-0.15% manganese, 0.08-0.2% rare earth metal element, and the balance is zinc and unavoidable impurities.

3. The method for producing a highly heat-resistant alloyed oxygen-free copper strip according to claim 1, characterized in that: The annealing process of step (V) includes intermediate annealing and finished product annealing.

4. The method for producing a highly heat-resistant alloyed oxygen-free copper strip according to claim 3, characterized in that: The intermediate annealing process in the step also includes intermediate cleaning.

5. The method for producing a highly heat-resistant alloyed oxygen-free copper strip according to claim 3, characterized in that: The steps of intermediate cleaning and finished product annealing also include finishing rolling.

6. The method for producing a highly heat-resistant alloyed oxygen-free copper strip according to claim 3, characterized in that: The process of annealing the finished product in the step also includes cleaning the finished product.