Multi-layer extension film with large draw ratio, preparation method and application

By bonding and stretching the thermoplastic elastomer film after plasma treatment with the polyvinyl alcohol film, the problem of breaking the film and horizontal stripes during the stretching process of the polyvinyl alcohol film is solved, and the stretching ratio of the polyvinyl alcohol film is improved The performance of the polarizing film meets the thinner requirements of new display devices.

CN118977489APending Publication Date: 2024-11-19UNIV OF SCI & TECH OF CHINA
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411367584.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the prior art, it is difficult to improve the stretching ratio during the stretching process of polyvinyl alcohol film, and it is prone to cross-sectional stripes, which affects the thinning and performance of the polarizing film.

Method used

The thermoplastic elastomer film treated with plasma is bonded to the polyvinyl alcohol film, and a multi-layer ductile film is made by stretching to improve the stretching ratio of the polyvinyl alcohol film and avoid the appearance of horizontal and vertical stripes.

Benefits of technology

The production of polyvinyl alcohol films with high stretch ratios has been achieved, which improves the yield and performance of polarized films, reduces production costs, and meets the demand for thin display panels of new display equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118977489A_ABST
    Figure CN118977489A_ABST
Patent Text Reader

Abstract

The invention provides a multi-layer extension film with a large draw ratio, a preparation method and application, and belongs to the technical field of high-molecular compounds. According to a plasma treatment process, a thermoplastic elastomer film is subjected to plasma treatment, the thermoplastic elastomer film and a polyvinyl alcohol film are attached into multiple layers, and then stretching is conducted to prepare the multi-layer extension film; the polyvinyl alcohol film with high stretch ratio and without transverse and longitudinal stripes can be obtained, and is used for preparing a polarizing film with excellent polarizing performance. The production process is simple, the yield of the polyvinyl alcohol polarizing film is improved, efficient production of the polyvinyl alcohol polarizing film is promoted, and the production and preparation cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer compounds, and particularly relates to a multi-layer stretched film with a large stretch ratio, a preparation method and an application thereof. Background Art

[0002] In recent years, based on the diversification of application scenarios, the portability of production and life, and the intelligentization of engineering technology, new displays have gradually developed in the direction of lightness, thinness, flexibility, high contrast, and high weather resistance. In particular, the increasing popularity of mainstream information products and equipment such as smartphones and thin and light notebooks has greatly accelerated the market demand for thin display panels, which in turn has led to an urgent need for thin polarizer technology.

[0003] To meet the demand for thinner polarizers, thinning polarizing films is an effective way, and thinning the raw material polyvinyl alcohol film becomes the key. However, it is difficult to increase the stretching ratio of polyvinyl alcohol film, and problems such as horizontal and vertical stripes will appear during the stretching process.

[0004] As a technology for preparing a thin polarizing film by increasing the stretching ratio of a polyvinyl alcohol film and reducing the occurrence of horizontal and vertical stripes during stretching, patent document CN104903761B discloses a method of forming a polyvinyl alcohol film layer on a thermoplastic resin film by a coating technique and stretching the laminated film. However, the method of preparing a laminated film by forming a polyvinyl alcohol film layer on a thermoplastic resin film by a coating technique has the following problems.

[0005] 1. The coating and drying processes are complicated and arduous.

[0006] 2. In the laminated structure where the polyvinyl alcohol film layer is formed on the thermoplastic resin film by coating technology, the bonding strength between the thermoplastic resin film and the polyvinyl alcohol film layer is high. If this laminated structure with high bonding strength is stretched, the appropriate shrinkage of the polyvinyl alcohol film layer is affected, making it difficult to obtain a polarizing film with excellent performance. Summary of the invention

[0007] In order to solve the above technical problems, the purpose of the present invention is to provide a multilayer stretched film with a large stretch ratio and a preparation method thereof, so as to increase the stretch ratio of the polyvinyl alcohol film and improve the phenomenon of horizontal and vertical stripes during stretching, and produce high-quality polyvinyl alcohol film materials for high-performance polarizers to meet the needs of new display preparation.

[0008] In order to achieve the above object, the present invention adopts the following technical solution:

[0009] In order to achieve the above purpose, in-depth research has been conducted. In order to obtain a thin polyvinyl alcohol film, the higher the total stretching ratio of the polyvinyl alcohol film relative to the original length, the better. However, in the existing actual production process, in order to increase the total stretching ratio of the polyvinyl alcohol film, the film may break and have horizontal and vertical stripes during the production process, making it difficult to achieve a thin polarizing film. The present invention laminates the polyvinyl alcohol film with a high stretch ratio thermoplastic elastomer film that has been treated with plasma, and then stretches it to form a multi-layer stretched film.

[0010] A multi-layer stretched film with a large stretching ratio comprises a substrate film and a polyvinyl alcohol film bonded thereto. The substrate film is treated with plasma, bonded to the polyvinyl alcohol film and stretched to obtain the multi-layer stretched film.

[0011] Furthermore, the thickness of the substrate film is 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm or 60 μm.

[0012] Furthermore, the alcoholysis degree of the polyvinyl alcohol is greater than 98.0%; the degree of polymerization of the polyvinyl alcohol is greater than 1200; for example, the alcoholysis degree of the polyvinyl alcohol is greater than 99.0%; the degree of polymerization of the polyvinyl alcohol is 2400.

[0013] Furthermore, the thickness of the polyvinyl alcohol film is 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm or 60 μm.

[0014] To achieve the above object, the present invention discloses a method for preparing a multilayer stretched film with a large stretch ratio, comprising the following steps:

[0015] Step S1: Plasma-treating a thermoplastic elastomer substrate film in air and immediately laminating it with a polyvinyl alcohol film to obtain a laminated film; the plasma treatment time is 60-180 seconds, the treatment distance is 1-5 cm, and the corona treatment voltage is 30-80 V. For example, the plasma treatment time is 60 seconds, 80 seconds, 100 seconds, 120 seconds, 140 seconds, 160 seconds or 180 seconds, the treatment distance is 1 cm, 2 cm, 3 cm, 4 cm or 5 cm, and the corona treatment voltage is 30 V, 40 V, 50 V, 60 V, 70 V or 80 V.

[0016] Step S2: stretching the laminated film prepared in step 1 by a stretching device.

[0017] Step S3: peeling off the outer thermoplastic resin film in the laminated film to obtain a stretched film with a large stretching ratio.

[0018] Furthermore, in step S1, the polyvinyl alcohol film is prepared by the following method: PVA raw material, glycerol and sodium dodecylbenzene sulfonate surfactant are dissolved in deionized water in a sealed state at 100~150℃ to prepare PVA casting solution, and the dissolution reaction time is 1~10h; the formed casting solution is degassed and filtered by an extruder, extruded from a die, dried by a casting roller at 70~100℃, and then enters a drying roller to repeatedly dry the front and back sides of the film in the range of 40-100℃, and then enters an air flotation oven for heat treatment, and finally rolled up to obtain a PVA optical film; wherein the mass ratio of PVA raw material: glycerol: sodium dodecylbenzene sulfonate surfactant: deionized water is 950~1000:90~100:1:4000~5000.

[0019] The present invention discloses a multilayer stretched film with a large stretch ratio and a method for preparing the multilayer stretched film, so as to solve the problem of film breaking when the existing polyvinyl alcohol film is stretched, and produce high-quality multilayer stretched film materials used in high-performance polarizers for new display manufacturing. The yield of polyvinyl alcohol polarizing films is improved, the efficient production of polyvinyl alcohol polarizing films is promoted, the production cost is reduced, and the demand for thin display panels in today's information society is met.

[0020] Advantages and positive effects:

[0021] The present invention provides a method for preparing a multi-layer stretched film with a large stretch ratio, a plasma treatment process - a thermoplastic elastomer film is subjected to plasma treatment, and then laminated with a polyvinyl alcohol film into multiple layers, and then stretched to form a multi-layer stretched film, which can obtain a high-stretch ratio polyvinyl alcohol film without horizontal and vertical stripes, and is used to prepare a polarizing film with excellent polarizing performance. The production process is simple, the yield of the polyvinyl alcohol polarizing film is improved, the efficient production of the polyvinyl alcohol polarizing film is promoted, and the production and preparation cost is reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to explain the embodiments of the present invention and the design technology in the prior art in more detail, the following briefly summarizes the contents of the drawings that must be referred to when explaining the embodiments or the prior art. The present invention is further explained below in conjunction with the drawings.

[0023] FIG. 1 is a schematic flow diagram of a method for preparing a multilayer stretched film with a large stretch ratio.

[0024] FIG. 2 is a schematic diagram of the structure of a multilayer stretched film with a large stretch ratio.

[0025] FIG. 3 is a bar graph showing the contact angle change of the thermoplastic elastomer film before and after plasma treatment provided in Example 1 of the present invention.

[0026] FIG. 4 is an engineering stress-strain curve (a) of the multilayer stretched film provided in Example 2 of the present invention and a bar graph (b) showing the change in stretching ratio before and after lamination of the polyvinyl alcohol film.

[0027] FIG. 5 is a one-dimensional integral curve of wide-angle X-ray scattering of the multilayer stretched film provided in Example 2 of the present invention (a) and a graph showing the relationship between the stretching ratio and the crystallinity (b). DETAILED DESCRIPTION

[0028] The present invention provides a multilayer stretched film with a large stretch ratio and a method for preparing the multilayer stretched film, so as to increase the stretch ratio of the polyvinyl alcohol film and improve the phenomenon of horizontal and vertical stripes during stretching, so as to produce high-quality polyvinyl alcohol film materials for high-performance polarizers to meet the needs of new display preparation.

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] The preparation method of the multilayer stretched film provided by the present invention is as follows: as shown in FIG1 , a thermoplastic elastomer substrate film with a thickness of 45 μm is continuously rolled out from its film roll, and then immediately laminated with a polyvinyl alcohol film with a thickness of 30 μm continuously rolled out from its film roll after being subjected to plasma treatment in air to obtain a laminated film; the plasma treatment time is 180 seconds, the treatment distance is 5 cm, and the corona treatment voltage is 30 V. The laminated film is stretched by a stretching device to obtain a multilayer stretched film with a large stretch ratio.

[0031] Plasma treatment process

[0032] The plasma treatment bonding (the thermoplastic elastomer film is subjected to plasma treatment (plasma treatment time is 180 seconds, treatment distance is 5 cm, corona treatment voltage is 30V) by a corona treatment machine ("TW-2K" manufactured by Ruian Zhilin Corona Equipment Co., Ltd.) to activate its surface and bond it with the polyvinyl alcohol film. This is based on the convenience of subsequent stretching process and peeling of the thermoplastic elastomer film, as shown in Figure 2 (the 45μm thermoplastic elastomer substrate film is tightly bonded to the 30μm thick polyvinyl alcohol film).

[0033] Example 1

[0034] Step 1: 909g of polyvinyl alcohol (PVA) (polymerization degree 2400, alcoholysis degree greater than 99%, weight average molecular weight Mw of about 75kg·mo1-1, dispersity of 1.8, manufactured by Wanwei High-tech) raw material, 90.9g of glycerol, and 1g of sodium dodecylbenzene sulfonate surfactant were dissolved in 4000g of deionized water under a sealed condition at 150°C to prepare PVA casting solution, and the dissolution reaction time was 10h. The formed casting solution was degassed and filtered by the extruder and extruded from the die. After pre-drying treatment for 1 minute by a casting roller at 90°C, it entered 11 groups of drying rollers (temperature in the range of 40-100°C) to repeatedly dry the front and back of the film, and then entered an air flotation oven for drying (80°C, 5 minutes), and finally rolled up to obtain a PVA optical film with a thickness of 30μm.

[0035] Step 2: After a thermoplastic elastomer substrate film (Bemis Parafilm sealing film, PM998) with a thickness of 45 μm is continuously rolled out from its film roll, it is immediately laminated with a polyvinyl alcohol film with a thickness of 30 μm continuously rolled out from the film roll after plasma treatment in air to obtain a laminated film; the plasma treatment time is 180 seconds, the treatment distance is 5 cm, and the corona treatment voltage is 30 V.

[0036] Step 3: Stretch the laminated film prepared in step 2 by a stretching device. The stretching test is performed at a constant strain rate of 0.1 s -1 Uniaxial stretching was performed at room temperature in air at a fixed stretching ratio of 5.5.

[0037] Step 4: Peel off the outer thermoplastic resin film in the laminated film to obtain a stretched film with a large stretching ratio.

[0038] In step 2, the surface of the substrate film is activated after plasma treatment. The hydrophilicity of the sample surface is measured using the OCA 25 fully automatic contact angle measurement and profile analysis system. As shown in Figure 3, the contact angle of the paraffin sealing film (Parafilm) before and after plasma treatment changes. The contact angle of the untreated paraffin sealing film is 96.2°, and the contact angle of the paraffin sealing film after plasma treatment is reduced to 82.3°.

[0039] During the stretching process, the engineering stress-strain curves under different stretching conditions were obtained at room temperature by using a stretching rheometer. Among them, the stretching experiments were all performed at a constant strain rate of 0.1 s -1 The laminated film was uniaxially stretched in air at room temperature at a fixed stretch ratio of 5.5.

[0040] In the preparation of the above-mentioned multilayer stretched film, the substrate film was treated with plasma before lamination, and no curling was observed at the edge of the polyvinyl alcohol film, and no horizontal or vertical stripes were observed in the subsequent stretching process of the laminated film. A PVA film with a large stretch ratio (stretch ratio of 5.5) was obtained.

[0041] Example 2

[0042] The laminated film was prepared in the same manner as in Example 1 (same as step 1 and step 2 in Example 1). However, in the stretching process, the laminated film was uniaxially stretched in air at room temperature in the same manner as in Example 1, and the prepared laminated film was subjected to a stretchability test to record the elongation at break when stretched, which was recorded as the maximum stretch ratio. Similarly, the unlaminated polyvinyl alcohol film (prepared in step 1 of Example 1) was uniaxially stretched under the same conditions to obtain a series of mechanical property data as shown in Figure 4 (a). As shown in Figure 4 (b), the stretching ratio of the polyvinyl alcohol film was significantly improved before and after lamination. When the unlaminated polyvinyl alcohol film was uniaxially stretched, the maximum stretching ratio was 3.95, and when the prepared laminated film was stretched, the maximum stretching ratio was increased to 5.63.

[0043] After peeling off the thermoplastic elastomer film from the prepared multilayer stretched film, the obtained polyvinyl alcohol film with a large stretching ratio was measured for crystallinity by wide-angle X-ray diffraction (the incident beam used was CuKα rays with a wavelength of 1.54Å. The data were collected by a Pilatus300K detector with an exposure time of 30 min) (as shown in (a) in Figure 5). The crystallinity was compared with that of the unstretched polyvinyl alcohol film, as shown in (b) in Figure 5. The crystallinity of the unstretched polyvinyl alcohol film was 27.3%, and the crystallinity of the stretched polyvinyl alcohol film (stretching ratio of 4) was 25.2%, and the crystallinity decreased significantly.

[0044] In the preparation of the above-mentioned multilayer stretched film, the substrate film was plasma treated and then laminated, and no curling was observed at the edge of the polyvinyl alcohol film. In the subsequent stretching process of the laminated film, the maximum stretching ratio of the laminated film was significantly increased compared to the unlaminated polyvinyl alcohol film.

[0045] Example 3

[0046] A multilayer stretched film was prepared in the same manner as in Example 1 except that a polyolefin elastomer film (POE film, manufactured by Mitsui Chemicals, DF760) having a thickness of 45 μm was used as the thermoplastic resin film.

[0047] In the preparation of the multilayer stretched film, the substrate film was plasma treated for post-lamination, and no curling of the edge of the polyvinyl alcohol film was observed, and no horizontal or vertical stripes were observed in the subsequent stretching process of the laminated film. In addition, the thermoplastic elastomer film was easily peeled off.

[0048] Comparative Example 1

[0049] A pure polyvinyl alcohol film (prepared in step 1 of Example 1) without being laminated with a thermoplastic elastomer film was uniaxially stretched in air at room temperature, and the stretching process was the same as in Example 1. In the subsequent stretching process, the polyvinyl alcohol film broke when the stretching ratio was 300%.

[0050] Comparative Example 2

[0051] A multilayer stretched film was prepared in the same manner as in Example 1 except that a laminated film in which a 30 μm polyvinyl alcohol thin film layer was formed on a 45 μm thermoplastic elastomer film (Bemis Parafilm sealing film, PM998) by coating was used.

[0052] In the preparation of the above-mentioned multilayer stretched film, the substrate film was plasma treated for post-lamination, and no curling of the edge of the polyvinyl alcohol film was observed, and no horizontal and vertical stripes were observed in the subsequent stretching process of the laminated film. However, it was difficult to peel off the thermoplastic elastomer film.

[0053] Comparative Example 3

[0054] A multilayer stretched film was prepared in the same manner as in Example 1 except that a 45 μm thick polyvinyl chloride (PVC film, manufactured by Shengtai Plastics) was used as the base film instead of the 45 μm thick thermoplastic elastomer film (Bemis Parafilm sealing film, PM998).

[0055] In the preparation of the multilayer stretched film, the substrate film was post-laminated by plasma treatment, and the edge of the polyvinyl alcohol film curled up, and horizontal and vertical stripes appeared in the subsequent stretching process of the laminated film.

[0056] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A multi-layer stretched film with a large stretch ratio, characterized in that: The multilayer stretched film comprises a substrate film and a polyvinyl alcohol film bonded thereto. The substrate film is treated with plasma and then bonded to the polyvinyl alcohol film and stretched to obtain the multilayer stretched film.

2. The film according to claim 1, characterized in that The substrate film is a thermoplastic elastomer film, and the thermoplastic elastomer film includes a polyurethane-based TPE film (TPU), a styrene-based TPE film (SBS, SEBS, etc.), a polyolefin-based TPE film (TPO), a thermoplastic vulcanized rubber (TPV), a thermoplastic polyester elastomer (TPEE / COPE), a polyester copolymer TPE (COPE), an ethylene vinyl acetate copolymer (EVA) film, a polyolefin elastomer (POE), a polyallyl ester TPE (PEBA), a polylactic acid-based TPE (PLA-TPE), a polycarbonate / elastomer blend (PC / TPU, PC / ABS), a polyether ester TPE (COPE / PTG), a polycaprolactone-based TPE (PCL-TPE), a vinyl TPE (TPV / EVA), a polyurethane / polyester blend TPE (TPU / PET), a polyolefin elastomer (POE) plastic or a paraffin sealing film (parafilm).

3. The film according to claim 1, characterized in that The thickness of the substrate film is 10-60 μm.

4. The film according to claim 1, characterized in that The polyvinyl alcohol film is prepared by forming a film from polyvinyl alcohol without graft copolymerization reaction or through monomer graft copolymerization reaction.

5. The film according to claim 1, characterized in that The polyvinyl alcohol film is made of polyvinyl alcohol by a film-making method such as solution casting, extrusion blown film molding (dry and wet methods), water-added melt extrusion, anhydrous melt extrusion, continuous biaxial orientation, dry extrusion blow molding or film drawing machine.

6. The film according to claim 1, characterized in that The alcoholysis degree of the polyvinyl alcohol is greater than 98.0%; the polymerization degree of the polyvinyl alcohol is greater than 1200; The thickness of the polyvinyl alcohol film is 5 μm-60 μm.

7. The method for preparing a multi-layer stretched film with a large stretch ratio according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step S1: After the thermoplastic elastomer substrate film is treated with plasma in air, it is immediately laminated with the polyvinyl alcohol film to obtain a laminated film; the plasma treatment time is 60-180 seconds, the treatment distance is 1-5 cm, and the corona treatment voltage is 30-80 V; Step S2: stretching the laminated film prepared in step 1 by a stretching device; Step S3: peeling off the outer thermoplastic resin film in the laminated film to obtain a stretched film with a large stretching ratio.

8. The method according to claim 7, characterized in that In step S1, the polyvinyl alcohol film is prepared by the following method: PVA raw material, glycerol and sodium dodecylbenzene sulfonate surfactant are dissolved in deionized water under a sealed condition at 100-150°C to prepare a PVA casting solution, and the dissolution reaction time is 1-10 hours; the formed casting solution is degassed and filtered by an extruder, extruded from a die, dried by a casting roller at 70-100°C, and then enters a drying roller to repeatedly dry the front and back sides of the film in the range of 40-100°C, and then enters an air flotation oven for heat treatment, and finally rolled up to obtain a PVA optical film; wherein the mass ratio of PVA raw material: glycerol: sodium dodecylbenzene sulfonate surfactant: deionized water is 850-1000:80-100:1:3000-5000.

9. Use of the multi-layer stretched film with a large stretch ratio as claimed in claim 1 in a polarizer.

Citation Information

Patent Citations

  • Stretched laminate, preparation method for thin polarizer, thin polarizer prepared by using same and polarizing plate comprising same

    CN104395793A

  • Multilayer film

    CN104903761A

  • Stretch lamination body making method, stretch lamination body, polarizing film and making method thereof

    CN104950368A

  • Preparation method for thin polyvinyl alcohol (PVA) polarizing film

    CN105223639A

  • Laminate and method for preparing the same, and method for preparing polarizing film

    CN106526734A