Intermediate film for laminated glass, and laminated glass

By using an intermediate film of polyvinyl acetal resin with more than three layers of structure and a plasticizer in laminated glass, the problem of difficult to take into account both the bending rigidity and sound insulation properties of laminated glass in the prior art is solved, and the thin glass plate is realized High bending rigidity and good sound insulation.

CN118978348APending Publication Date: 2024-11-19SEKISUI CHEMICAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411149509.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2015-09-11
Filing Date
2016-09-08
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing laminated glass has insufficient bending rigidity, especially after the thickness of the glass plate is reduced, it is difficult to maintain high bending rigidity, and at the same time, it is difficult to take into account both sound insulation and bending rigidity.

Method used

The intermediate film for laminated glass with three or more layers of structure is adopted, which contains polyvinyl acetal resin and plasticizer. By adjusting the hydroxyl content and plasticizer content of each layer, it ensures that the intermediate film of laminated glass is completed and The bending rigidity and sound insulation during long-term use have been improved.

Benefits of technology

The bending rigidity and sound insulation of laminated glass are improved, ensuring that laminated glass of thin glass plates maintains high performance during use, and reducing material usage and environmental load.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978348A_ABST
    Figure CN118978348A_ABST
Patent Text Reader

Abstract

Provided is an intermediate film for laminated glass, which is capable of improving the flexural rigidity of laminated glass and improving the sound insulation properties of laminated glass. The intermediate film for laminated glass according to the present invention comprises first, second, and third layers containing a polyvinyl acetal resin and a plasticizer, and is characterized in that: the hydroxyl group content of the polyvinyl acetal resin in the first layer is lower than the hydroxyl group content of the polyvinyl acetal resin in the second and third layers; when the absolute value of the difference between the hydroxyl group content of the polyvinyl acetal resin in the second and third layers and the hydroxyl group content of the polyvinyl acetal resin in the first layer is XA and XB, the absolute values XA and XB are from 9 mol% to 11 mol% (inclusive). If Y is the content of the plasticizer in the interlayer for laminated glass relative to 100 parts by weight of the polyvinyl acetal resin in the interlayer for laminated glass, Y < =-1.68 XA + 56 and Y < =-1.68 XB + 56 are satisfied.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application based on a patent application with an application date of September 8, 2016, a priority date of September 11, 2015, an application number of 201680049703.0, and an invention name of “Intermediate film for laminated glass and laminated glass”. Technical Field

[0002] The present invention relates to an interlayer film for laminated glass for obtaining laminated glass. In addition, the present invention relates to laminated glass using the interlayer film for laminated glass. Background Art

[0003] Even if laminated glass is damaged by external impact, the amount of scattered glass fragments is small, and it is excellent in safety. Therefore, the laminated glass is widely used in automobiles, railway vehicles, aircraft, ships, buildings, etc. The laminated glass is manufactured by sandwiching an interlayer film for laminated glass between two glass plates.

[0004] The interlayer film for laminated glass includes a single-layer interlayer film having a single-layer structure and a multi-layer interlayer film having a structure of two or more layers.

[0005] As an example of the above-mentioned interlayer film for laminated glass, the following Patent Document 1 discloses a sound insulation layer comprising 100 parts by weight of a polyvinyl acetal resin having an acetalization degree of 60 to 85 mol%, 0.001 to 1.0 parts by weight of at least one metal salt of an alkali metal salt and an alkaline earth metal salt, and more than 30 parts by weight of a plasticizer. The sound insulation layer can be used as an interlayer film in a single layer.

[0006] In addition, a multilayer interlayer film in which the above-mentioned sound insulation layer and other layers are laminated is also described in the following Patent Document 1. The other layer laminated on the sound insulation layer comprises 100 parts by weight of a polyvinyl acetal resin having an acetalization degree of 60 to 85 mol%, 0.001 to 1.0 parts by weight of at least one metal salt of an alkali metal salt and an alkaline earth metal salt, and 30 parts by weight or less of a plasticizer.

[0007] Patent Document 2 below discloses an interlayer film which is a polymer layer having a glass transition temperature of 33° C. or higher. Patent Document 2 describes that the polymer layer is disposed between glass plates having a thickness of 4.0 mm or less.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2007-070200

[0011] Patent Document 2: US2013 / 0236711A1 Summary of the invention

[0012] Technical problem to be solved by the invention

[0013] The laminated glass using the conventional interlayer film described in Patent Documents 1 and 2 sometimes has low bending rigidity. Therefore, when the laminated glass is used as, for example, the side glass of an automobile, there is no frame to fix the laminated glass, and the laminated glass has low rigidity and bends, which sometimes causes a malfunction when the glass is opened or closed.

[0014] In recent years, in order to reduce the weight of laminated glass, the thickness of the glass plate has been reduced. In laminated glass obtained by sandwiching an interlayer film between two glass plates, if the thickness of the glass plate is reduced, it is difficult to maintain sufficiently high bending rigidity.

[0015] Even if the glass sheets are very thin, if the bending rigidity of the laminated glass can be increased by the interlayer film, the laminated glass can be made lighter. When the laminated glass is lightweight, the amount of materials used in the laminated glass can be reduced, thereby reducing the environmental load. In addition, when lightweight laminated glass is used in automobiles, fuel costs can be improved, resulting in a reduction in environmental load.

[0016] In addition, laminated glass using an intermediate film is also expected to have high sound insulation in addition to high bending rigidity. Patent Document 1 discloses laminated glass with high sound insulation, but it is difficult to improve the bending rigidity. Patent Document 2 discloses an intermediate film, which is formed by laminating a polymer layer having a glass transition temperature exceeding 33°C and a polymer layer having a glass transition temperature below 20°C. However, the laminated glass obtained using the intermediate film disclosed in Patent Document 2 has the following problems: not only is the bending rigidity of the laminated glass not sufficiently improved immediately after it is manufactured, but also the bending rigidity of the laminated glass is significantly reduced after a period of time has passed since the manufacture is completed.

[0017] The object of the present invention is to provide an intermediate film for laminated glass, which can not only improve the bending rigidity of the laminated glass just after it is manufactured, but also improve the bending rigidity of the laminated glass after a period of time has passed since the manufacture is completed, and can improve the sound insulation of the laminated glass. In addition, the object of the present invention is also to provide laminated glass using the above-mentioned intermediate film for laminated glass.

[0018] Technical solutions to solve problems

[0019] According to a broad aspect of the present invention, there is provided an interlayer film for laminated glass, which has a structure of three or more layers and contains a polyvinyl acetal resin and a plasticizer, and has:

[0020] The first layer contains a polyvinyl acetal resin and a plasticizer,

[0021] a second layer, which is laminated on the first surface of the first layer and contains a polyvinyl acetal resin and a plasticizer,

[0022] a third layer, which is laminated on a second surface of the first layer opposite to the first surface and contains a polyvinyl acetal resin and a plasticizer,

[0023] The hydroxyl content of the polyvinyl acetal resin in the first layer is lower than the hydroxyl content of the polyvinyl acetal resin in the second layer, and when the absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin in the second layer and the hydroxyl content of the polyvinyl acetal resin in the first layer is denoted as XA, the absolute value XA is 9 mol% or more and 11 mol% or less,

[0024] The hydroxyl content of the polyvinyl acetal resin in the first layer is lower than the hydroxyl content of the polyvinyl acetal resin in the third layer, and when the absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin in the third layer and the hydroxyl content of the polyvinyl acetal resin in the first layer is denoted as XB, the absolute value XB is 9 mol% or more and 11 mol% or less,

[0025] When the content of the plasticizer in the interlayer film for laminated glass relative to 100 parts by weight of the polyvinyl acetal resin in the interlayer film for laminated glass is denoted by Y,

[0026] Satisfies: Y≤-1.68XA+56, and Y≤-1.68XB+56.

[0027] In a specific aspect of the interlayer film for laminated glass of the present invention, the content of the plasticizer in the first layer relative to 100 parts by weight of the polyvinyl acetal resin in the first layer is greater than the content of the plasticizer in the second layer relative to 100 parts by weight of the polyvinyl acetal resin in the second layer.

[0028] In a specific aspect of the interlayer film for laminated glass of the present invention, the content of the plasticizer in the first layer relative to 100 parts by weight of the polyvinyl acetal resin in the first layer is greater than the content of the plasticizer in the third layer relative to 100 parts by weight of the polyvinyl acetal resin in the third layer.

[0029] In a specific aspect of the interlayer film for laminated glass of the present invention, the hydroxyl content of the polyvinyl acetal resin in the second layer is 32 mol % or more. In a specific aspect of the interlayer film for laminated glass of the present invention, the hydroxyl content of the polyvinyl acetal resin in the third layer is 32 mol % or more.

[0030] In a specific aspect of the interlayer film for laminated glass of the present invention, the absolute value XA is greater than 9.3 mol %. In a specific aspect of the interlayer film for laminated glass of the present invention, the absolute value XB is greater than 9.3 mol %.

[0031] In a specific aspect of the interlayer film for laminated glass of the present invention, the content of the plasticizer in the first layer is 55 parts by weight or more and 100 parts by weight or less based on 100 parts by weight of the polyvinyl acetal resin in the first layer.

[0032] In a specific aspect of the interlayer film for laminated glass of the present invention, the content of the plasticizer in the second layer relative to 100 parts by weight of the polyvinyl acetal resin in the second layer and the content of the plasticizer in the third layer relative to 100 parts by weight of the polyvinyl acetal resin in the third layer are 50 parts by weight or less.

[0033] In a specific aspect of the interlayer film for laminated glass of the present invention, the content Y of the plasticizer in the interlayer film for laminated glass is 25 parts by weight or more and 40 parts by weight or less based on 100 parts by weight of the polyvinyl acetal resin in the interlayer film for laminated glass.

[0034] In a specific aspect of the interlayer film for laminated glass of the present invention,

[0035] The polyvinyl acetal resin in the first layer is polyvinyl butyral resin,

[0036] The polyvinyl acetal resin in the second layer is polyvinyl butyral resin,

[0037] The polyvinyl acetal resin in the third layer is polyvinyl butyral resin.

[0038] In a specific aspect of the interlayer film for laminated glass of the present invention, the interlayer film for laminated glass is used to obtain laminated glass by using a first glass plate having a thickness of less than 2 mm and disposing the interlayer film for laminated glass between the first glass plate and a second glass plate.

[0039] According to a broad aspect of the present invention, there is provided a laminated glass comprising:

[0040] The first laminated glass component,

[0041] a second laminated glass component, and

[0042] The intermediate film for laminated glass,

[0043] The interlayer film for laminated glass is arranged between the first laminated glass component and the second laminated glass component.

[0044] In a specific aspect of the laminated glass of the present invention, the first laminated glass component is a first glass plate, and the thickness of the first glass plate is less than 2 mm.

[0045] Effects of the Invention

[0046] The interlayer film for laminated glass of the present invention has a structure of three or more layers and contains a polyvinyl acetal resin and a plasticizer, and has:

[0047] The first layer contains a polyvinyl acetal resin and a plasticizer,

[0048] a second layer, which is laminated on the first surface of the first layer and contains a polyvinyl acetal resin and a plasticizer,

[0049] a third layer, which is laminated on a second surface of the first layer opposite to the first surface and contains a polyvinyl acetal resin and a plasticizer,

[0050] The hydroxyl content of the polyvinyl acetal resin in the first layer is lower than the hydroxyl content of the polyvinyl acetal resin in the second layer, and when the absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin in the second layer and the hydroxyl content of the polyvinyl acetal resin in the first layer is denoted as XA, the absolute value XA is 9 mol% or more and 11 mol% or less,

[0051] The hydroxyl content of the polyvinyl acetal resin in the first layer is lower than the hydroxyl content of the polyvinyl acetal resin in the third layer, and when the absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin in the third layer and the hydroxyl content of the polyvinyl acetal resin in the first layer is denoted as XB, the absolute value XB is 9 mol% or more and 11 mol% or less,

[0052] When the content of the plasticizer in the interlayer film for laminated glass relative to 100 parts by weight of the polyvinyl acetal resin in the interlayer film for laminated glass is denoted by Y,

[0053] Satisfies: Y≤-1.68XA+56, and Y≤-1.68XB+56. Thus, the bending rigidity of the laminated glass can be improved not only immediately after production but also after a period of time has passed since production, and the sound insulation of the laminated glass can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] Figure 1 is a cross-sectional view schematically showing an interlayer film for laminated glass according to a first embodiment of the present invention;

[0055] Figure 2is a cross-sectional view schematically showing an interlayer film for laminated glass according to a second embodiment of the present invention;

[0056] Figure 3 This is a schematic diagram for explaining the method of measuring bending rigidity.

[0057] Marking Description

[0058] 1 First floor

[0059] 1a First surface

[0060] 1b Second surface

[0061] 2 Second floor

[0062] 2a Outer surface

[0063] 3 Third floor

[0064] 3a Outer surface

[0065] 11Intermediate film

[0066] 11A interlayer film (first layer)

[0067] 11a First surface

[0068] 11b Second surface

[0069] 21 First laminated glass component

[0070] 22 Second laminated glass component

[0071] 31 Laminated glass

[0072] 31A Laminated Glass DETAILED DESCRIPTION

[0073] Hereinafter, the present invention will be described in detail.

[0074] The intermediate film for laminated glass of the present invention (sometimes abbreviated as "intermediate film" in this specification) has a structure of more than three layers and contains a polyvinyl acetal resin and a plasticizer. The intermediate film of the present invention may have a structure of three layers or more than four layers. The intermediate film of the present invention has a first layer containing a polyvinyl acetal resin and a plasticizer. For example, the intermediate film of the present invention preferably has: a first layer containing a polyvinyl acetal resin and a plasticizer; a second layer laminated on a first surface of the first layer and containing a polyvinyl acetal resin and a plasticizer; and a third layer laminated on a second surface of the first layer opposite to the first surface and containing a polyvinyl acetal resin and a plasticizer. The second layer may be the outermost layer, or other layers may be laminated on the side of the second layer opposite to the side on which the first layer is laminated. The third layer may be the outermost layer, or other layers may be laminated on the side of the third layer opposite to the side on which the first layer is laminated.

[0075] In the intermediate film of the present invention, the hydroxyl content of the polyvinyl acetal resin in the first layer is lower than the hydroxyl content of the polyvinyl acetal resin in the second layer, and when the absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin in the second layer and the hydroxyl content of the polyvinyl acetal resin in the first layer is set to XA, the absolute value XA is greater than or equal to 9 mol% and less than or equal to 11 mol%, the hydroxyl content of the polyvinyl acetal resin in the first layer is lower than the hydroxyl content of the polyvinyl acetal resin in the third layer, and when the absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin in the third layer and the hydroxyl content of the polyvinyl acetal resin in the first layer is set to XB, the absolute value XB is greater than or equal to 9 mol% and less than or equal to 11 mol%.

[0076] In the interlayer film of the present invention, when the content of the plasticizer in the interlayer film for laminated glass relative to 100 parts by weight of the polyvinyl acetal resin in the interlayer film for laminated glass is denoted by Y, the following conditions are satisfied: Y≤-1.68XA+56 and Y≤-1.68XB+56.

[0077] In the intermediate film of the present invention, due to the above-mentioned structure, the bending rigidity of the laminated glass can be improved not only immediately after it is manufactured, but also after a period of time has passed since the manufacture is completed, and the sound insulation of the laminated glass can be improved. In addition, in order to obtain laminated glass, the intermediate film is mostly arranged between the first glass plate and the second glass plate. Even if the thickness of the first glass plate is very thin, the bending rigidity of the laminated glass can be sufficiently improved by using the intermediate film of the present invention. In addition, even if the thickness of both the first glass plate and the second glass plate is very thin, the bending rigidity of the laminated glass can be sufficiently improved by using the intermediate film of the present invention. It should be noted that when the thickness of both the first glass plate and the second glass plate is very thick, the bending rigidity of the laminated glass is further improved.

[0078] Furthermore, in the interlayer film of the present invention, since it has the above-mentioned structure, the sound insulating property of the laminated glass using the interlayer film can be improved.

[0079] The surface of the second layer opposite to the first layer side is preferably a surface of a laminated laminated glass component or a glass plate. The thickness of the glass plate laminated on the second layer is preferably less than 2 mm (preferably less than 1 mm). The surface of the third layer opposite to the first layer side is preferably a surface of a laminated laminated glass component or a glass plate. The thickness of the glass plate laminated on the third layer is preferably less than 2 mm (preferably less than 1 mm).

[0080] Since the bending rigidity can be sufficiently improved by the intermediate film, the intermediate film is preferably used to obtain laminated glass by using a first glass plate having a thickness of less than 2 mm (preferably less than 1 mm) and arranging the intermediate film for laminated glass between the first glass plate and the second glass plate. Since the bending rigidity can be sufficiently improved by the intermediate film, the intermediate film is more preferably used to obtain laminated glass by using a first glass plate having a thickness of less than 2 mm (preferably less than 1 mm) and a second glass plate having a thickness of less than 2 mm (preferably less than 1 mm) and arranging the intermediate film for laminated glass between the first glass plate and the second glass plate.

[0081] Hereinafter, specific embodiments of the present invention will be described with reference to the accompanying drawings.

[0082] Figure 1 In FIG. 1 , an interlayer film for laminated glass according to a first embodiment of the present invention is schematically shown in a cross-sectional view.

[0083] Figure 1The intermediate film 11 shown is a multilayer intermediate film having a structure of more than three layers. The intermediate film 11 is used to obtain laminated glass. The intermediate film 11 is an intermediate film for laminated glass. The intermediate film 11 includes a first layer 1, a second layer 2, and a third layer 3. The second layer 2 is laminated on the first surface 1a of the first layer 1. The third layer 3 is laminated on the second surface 1b of the first layer 1 opposite to the first surface 1a. The first layer 1 is an intermediate layer. The second layer 2 and the third layer 3 are protective layers, respectively, and in this embodiment, they are surface layers. The first layer 1 is sandwiched between the second layer 2 and the third layer 3. Therefore, the intermediate film 11 has a multilayer structure (second layer 2 / first layer 1 / third layer 3) in which the second layer 2, the first layer 1, and the third layer 3 are laminated in this order.

[0084] Hereinafter, details of the first layer, the second layer, and the third layer constituting the interlayer film of the present invention and details of each component contained in the first layer, the second layer, and the third layer will be described.

[0085] (Polyvinyl acetal resin)

[0086] The first layer contains a polyvinyl acetal resin (hereinafter, sometimes described as polyvinyl acetal resin (1)). The second layer preferably contains a polyvinyl acetal resin (hereinafter, sometimes described as polyvinyl acetal resin (2)). The third layer preferably contains a polyvinyl acetal resin (hereinafter, sometimes described as polyvinyl acetal resin (3)). The polyvinyl acetal resin (1), the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) may be the same or different, but from the perspective of further improving the sound insulation, the polyvinyl acetal resin (1) is preferably different from the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3). The polyvinyl acetal resin (1), the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) may be used alone or in combination of two or more.

[0087] The polyvinyl acetal resin can be produced, for example, by acetalizing polyvinyl alcohol with aldehyde. The polyvinyl acetal resin is preferably an acetalized product of polyvinyl alcohol. The polyvinyl alcohol is obtained, for example, by saponifying polyvinyl acetate. The degree of saponification of the polyvinyl alcohol is generally 70 to 99.9 mol%.

[0088] The average degree of polymerization of the polyvinyl alcohol (PVA) is preferably 200 or more, more preferably 500 or more, further preferably 1500 or more, further preferably 1600 or more, particularly preferably 2600 or more, and most preferably 2700 or more, preferably 5000 or less, more preferably 4000 or less, and further preferably 3500 or less. If the average degree of polymerization is greater than or equal to the lower limit, the penetration resistance of the laminated glass is further improved. If the average degree of polymerization is less than or equal to the upper limit, the interlayer film is easily formed.

[0089] The average degree of polymerization of the polyvinyl alcohol can be determined by a method in accordance with JIS K6726 "Testing methods for polyvinyl alcohol".

[0090] The acetal group in the polyvinyl acetal resin preferably has 3 to 5 carbon atoms, and preferably 4 or 5 carbon atoms.

[0091] As the above-mentioned aldehyde, an aldehyde having 1 to 10 carbon atoms can be preferably used. Examples of the above-mentioned aldehyde having 1 to 10 carbon atoms include formaldehyde, acetaldehyde, propionaldehyde, n-butyraldehyde, isobutyraldehyde, n-valeraldehyde, 2-ethylbutyraldehyde, n-hexanal, n-octanal, n-nonanal, n-decanal, and benzaldehyde. Among them, formaldehyde, propionaldehyde, n-butyraldehyde, isobutyraldehyde, n-hexanal, or n-valeraldehyde is preferred, formaldehyde, propionaldehyde, n-butyraldehyde, isobutyraldehyde, or n-valeraldehyde is more preferred, and n-butyraldehyde or n-valeraldehyde is further preferred. The above-mentioned aldehydes may be used alone or in combination of two or more.

[0092] The hydroxyl content of the polyvinyl acetal resin in the first layer is lower than that of the polyvinyl acetal resin in the second layer, thereby improving the sound insulation of the laminated glass. In addition, when the absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin in the second layer and the hydroxyl content of the polyvinyl acetal resin in the first layer is set to XA, the absolute value XA is greater than 9 mol% and less than 11 mol%, thereby improving the bending rigidity and sound insulation of the laminated glass. The hydroxyl content of the polyvinyl acetal resin in the first layer is preferably lower than that of the polyvinyl acetal resin in the second layer by 12 mol% or more, more preferably lower by 13 mol% or more, and further preferably lower by 14 mol% or more. The preferred lower limit of the above absolute value XA is 6 mol%, the more preferred lower limit is 7 mol%, the more preferred lower limit is 8 mol%, the preferred upper limit is 14 mol%, the more preferred upper limit is 13 mol%, and the further preferred upper limit is 12 mol%.

[0093] The hydroxyl content of the polyvinyl acetal resin in the first layer is lower than that of the polyvinyl acetal resin in the third layer, thereby improving the sound insulation of the laminated glass. In addition, when the absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin in the third layer and the hydroxyl content of the polyvinyl acetal resin in the first layer is set to XB, the absolute value XB is greater than 9 mol% and less than 11 mol%, thereby improving the bending rigidity and sound insulation of the laminated glass. The hydroxyl content of the polyvinyl acetal resin in the first layer is preferably lower than that of the polyvinyl acetal resin in the third layer by 12 mol% or more, more preferably lower by 13 mol% or more, and further preferably lower by 14 mol% or more. The preferred lower limit of the above absolute value XB is 6 mol%, the more preferred lower limit is 7 mol%, the more preferred lower limit is 8 mol%, the preferred upper limit is 14 mol%, the more preferred upper limit is 13 mol%, and the further preferred upper limit is 12 mol%.

[0094] The hydroxyl content (hydroxyl amount) of the polyvinyl acetal resin (1) is preferably 17 mol% or more, more preferably 20 mol% or more, further preferably 22 mol% or more, preferably 28 mol% or less, more preferably 27 mol% or less, further preferably 25 mol% or less, and particularly preferably 24 mol% or less. If the hydroxyl content is above the lower limit, the mechanical strength of the interlayer film is further improved. In particular, if the hydroxyl content of the polyvinyl acetal resin (1) is 20 mol% or more, the reaction efficiency is high and the productivity is excellent. If it is 28 mol% or less, the sound insulation of the laminated glass is further improved. In addition, if the hydroxyl content is below the upper limit, the softness of the interlayer film is increased, and the handling of the interlayer film becomes easy.

[0095] The hydroxyl content of the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) is preferably 25 mol% or more, more preferably 28 mol% or more, more preferably 30 mol% or more, further preferably 31.5 mol% or more, further preferably 32 mol% or more, particularly preferably 33 mol% or more, preferably 40 mol% or less, preferably 38 mol% or less, more preferably 37 mol% or less, particularly preferably 36 mol% or less. If the hydroxyl content is above the lower limit, the bending rigidity is further improved, and the adhesive force of the intermediate film is further improved. In addition, if the hydroxyl content is below the upper limit, the softness of the intermediate film becomes high, and the handling of the intermediate film becomes easy.

[0096] From the viewpoint of further improving the sound insulation, the absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin (1) and the hydroxyl content of the polyvinyl acetal resin (2), and the absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin (1) and the hydroxyl content of the polyvinyl acetal resin (3) are preferably 1 mol% or more, more preferably 5 mol% or more, further preferably 9 mol% or more, particularly preferably 10 mol% or more, and most preferably 12 mol% or more. The absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin (1) and the hydroxyl content of the polyvinyl acetal resin (2), and the absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin (1) and the hydroxyl content of the polyvinyl acetal resin (3) are preferably 20 mol% or less.

[0097] The hydroxyl content of the polyvinyl acetal resin is a value expressed as a percentage of the molar fraction obtained by dividing the amount of ethylene groups bonded with hydroxyl groups by the total amount of ethylene groups in the main chain. The amount of ethylene groups bonded with hydroxyl groups can be measured, for example, in accordance with JIS K6728 "Testing methods for polyvinyl butyral".

[0098] The degree of acetylation (acetyl group content) of the polyvinyl acetal resin (1) is preferably 0.01 mol% or more, more preferably 0.1 mol% or more, further preferably 7 mol% or more, further preferably 9 mol% or more, preferably 30 mol% or less, more preferably 25 mol% or less, further preferably 24 mol% or less, and particularly preferably 20 mol% or less. When the degree of acetylation is above the lower limit, the compatibility of the polyvinyl acetal resin and the plasticizer becomes high. When the degree of acetylation is below the upper limit, the moisture resistance of the interlayer film and the laminated glass becomes high. In particular, when the degree of acetylation of the polyvinyl acetal resin (1) is 0.1 mol% or more and 25 mol% or less, the penetration resistance is excellent.

[0099] The acetylation degree of the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) is preferably 0.01 mol% or more, more preferably 0.5 mol% or more, preferably 10 mol% or less, more preferably 2 mol% or less. If the acetylation degree is above the lower limit, the compatibility of the polyvinyl acetal resin and the plasticizer is improved. If the acetylation degree is below the upper limit, the moisture resistance of the interlayer film and the laminated glass is improved.

[0100] The acetylation degree is a value expressed as a percentage, which is a molar fraction obtained by dividing the amount of ethylene groups bonded with acetyl groups by the total amount of ethylene groups in the main chain. The amount of ethylene groups bonded with acetyl groups can be measured, for example, in accordance with JIS K6728 "Testing methods for polyvinyl butyral".

[0101] The degree of acetalization of the polyvinyl acetal resin (1) (the degree of butyralization in the case of a polyvinyl butyral resin) is preferably 47 mol% or more, more preferably 60 mol% or more, preferably 85 mol% or less, more preferably 80 mol% or less, and further preferably 75 mol% or less. If the degree of acetalization is above the lower limit, the compatibility of the polyvinyl acetal resin and the plasticizer becomes high. If the degree of acetalization is below the upper limit, the reaction time required for producing the polyvinyl acetal resin is shortened.

[0102] The acetalization degree of the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) (the butyralization degree in the case of using a polyvinyl butyral resin) is preferably 55 mol% or more, more preferably 60 mol% or more, preferably 75 mol% or less, more preferably 71 mol% or less. If the acetalization degree is above the lower limit, the compatibility of the polyvinyl acetal resin and the plasticizer becomes high. If the acetalization degree is below the upper limit, the reaction time required for producing the polyvinyl acetal resin is shortened.

[0103] The degree of acetalization is expressed as a percentage by subtracting the amount of ethylene groups bonded with hydroxyl groups and the amount of ethylene groups bonded with acetyl groups from the total amount of ethylene groups in the main chain and dividing the resulting difference by the total amount of ethylene groups in the main chain to obtain a molar percentage.

[0104] It should be noted that the above-mentioned hydroxyl content (hydroxyl amount), acetalization degree (butyralization degree) and acetylation degree are preferably calculated from the results of measurement according to the method of JIS K6728 "Testing methods for polyvinyl butyral". However, measurement according to ASTM D1396-92 may also be used. In the case where the polyvinyl acetal resin is a polyvinyl butyral resin, the above-mentioned hydroxyl content (hydroxyl amount), the above-mentioned acetalization degree (butyralization degree) and the above-mentioned acetylation degree can be calculated from the results of measurement according to the method of JIS K6728 "Testing methods for polyvinyl butyral".

[0105] From the viewpoint of further improving the penetration resistance of laminated glass, the polyvinyl acetal resin (1) is preferably a polyvinyl acetal resin (A) having an acetylation degree (a) of less than 8 mol % and 65 mol % or more, or a polyvinyl acetal resin (B) having an acetylation degree (b) of 8 mol % or more. The polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) may be the polyvinyl acetal resin (A) or the polyvinyl acetal resin (B).

[0106] The acetylation degree (a) of the polyvinyl acetal resin (A) is less than 8 mol%, preferably 7.9 mol% or less, more preferably 7.8 mol% or less, further preferably 6.5 mol% or less, particularly preferably 6 mol% or less, preferably 0.1 mol% or more, more preferably 0.5 mol% or more, further preferably 2 mol% or more, particularly preferably 5 mol% or more, and most preferably 5.5 mol% or more. When the acetylation degree (a) is 0.1 mol% or more and less than 8 mol%, the migration of the plasticizer can be easily controlled, and the sound insulation of the laminated glass is further improved.

[0107] The acetalization degree (a) of the polyvinyl acetal resin (A) is 65 mol% or more, preferably 66 mol% or more, more preferably 67 mol% or more, further preferably 67.5 mol% or more, particularly preferably 75 mol% or more, preferably 85 mol% or less, more preferably 84 mol% or less, further preferably 83 mol% or less, and particularly preferably 82 mol% or less. If the acetalization degree (a) is above the lower limit, the sound insulation of the laminated glass is further improved. If the acetalization degree (a) is below the upper limit, the reaction time required for producing the polyvinyl acetal resin (A) can be shortened.

[0108] The hydroxyl content (a) of the polyvinyl acetal resin (A) is preferably 18 mol% or more, more preferably 19 mol% or more, further preferably 20 mol% or more, particularly preferably 21 mol% or more, and most preferably 23 mol% or more, preferably 31 mol% or less, more preferably 30 mol% or less, further preferably 29 mol% or less, and particularly preferably 28 mol% or less. If the hydroxyl content (a) is above the lower limit, the adhesive force of the first layer is further improved. If the hydroxyl content (a) is below the upper limit, the sound insulation of the laminated glass is further improved.

[0109] The degree of acetylation (b) of the polyvinyl acetal resin (B) is 8 mol% or more, preferably 9 mol% or more, more preferably 9.5 mol% or more, further preferably 10 mol% or more, particularly preferably 10.5 mol% or more, preferably 30 mol% or less, more preferably 28 mol% or less, further preferably 26 mol% or less, particularly preferably 24 mol% or less. If the degree of acetylation (b) is above the lower limit, the sound insulation of the laminated glass is further improved. If the degree of acetylation (b) is below the upper limit, the reaction time required for producing the polyvinyl acetal resin (B) can be shortened.

[0110] The acetalization degree (b) of the polyvinyl acetal resin (B) is preferably 50 mol% or more, more preferably 53 mol% or more, further preferably 55 mol% or more, particularly preferably 60 mol% or more, preferably 78 mol% or less, more preferably 75 mol% or less, further preferably 72 mol% or less, particularly preferably 70 mol% or less. If the acetalization degree (b) is above the lower limit, the sound insulation of the laminated glass is further improved. If the acetalization degree (b) is below the upper limit, the reaction time required for producing the polyvinyl acetal resin (B) can be shortened.

[0111] The hydroxyl content (b) of the polyvinyl acetal resin (B) is preferably 18 mol% or more, more preferably 19 mol% or more, further preferably 20 mol% or more, particularly preferably 21 mol% or more, and most preferably 23 mol% or more, preferably 31 mol% or less, more preferably 30 mol% or less, further preferably 29 mol% or less, and particularly preferably 28 mol% or less. If the hydroxyl content (b) is above the lower limit, the adhesive force of the first layer is further improved. If the hydroxyl content (b) is below the upper limit, the sound insulation of the laminated glass is further improved.

[0112] It is preferable that the polyvinyl acetal resin (A) and the polyvinyl acetal resin (B) are each a polyvinyl butyral resin.

[0113] (Plasticizer)

[0114] The first layer preferably contains a plasticizer (hereinafter, sometimes described as plasticizer (1)). The second layer preferably contains a plasticizer (hereinafter, sometimes described as plasticizer (2)). The third layer preferably contains a plasticizer (hereinafter, sometimes described as plasticizer (3)). By using a polyvinyl acetal resin and a plasticizer in combination, the adhesion of the layer containing the polyvinyl acetal resin and the plasticizer to the laminated glass component or other layers becomes moderately high. The plasticizer is not particularly limited. The plasticizer (1), the plasticizer (2) and the plasticizer (3) may be the same or different. The plasticizer (1), the plasticizer (2) and the plasticizer (3) may be used alone or in combination of two or more.

[0115] Examples of the plasticizer include organic ester plasticizers such as monobasic organic acid esters and polybasic organic acid esters, and organic phosphoric acid plasticizers such as organic phosphoric acid plasticizers and organic phosphorous acid plasticizers. Among them, organic ester plasticizers are preferred. The plasticizer is preferably a liquid plasticizer.

[0116] Examples of the monobasic organic acid ester include glycol esters obtained by reacting glycols with monobasic organic acids. Examples of the glycol include triethylene glycol, tetraethylene glycol, and tripropylene glycol. Examples of the monobasic organic acid include butyric acid, isobutyric acid, hexanoic acid, 2-ethylbutyric acid, heptanoic acid, n-octanoic acid, 2-ethylhexanoic acid, n-nonanoic acid, and decanoic acid.

[0117] Examples of the polybasic organic acid esters include ester compounds of polybasic organic acids and linear or branched alcohols having 4 to 8 carbon atoms. Examples of the polybasic organic acids include adipic acid, sebacic acid, and azelaic acid.

[0118] Examples of the organic ester plasticizer include triethylene glycol di-2-ethyl propionate, triethylene glycol di-2-ethyl butyrate, triethylene glycol di-2-ethyl hexanoate, triethylene glycol dioctanoate, triethylene glycol di-n-octanoate, triethylene glycol di-n-heptanoate, tetraethylene glycol di-n-heptanoate, dibutyl sebacate, dioctyl azelate, dibutyl carbitol adipate, ethylene glycol di-2-ethyl butyrate, 1,3-propylene glycol di-2-ethyl butyrate, 1,4-butylene glycol di-2-ethyl butyrate, diethylene glycol dioctanoate, dibutyl sebacate, dioctyl azelate, dibutyl carbitol adipate, ethylene glycol di-2-ethyl butyrate, 1,3-propylene glycol di-2-ethyl butyrate, 1,4-butylene glycol di-2-ethyl butyrate, diethylene glycol dioctanoate, dibutyl sebacate, dibutyl azelate, dibutyl carbitol adipate, ethylene glycol di-2-ethyl butyrate, 1,3-propylene glycol di-2-ethyl butyrate, 1,4-butylene glycol di-2-ethyl butyrate, diethylene glycol dioctanoate ... The invention also includes the following: alcohol di-2-ethylbutyrate, diethylene glycol di-2-ethylhexanoate, dipropylene glycol di-2-ethylbutyrate, triethylene glycol di-2-ethylvalerate, tetraethylene glycol di-2-ethylbutyrate, diethylene glycol dicaprylate, dihexyl adipate, dioctyl adipate, hexylcyclohexyl adipate, a mixture of heptyl adipate and nonyl adipate, diisononyl adipate, diisodecyl adipate, heptylnonyl adipate, dibutyl sebacate, oil-modified sebacic acid alcohol acid, and a mixture of phosphoric acid ester and adipic acid ester, etc. Organic ester plasticizers other than these can be used. Other adipic acid esters other than the above-mentioned adipic acid esters can also be used.

[0119] Examples of the organic phosphoric acid plasticizer include tributoxyethyl phosphate, isodecylphenyl phosphate, and triisopropyl phosphate.

[0120] The plasticizer is preferably a diester plasticizer represented by the following formula (1).

[0121] [Chemical formula 1]

[0122]

[0123] In the above formula (1), R1 and R2 each represent an organic group having 2 to 10 carbon atoms, R3 represents an ethylene group, an isopropylene group or an n-propylene group, and p represents an integer from 3 to 10. In the above formula (1), R1 and R2 each represent an organic group having 5 to 10 carbon atoms, more preferably an organic group having 6 to 10 carbon atoms.

[0124] The plasticizer is preferably di(2-butoxyethyl)adipate (DBEA), triethylene glycol di-2-ethylhexanoate (3GO), triethylene glycol di-2-ethylbutyrate (3GH) or triethylene glycol di-2-ethylpropionate, more preferably contains triethylene glycol di-2-ethylhexanoate (3GO), triethylene glycol di-2-ethylbutyrate (3GH) or triethylene glycol di-2-ethylpropionate, further preferably contains triethylene glycol di-2-ethylhexanoate or triethylene glycol di-2-ethylbutyrate, and particularly preferably contains triethylene glycol di-2-ethylhexanoate.

[0125] The content of the plasticizer (2) relative to 100 parts by weight of the polyvinyl acetal resin (2) (hereinafter, sometimes described as content (2)) and the content of the plasticizer (3) relative to 100 parts by weight of the polyvinyl acetal resin (3) (hereinafter, sometimes described as content (3)) are preferably 10 parts by weight or more, more preferably 15 parts by weight or more, further preferably 20 parts by weight or more, particularly preferably 24 parts by weight or more, preferably 50 parts by weight or less, more preferably 40 parts by weight or less, further preferably 35 parts by weight or less, particularly preferably 32 parts by weight or less, and most preferably 30 parts by weight or less. When the content (2) and the content (3) are at least the lower limit, the softness of the interlayer film is improved, and the handling of the interlayer film is facilitated. When the content (2) and the content (3) are at most the upper limit, the penetration resistance of the laminated glass is further improved.

[0126] The content of the plasticizer (1) relative to 100 parts by weight of the polyvinyl acetal resin (1) (hereinafter, sometimes described as content (1)) is preferably 50 parts by weight or more, more preferably 55 parts by weight or more, further preferably 60 parts by weight or more, preferably 100 parts by weight or less, more preferably 90 parts by weight or less, further preferably 85 parts by weight or less, and particularly preferably 80 parts by weight or less. When the content (1) is at least the lower limit, the softness of the interlayer film increases, and the handling of the interlayer film becomes easy. When the content (1) is at most the upper limit, the penetration resistance of the laminated glass is further improved.

[0127] In order to improve the sound insulation of laminated glass, the content (1) is preferably greater than the content (2), and the content (1) is preferably greater than the content (3).

[0128] In order to further improve the sound insulation of laminated glass, the absolute value of the difference between the content (2) and the content (1), and the absolute value of the difference between the content (3) and the content (1) are preferably 10 parts by weight or more, more preferably 15 parts by weight or more, and even more preferably 20 parts by weight or more. The absolute value of the difference between the content (2) and the content (1), and the absolute value of the difference between the content (3) and the content (1) are preferably 80 parts by weight or less, more preferably 75 parts by weight or less, and even more preferably 70 parts by weight or less.

[0129] In addition, from the viewpoint of further improving the sound insulation of the laminated glass, the content Y is preferably 25 parts by weight or more, more preferably 26 parts by weight or more, and further preferably 27 parts by weight or more. From the viewpoint of further improving the rigidity of the laminated glass, the content Y is preferably 41 parts by weight or less, more preferably 40.5 parts by weight or less, and further preferably 40 parts by weight or less.

[0130] The conventional sound insulation film is composed of a surface layer, a sound insulation layer and a laminated surface layer, and the sound insulation layer is softer than the surface layer. The rigidity of the laminated glass obtained by using such a sound insulation film becomes lower. In order to prevent the rigidity of the laminated glass from being reduced due to the sound insulation layer, US2013 / 0236711A1 discloses a method of increasing the glass transition temperature of the surface layer. However, it is only to increase the glass transition temperature of the surface layer. Not only can the rigidity of the intermediate film of the laminated glass just after it is manufactured not be fully obtained, but there is also a problem that the rigidity of the laminated glass is significantly reduced after a period of time from the completion of the manufacture. On the other hand, if the sound insulation layer is hardened, there is a problem that sufficient sound insulation cannot be obtained. Therefore, the inventors of the present invention studied the causes of the above problems and found that the migration of the plasticizer contained in the surface layer and the sound insulation layer is the cause of the above problems. That is to say, if the plasticizer contained in the surface layer can be prevented from excessively migrating to the sound insulation layer or if the plasticizer contained in the sound insulation layer can be prevented from excessively migrating to the surface layer, not only the rigidity of the laminated glass just after it is manufactured can be improved, but also the rigidity of the laminated glass after a period of time after it is manufactured can be improved.

[0131] Specific solutions to these problems are described below. By making the hydroxyl content of the polyvinyl acetal resin in the first layer lower than the hydroxyl content of the polyvinyl acetal resin in the third layer, and making the hydroxyl content of the polyvinyl acetal resin in the first layer lower than the hydroxyl content of the polyvinyl acetal resin in the third layer, the sound insulation of the laminated glass can be improved. However, there is a tendency for the plasticizer in the second layer and the plasticizer in the third layer to move to the first layer. The movement of the plasticizer will be excessive over time, and the first layer will become soft, and the bending rigidity of the laminated glass will decrease. In addition, by setting the lower limit of the absolute value XA of the difference between the hydroxyl content of the polyvinyl acetal resin in the first layer and the hydroxyl content of the polyvinyl acetal resin in the second layer and the absolute value XB of the difference between the hydroxyl content of the polyvinyl acetal resin in the first layer and the hydroxyl content of the polyvinyl acetal resin in the third layer to 6 mol%, the sound insulation of the laminated glass can be improved, and by setting the upper limit to 14 mol%, the bending rigidity of the laminated glass can be improved. The preferred lower limit of the absolute value XA and the absolute value XB is 7 mol%, more preferably 8 mol%, and further preferably 9 mol%, and the preferred upper limit is 13 mol%, more preferably 12 mol%, and further preferably 11 mol%.

[0132] In addition, when the content of the plasticizer in the interlayer film for laminated glass relative to 100 parts by weight of the polyvinyl acetal resin in the interlayer film for laminated glass is Y, the following conditions are satisfied: Y≤-1.68XA+56 and Y≤-1.68XB+56. As the absolute value XA and the absolute value XB increase, the plasticizer in the second layer and the plasticizer in the third layer tend to move to the first layer. Therefore, even when the absolute value XA and the absolute value XB increase, by reducing the content of the plasticizer in the interlayer film for laminated glass relative to 100 parts by weight of the polyvinyl acetal resin in the interlayer film for laminated glass to Y, that is, the total number of plasticizers in the interlayer film for laminated glass, the flexural rigidity of the interlayer film for laminated glass can be improved not only when the laminated glass is just manufactured, but also when a period of time has passed since the manufacture is completed. On the other hand, as the absolute value XA and the absolute value XB become smaller, the plasticizer in the second layer and the plasticizer in the third layer tend not to move to the first layer. Therefore, even when the absolute value XA and the absolute value XB become smaller, by increasing the content of the plasticizer in the interlayer film for laminated glass to Y, i.e., the total number of parts of the plasticizer in the interlayer film for laminated glass, the sound insulation property of the interlayer film for laminated glass can be improved.

[0133] In order to further improve the rigidity of laminated glass, the content Y preferably satisfies: Y≤-1.68XA+56, more preferably: Y≤-1.68XA+55.5, and more preferably: Y≤-1.68XA+55. In order to further improve the sound insulation of laminated glass, the content Y preferably satisfies: Y≥-1.68XA+47, more preferably: Y≥-1.68XA+48, and more preferably: Y≥-1.68XA+49. In order to further improve the rigidity of laminated glass, the content Y preferably satisfies: Y≤-1.68XB+56, more preferably: Y≤-1.68XB+55.5, and more preferably: Y≤-1.68XB+55. In order to further improve the sound insulation of the laminated glass, the content Y preferably satisfies: Y ≥ -1.68XB+47, more preferably satisfies: Y ≥ -1.68XB+48, further preferably satisfies: Y ≥ -1.68XB+49, and particularly preferably satisfies: Y ≥ -1.68XB+50.

[0134] Here, the content Y of the plasticizer in the interlayer film for laminated glass relative to 100 parts by weight of the polyvinyl acetal resin in the interlayer film for laminated glass is described. When the interlayer film for laminated glass is cut into 0.5 cm in length and 5 cm in width, and the second layer, the first layer, and the third layer are stacked in a three-layer structure, the interlayer film for laminated glass is placed in an environment of 23±2°C and 25±5% humidity for 12 hours, and then the second layer is peeled off from the first layer, and then the third layer is peeled off from the first layer. The weight of the first layer after peeling is measured using an analytical electronic balance (GH-200 manufactured by A&D Co.), and the weight of the first layer after peeling is set to X1 (mg). The first layer after peeling was measured using a gas chromatograph (GC-2014 manufactured by Shimadzu Corporation) to measure the content of polyvinyl acetal resin in the first layer as a percentage of the total amount of polyvinyl acetal resin and plasticizer (R1) and the content of plasticizer in the first layer as a percentage of the total amount of polyvinyl acetal resin and plasticizer (P1). It should be noted that the R1 is obtained by dividing the content of polyvinyl acetal resin in the first layer by the total amount of polyvinyl acetal resin and plasticizer in the first layer, and the P1 is obtained by dividing the content of plasticizer in the first layer by the total amount of polyvinyl acetal resin and plasticizer in the first layer. Similarly, the weight X2 (mg) of the second layer, the content of polyvinyl acetal resin in the second layer as a percentage of the total amount of polyvinyl acetal resin and plasticizer (R2) and the content of plasticizer in the second layer as a percentage of the total amount of polyvinyl acetal resin and plasticizer (P2) were measured. Similarly, the weight X3 (mg) of the third layer, the content of the polyvinyl acetal resin in the third layer relative to the total amount of the polyvinyl acetal resin and the plasticizer (R3), and the content of the plasticizer in the third layer relative to the total amount of the polyvinyl acetal resin and the plasticizer (P3) are measured. In addition, the content of the polyvinyl acetal resin in the first layer X1 (mg) × R1, the content of the polyvinyl acetal resin in the second layer X2 (mg) × R2, and the content of the polyvinyl acetal resin in the third layer X3 (mg) × R3 are calculated, and the content of the polyvinyl acetal resin in the interlayer film for laminated glass is set to X1 (mg) × R1 + X2 (mg) × R2 + X3 (mg) × R3. Similarly, calculate the content of plasticizer in the first layer X1 (mg) × P1, the content of plasticizer in the second layer X2 (mg) × P2, and the content of plasticizer in the third layer X3 (mg) × P3, and set the content of plasticizer in the laminated glass intermediate film to X1 (mg) × P1 + X2 (mg) × P2 + X3 (mg) × P3.From the result, the content Y of the plasticizer in the interlayer film for laminated glass relative to 100 parts by weight of the polyvinyl acetal resin in the interlayer film for laminated glass is calculated by [{X1(mg)×P1+X2(mg)×P2+X3(mg)×P3} / {X1(mg)×R1+X2(mg)×R2+X3(mg)×R3}]. When the interlayer film for laminated glass has a multilayer structure of 4 or more layers, it is preferred to determine the first layer, the second layer, and the third layer, and measure the content Y of the plasticizer in the interlayer film for laminated glass relative to 100 parts by weight of the polyvinyl acetal resin in the interlayer film for laminated glass in a similar manner to the case of having a three-layer structure. It should be noted that, when at least one of the first layer, the second layer and the third layer contains a colored region, and the colored region is present only on a portion of the planar direction of the intermediate film for laminated glass, it is preferred that the intermediate film for laminated glass be cut into a piece with a length of 0.5 cm and a width of 5 cm without containing a colored region, and the content Y of the plasticizer in the intermediate film for laminated glass relative to 100 parts by weight of the polyvinyl acetal resin in the intermediate film for laminated glass be measured.

[0135] (Silicon dioxide particles)

[0136] The first layer preferably contains silica particles. By using silica particles, the sound insulation can be maintained without reducing the rigidity, and the adhesion between the layers can be improved. The silica particles can be used alone or in combination of two or more.

[0137] The specific surface area of ​​the silica particles measured by the BET method is preferably 50 m 2 / g or more, more preferably 100m 2 / g or more, more preferably 200m 2 / g or more, particularly preferably 250m 2 / g or more, most preferably 300m 2 / g or more, preferably 500m 2 / g or less. The above-mentioned specific surface area can be measured by a gas adsorption method using a specific surface area / pore distribution measuring device. Examples of the above-mentioned measuring device include "ASAP2420" manufactured by Shimadzu Corporation.

[0138] The content of the silica particles is preferably 1 part by weight or more, more preferably 5 parts by weight or more, further preferably 10 parts by weight or more, particularly preferably 15 parts by weight or more, preferably 70 parts by weight or less, more preferably 64 parts by weight or less, further preferably 60 parts by weight or less, more preferably 55 parts by weight or less, particularly preferably 45 parts by weight or less, and most preferably 35 parts by weight or less, relative to 100 parts by weight of the polyvinyl acetal resin (1). When the content of the silica particles is above the lower limit, the adhesion between the layers is further improved, and the rigidity is further improved. When the content of the silica is below the upper limit, the sound insulation is further improved.

[0139] (Thermal insulation compound)

[0140] The intermediate film preferably contains a heat-insulating compound. The first layer preferably contains a heat-insulating compound. The second layer preferably contains a heat-insulating compound. The third layer preferably contains a heat-insulating compound. The heat-insulating compound may be used alone or in combination of two or more.

[0141] Ingredient X:

[0142] The intermediate film preferably contains at least one component X selected from the group consisting of a phthalocyanine compound, a naphthalocyanine compound, and an anthracyanine compound. The first layer preferably contains the component X. The second layer preferably contains the component X. The third layer preferably contains the component X. The component X is a heat-insulating compound. The component X may be used alone or in combination of two or more.

[0143] The component X is not particularly limited. As the component X, a conventionally known phthalocyanine compound, naphthalocyanine compound, or anthraphthalocyanine compound can be used.

[0144] From the viewpoint of further improving the heat shielding properties of the interlayer film and laminated glass, the component X is preferably at least one selected from phthalocyanine, phthalocyanine derivatives, naphthalocyanine and naphthalocyanine derivatives, and more preferably at least one selected from phthalocyanine and phthalocyanine derivatives.

[0145] From the viewpoint of effectively improving the heat insulation and maintaining the visible light transmittance at a higher level for a long time, the component X preferably contains a vanadium atom or a copper atom. The component X preferably contains a vanadium atom, and also preferably contains a copper atom. The component X is more preferably at least one of phthalocyanine containing a vanadium atom or a copper atom and a phthalocyanine derivative containing a vanadium atom or a copper atom. From the viewpoint of further improving the heat insulation of the interlayer film and the laminated glass, the component X preferably has a structural unit in which an oxygen atom is bonded to a vanadium atom.

[0146] In 100 wt% of the layer (first layer, second layer or third layer) containing the above-mentioned component X, the content of the above-mentioned component X is preferably 0.001 wt% or more, more preferably 0.005 wt% or more, further preferably 0.01 wt% or more, particularly preferably 0.02 wt% or more, preferably 0.2 wt% or less, more preferably 0.1 wt% or less, further preferably 0.05 wt% or less, particularly preferably 0.04 wt% or less. If the content of the above-mentioned component X is above the above lower limit and below the above upper limit, the heat insulation is sufficiently improved and the visible light transmittance is sufficiently improved. For example, the visible light transmittance can be 70% or more.

[0147] Thermal insulation particles:

[0148] The above-mentioned intermediate film preferably contains heat-insulating particles. The above-mentioned first layer preferably contains the above-mentioned heat-insulating particles. The above-mentioned second layer preferably contains the above-mentioned heat-insulating particles. The above-mentioned third layer preferably contains the above-mentioned heat-insulating particles. The above-mentioned heat-insulating particles are heat-insulating compounds. By using heat-insulating particles, infrared rays (heat rays) can be effectively blocked. The above-mentioned heat-insulating particles can be used alone or in combination of two or more.

[0149] From the viewpoint of further improving the heat shielding property of laminated glass, the heat shielding particles are more preferably metal oxide particles. The heat shielding particles are preferably particles formed of a metal oxide (metal oxide particles).

[0150] Compared with ultraviolet rays, infrared rays with wavelengths longer than visible light, which are longer than 780nm, have less energy. However, infrared rays have a greater thermal effect, and if they are absorbed by a substance, they are released in the form of heat. Therefore, infrared rays are generally referred to as heat rays. By using the above-mentioned heat-insulating particles, infrared rays (heat rays) can be effectively blocked. In addition, heat-insulating particles refer to particles that can absorb infrared rays.

[0151] As a specific example of the above-mentioned heat-insulating particles, metal oxide particles such as aluminum-doped tin oxide particles, indium-doped tin oxide particles, antimony-doped tin oxide particles (ATO particles), gallium-doped zinc oxide particles (GZO particles), indium-doped zinc oxide particles (IZO particles), aluminum-doped zinc oxide particles (AZO particles), niobium-doped titanium oxide particles, sodium-doped tungsten oxide particles, cesium-doped tungsten oxide particles, thallium-doped tungsten oxide particles, rubidium-doped tungsten oxide particles, tin-doped indium oxide particles (ITO particles), tin-doped zinc oxide particles, silicon-doped zinc oxide particles, or lanthanum hexaboride (LaB6) particles can be cited. Heat-insulating particles other than these can also be used. Among them, metal oxide particles are preferred because the blocking function of the heat line is high, and ATO particles, GZO particles, IZO particles, ITO particles or tungsten oxide particles are more preferred, and ITO particles or tungsten oxide particles are particularly preferred. In particular, because the blocking function of the heat line is high and easy to obtain, tin-doped indium oxide particles (ITO particles) and tungsten oxide particles are preferred.

[0152] From the viewpoint of further improving the heat insulation of the interlayer film and the laminated glass, the tungsten oxide particles are preferably metal-doped tungsten oxide particles. The above-mentioned "tungsten oxide particles" include metal-doped tungsten oxide particles. As the above-mentioned metal-doped tungsten oxide particles, specifically, sodium-doped tungsten oxide particles, cesium-doped tungsten oxide particles, thallium-doped tungsten oxide particles, and rubidium-doped tungsten oxide particles can be cited.

[0153] From the viewpoint of further improving the heat shielding property of the interlayer film and the laminated glass, the cesium-doped tungsten oxide particles are particularly preferred. From the viewpoint of further improving the heat shielding property of the interlayer film and the laminated glass, the cesium-doped tungsten oxide particles are preferably of the formula: Cs 0.33 Tungsten oxide particles represented by WO3.

[0154] The average particle size of the heat-insulating particles is preferably 0.01 μm or more, more preferably 0.02 μm or more, preferably 0.1 μm or less, and more preferably 0.05 μm or less. If the average particle size is above the lower limit, the heat-shielding property is sufficiently improved. If the average particle size is below the upper limit, the dispersibility of the heat-insulating particles is improved.

[0155] The above-mentioned “average particle diameter” refers to a volume average particle diameter. The average particle diameter can be measured using a particle size distribution measuring device (“UPA-EX150” manufactured by Nikkiso Co., Ltd.) or the like.

[0156] In 100 wt% of the layer (first layer, second layer or third layer) containing the above-mentioned heat-insulating particles, the content of the above-mentioned heat-insulating particles is preferably 0.01 wt% or more, more preferably 0.1 wt% or more, further preferably 1 wt% or more, particularly preferably 1.5 wt% or more, preferably 6 wt% or less, more preferably 5.5 wt% or less, further preferably 4 wt% or less, particularly preferably 3.5 wt% or less, and most preferably 3 wt% or less. If the content of the above-mentioned heat-insulating particles is above the above lower limit and below the above upper limit, the heat insulation is sufficiently improved and the visible light transmittance is sufficiently improved.

[0157] (Metal Salt)

[0158] The intermediate film preferably contains at least one metal salt selected from alkali metal salts, alkaline earth metal salts and Mg salts (hereinafter sometimes referred to as metal salt M). The first layer preferably contains the metal salt M. The second layer preferably contains the metal salt M. The third layer preferably contains the metal salt M. By using the metal salt M, it is easy to control the adhesion between the intermediate film and the laminated glass component or the adhesion between the layers of the intermediate film. The metal salt M may be used alone or in combination of two or more.

[0159] The metal salt M preferably includes at least one metal selected from the group consisting of Li, Na, K, Rb, Cs, Mg, Ca, Sr, and Ba. The metal salt included in the intermediate film preferably includes at least one metal selected from the group consisting of K and Mg.

[0160] The metal salt M is more preferably an alkali metal salt of an organic acid having 2 to 16 carbon atoms, an alkaline earth metal salt of an organic acid having 2 to 16 carbon atoms, or a magnesium salt of an organic acid having 2 to 16 carbon atoms, and is further preferably a magnesium salt of a carboxylate having 2 to 16 carbon atoms or a potassium salt of a carboxylate having 2 to 16 carbon atoms.

[0161] The magnesium salt of the carboxylate having 2 to 16 carbon atoms and the potassium salt of the carboxylate having 2 to 16 carbon atoms are not particularly limited, and examples thereof include magnesium acetate, potassium acetate, magnesium propionate, potassium propionate, magnesium 2-ethylbutyrate, potassium 2-ethylbutyrate, magnesium 2-ethylhexanoate, and potassium 2-ethylhexanoate.

[0162] The total content of Mg and K in the layer (first layer, second layer or third layer) containing the metal salt M is preferably 5 ppm or more, more preferably 10 ppm or more, further preferably 20 ppm or more, preferably 300 ppm or less, more preferably 250 ppm or less, further preferably 200 ppm or less. When the total content of Mg and K is above the lower limit and below the upper limit, the adhesion between the interlayer film and the laminated glass component and the adhesion between the layers of the interlayer film can be further well controlled.

[0163] (UV shielding agent)

[0164] The above-mentioned intermediate film preferably contains an ultraviolet shielding agent. The above-mentioned first layer preferably contains an ultraviolet shielding agent. The above-mentioned second layer preferably contains an ultraviolet shielding agent. The above-mentioned third layer preferably contains an ultraviolet shielding agent. By using an ultraviolet shielding agent, even if the intermediate film and the laminated glass are used for a long time, the visible light transmittance is not easy to be further reduced. The above-mentioned ultraviolet shielding agent can be used alone or in combination of two or more.

[0165] The ultraviolet shielding agent includes an ultraviolet absorber. The ultraviolet shielding agent is preferably an ultraviolet absorber.

[0166] As the above-mentioned ultraviolet shielding agent, for example, there can be mentioned: an ultraviolet shielding agent containing a metal atom, an ultraviolet shielding agent containing a metal oxide, an ultraviolet shielding agent having a benzotriazole structure, an ultraviolet shielding agent having a benzophenone structure, an ultraviolet shielding agent having a triazine structure, an ultraviolet shielding agent having a malonate structure, an ultraviolet shielding agent having an oxalylanilide structure, and an ultraviolet shielding agent having a benzoate structure.

[0167] Examples of the ultraviolet shielding agent containing a metal atom include platinum particles, particles whose surfaces are coated with silicon oxide, palladium particles, and particles whose surfaces are coated with silicon oxide. The ultraviolet shielding agent is preferably not a heat shielding particle.

[0168] The above-mentioned ultraviolet shielding agent is preferably an ultraviolet shielding agent with a benzotriazole structure, an ultraviolet shielding agent with a benzophenone structure, an ultraviolet shielding agent with a triazine structure or an ultraviolet shielding agent with a benzoate structure, more preferably an ultraviolet shielding agent with a benzotriazole structure or an ultraviolet shielding agent with a benzophenone structure, and further preferably an ultraviolet shielding agent with a benzotriazole structure.

[0169] As the above-mentioned ultraviolet shielding agent comprising metal oxide, for example, zinc oxide, titanium oxide and cerium oxide etc. can be enumerated. In addition, about the above-mentioned ultraviolet shielding agent comprising metal oxide, the surface can also be coated. As the coating material on the surface of the above-mentioned ultraviolet shielding agent comprising metal oxide, insulating metal oxide, hydrolyzable organosilicon compound and polysiloxane compound etc. can be enumerated.

[0170] As the ultraviolet shielding agent having a benzotriazole structure, for example, there can be mentioned ultraviolet shielding agents having a benzotriazole structure such as 2-(2'-hydroxy-5'-methylphenyl)benzotriazole ("Tinuvin P" manufactured by BASF), 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole ("Tinuvin 320" manufactured by BASF), 2-(2'-hydroxy-3'-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole ("Tinuvin 326" manufactured by BASF), and 2-(2'-hydroxy-3',5'-dipentylphenyl)benzotriazole ("Tinuvin 328" manufactured by BASF). From the aspect of excellent performance in absorbing ultraviolet rays, the ultraviolet shielding agent is preferably an ultraviolet shielding agent having a benzotriazole structure containing a halogen atom, and more preferably an ultraviolet shielding agent having a benzotriazole structure containing a chlorine atom.

[0171] Examples of the ultraviolet shielding agent having a benzophenone structure include octabenzone ("Chimassorb 81" manufactured by BASF Corporation) and the like.

[0172] Examples of the ultraviolet shielding agent having a triazine structure include "LA-F70" manufactured by ADEKA Corporation and 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[(hexyl)oxy]-phenol ("Tinuvin 1577FF" manufactured by BASF Corporation).

[0173] Examples of the ultraviolet shielding agent having a malonate structure include dimethyl 2-(p-methoxybenzylidene)malonate, tetraethyl-2,2-(1,4-phenylenedimethylene)bismalonate, and 2-(p-methoxybenzylidene)-bis(1,2,2,6,6-pentamethyl-4-piperidinyl)malonate.

[0174] Examples of commercially available products of the ultraviolet shielding agent having a malonic acid ester structure include Hostavin B-CAP, Hostavin PR-25, and Hostavin PR-31 (all manufactured by Clariant).

[0175] Examples of the ultraviolet shielding agent having an oxalic acid anilide structure include oxalic acid diamides having an aromatic group substituted on a nitrogen atom, such as N-(2-ethylphenyl)-N'-(2-ethoxy-5-tert-butylphenyl) oxalic acid diamide, N-(2-ethylphenyl)-N'-(2-ethoxy-phenyl) oxalic acid diamide, and 2-ethyl-2'-ethoxy-oxyanilide ("Sanduvor VSU" manufactured by Clariant).

[0176] Examples of the ultraviolet shielding agent having a benzoate structure include 2,4-di-tert-butylphenyl-3,5-di-tert-butyl-4-hydroxybenzoate ("Tinuvin 120" manufactured by BASF Corporation).

[0177] From the viewpoint of further suppressing the reduction of visible light transmittance after the time has passed, in the layer (first layer, second layer or third layer) 100 wt % comprising the above-mentioned ultraviolet shielding agent, the content of the above-mentioned ultraviolet shielding agent is preferably more than 0.1 wt %, more preferably more than 0.2 wt %, more preferably more than 0.3 wt %, particularly preferably more than 0.5 wt %, preferably less than 2.5 wt %, more preferably less than 2 wt %, further preferably less than 1 wt %, particularly preferably less than 0.8 wt %. Especially by in the layer 100 wt % comprising the above-mentioned ultraviolet shielding agent, the content of the above-mentioned ultraviolet shielding agent is more than 0.2 wt %, which can significantly suppress the reduction of the visible light transmittance after the time has passed of the intermediate film and the laminated glass.

[0178] (Antioxidant)

[0179] The intermediate film preferably contains an antioxidant. The first layer preferably contains an antioxidant. The second layer preferably contains an antioxidant. The third layer preferably contains an antioxidant. The antioxidant may be used alone or in combination of two or more.

[0180] As the above-mentioned antioxidant, phenolic antioxidants, sulfur antioxidants and phosphorus antioxidants can be mentioned. The above-mentioned phenolic antioxidants are antioxidants having a phenol skeleton. The above-mentioned sulfur antioxidants are antioxidants containing sulfur atoms. The above-mentioned phosphorus antioxidants are antioxidants containing phosphorus atoms.

[0181] The antioxidant is preferably a phenolic antioxidant or a phosphorus antioxidant.

[0182] Examples of the phenolic antioxidant include 2,6-di-tert-butyl-p-cresol (BHT), butylated hydroxyanisole (BHA), 2,6-di-tert-butyl-4-ethylphenol, stearyl-β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 2,2'-methylenebis(4-methyl-6-butylphenol), 2,2'-methylenebis-(4-ethyl-6-tert-butylphenol), 4,4'-butylidene-bis(3-methyl-6-tert-butylphenol), 1,1,3-tri( 2-methyl-hydroxy-5-tert-butylphenyl) butane, tetrakis[methylene-3-(3',5'-butyl-4-hydroxyphenyl) propionate]methane, 1,3,3-tris(2-methyl-4-hydroxy-5-tert-butylphenol) butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl) benzene, bis(3,3'-tert-butylphenol) butyrate and bis(3-tert-butyl-4-hydroxy-5-methylphenylpropionate) ethylenebis(ethylene oxide), etc. It is preferred to use one or two or more of these antioxidants.

[0183] Examples of the phosphorus antioxidant include tridecyl phosphite, tritridecyl phosphite, triphenyl phosphite, trinonylphenyl phosphite, bistridecyl pentaerythritol diphosphite, bisdecyl pentaerythritol diphosphite, tris(2,4-di-tert-butylphenyl)phosphite, bis(2,4-di-tert-butyl-6-methylphenyl)ethyl phosphite, tris(2,4-di-tert-butylphenyl)phosphite, and 2,2'-methylenebis(4,6-di-tert-butyl-1-phenoxy)(2-ethylhexyloxy)phosphite, etc. It is preferred to use one or two or more of these antioxidants.

[0184] Examples of commercially available antioxidants include “IRGANOX 245” manufactured by BASF, “IRGAFOS 168” manufactured by BASF, “IRGAFOS 38” manufactured by BASF, “Sumilizer BHT” manufactured by Sumitomo Chemical Industries, Ltd., and “IRGANOX 1010” manufactured by BASF.

[0185] In order to maintain a high visible light transmittance of the interlayer film and the laminated glass for a long time, the content of the antioxidant in 100 wt% of the interlayer film or in 100 wt% of the layer (first layer, second layer or third layer) containing the antioxidant is preferably 0.1 wt% or more. In addition, since the effect of adding the antioxidant will be saturated, the content of the antioxidant in 100 wt% of the interlayer film or in 100 wt% of the layer containing the antioxidant is preferably 2 wt% or less.

[0186] (Other ingredients)

[0187] The first layer, the second layer and the third layer may contain additives such as coupling agents containing silicon, aluminum or titanium, dispersants, surfactants, flame retardants, antistatic agents, pigments, dyes, adhesion modifiers, moisture resistance agents, fluorescent brighteners and infrared absorbers as needed. These additives may be used alone or in combination of two or more.

[0188] (Other details of interlayer film for laminated glass)

[0189] From the viewpoint of improving the bending rigidity of laminated glass, the equivalent rigidity of the interlayer film at 25°C is 2.4 MPa or more. From the viewpoint of further improving the bending rigidity of laminated glass, the equivalent rigidity of the interlayer film at 25°C is preferably 3 MPa or more, more preferably 4 MPa or more, more preferably 5 MPa or more, and particularly preferably 9 MPa or more. The bending rigidity of the interlayer film at 25°C is preferably 30 MPa or less, more preferably 20 MPa or less.

[0190] It should be noted that, in order to improve the equivalent rigidity, the first layer preferably contains silicon dioxide particles. In addition, in order to improve the equivalent rigidity, the crosslinking degree of the polyvinyl acetal resin in the first layer can be appropriately increased. In addition, in order to improve the equivalent rigidity, it is preferred to appropriately select the thickness of each layer.

[0191] From the viewpoint of further improving the sound insulation of laminated glass, the glass transition temperature of the first layer is preferably 15° C. or lower, more preferably 10° C. or lower, further preferably 5° C. or lower, particularly preferably 0° C. or lower. The glass transition temperature of the first layer is preferably -20° C. or higher.

[0192] From the viewpoint of further improving the bending rigidity of laminated glass, the glass transition temperature of the first layer is preferably lower than the glass transition temperatures of the second layer and the third layer. By containing silica particles in the first layer having a glass transition temperature lower than that of the second layer and the third layer, and having the second layer and the third layer having a glass transition temperature higher than that of the first layer, the bending rigidity of laminated glass can be significantly improved. From the viewpoint of further improving the bending rigidity of laminated glass, the absolute value of the difference between the glass transition temperature of the first layer and the glass transition temperature of the second layer and the third layer is preferably 10°C or more, more preferably 20°C or more, further preferably 30°C or more, and particularly preferably 35°C or more. The absolute value of the difference between the glass transition temperature of the first layer and the glass transition temperature of the second layer and the third layer is preferably 70°C or less.

[0193] As a method for measuring the glass transition temperature, the following method can be cited: the obtained interlayer is stored at room temperature of 23±2°C and humidity of 25±5% for 12 hours, and then the viscoelasticity is measured using a viscoelasticity measuring device "DVA-200" of IT Measurement Control Co., Ltd. Preferably, the interlayer is cut into a longitudinal width of 8 mm and a transverse width of 5 mm, and the temperature is raised from -30°C to 100°C at a heating rate of 5°C / min in a shear mode, and the glass transition temperature is measured under the conditions of a frequency of 1 Hz and a strain of 0.08%.

[0194] From the viewpoint of improving the flexural rigidity of laminated glass, the Young's modulus of the first layer at 25°C is preferably 0.4 MPa or more, more preferably 0.6 MPa or more, further preferably 0.8 MPa or more, and is preferably 6 MPa or less, more preferably 5 MPa or less, further preferably 4 MPa or less.

[0195] From the viewpoint of improving the flexural rigidity of laminated glass, the Young's modulus of the second layer and the third layer at 25°C is preferably 3 MPa or more, more preferably 10 MPa or more, further preferably 100 MPa or more, and preferably 700 MPa or less, more preferably 500 MPa or less, further preferably 400 MPa or less.

[0196] It should be noted that, in order to adjust the Young's modulus to an appropriate range, the first layer preferably contains silica particles. In addition, in order to adjust the Young's modulus to an appropriate range, the crosslinking degree of the thermoplastic resin in the first layer may be appropriately increased.

[0197] The thickness of the intermediate film is not particularly limited. From the perspective of practicality and sufficient improvement of the penetration resistance and bending rigidity of the laminated glass, the thickness of the intermediate film is preferably 0.1 mm or more, more preferably 0.25 mm or more, preferably 3 mm or less, further preferably 2 mm or less, and more preferably 1.5 mm or less. If the thickness of the intermediate film is above the lower limit, the penetration resistance and bending rigidity of the laminated glass become higher. If the thickness of the intermediate film is below the upper limit, the transparency of the intermediate film becomes better.

[0198] The thickness of the intermediate film is set to T. The thickness of the first layer is preferably 0.0625T or more. More preferably, it is 0.1T or more, preferably 0.4T or less, more preferably 0.375T or less, further preferably 0.25T or less, and further preferably 0.15T or less. When the thickness of the first layer is 0.4T or less, the bending rigidity is further improved.

[0199] The thickness of each of the second layer and the third layer is preferably 0.3T or more, more preferably 0.3125T or more, further preferably 0.375T or more, preferably 0.9375T or less, more preferably 0.9T or less. The thickness of each of the second layer and the third layer may be 0.46875T or less, or 0.45T or less. In addition, when the thickness of each of the second layer and the third layer is above the lower limit and below the upper limit, the rigidity and sound insulation of the laminated glass are further improved.

[0200] The total thickness of the second layer and the third layer is preferably 0.625 T or more, more preferably 0.75 T or more, further preferably 0.85 T or more, preferably 0.9375 T or less, more preferably 0.9 T or less. In addition, when the total thickness of the second layer and the third layer is below the upper limit and below the lower limit, the rigidity and sound insulation of the laminated glass are further improved.

[0201] There is no particular limitation on the method for producing the intermediate film. Examples of the method for producing the intermediate film of the present invention include a method of laminating the obtained layers after forming the layers using the resin compositions for forming the layers; and a method of laminating the layers by co-extruding the resin compositions for forming the layers using an extruder. In order to be suitable for continuous production, a method of producing by extrusion molding is preferred.

[0202] From the perspective of excellent manufacturing efficiency of the intermediate film, it is preferred that the second layer and the third layer contain the same polyvinyl acetal resin, more preferably the second layer and the third layer contain the same polyvinyl acetal resin and the same plasticizer, and further preferably the second layer and the third layer are formed by the same resin composition.

[0203] The intermediate film preferably has a concavo-convex shape on at least one of the two side surfaces. The intermediate film preferably has a concavo-convex shape on the two side surfaces. There is no particular limitation on the method for forming the concavo-convex shape, and for example, a lip embossing method, an embossing roller method, a calendering roller method, and a profile extrusion method can be cited. The embossing roller method is preferred because a large number of concavo-convex shapes with a constant concavo-convex pattern can be quantitatively formed.

[0204] (Laminated glass)

[0205] Figure 2 It is a schematic representation of the use Figure 1 1 is a cross-sectional view of an example of a laminated glass including the interlayer film for laminated glass shown.

[0206] Figure 2The laminated glass 31 shown includes a first laminated glass member 21, a second laminated glass member 22, and an intermediate film 11. The intermediate film 11 is disposed between the first laminated glass member 21 and the second laminated glass member 22 in a sandwiched manner.

[0207] A first laminated glass component 21 is laminated on a first surface 11a of the intermediate film 11. A second laminated glass component 22 is laminated on a second surface 11b of the intermediate film 11 opposite to the first surface 11a. The first laminated glass component 21 is laminated on an outer surface 2a of the second layer 2. The second laminated glass component 22 is laminated on an outer surface 3a of the third layer 3.

[0208] Thus, the laminated glass of the present invention comprises a first laminated glass component, a second laminated glass component, and an interlayer film, and the interlayer film is the interlayer film for laminated glass of the present invention. In the laminated glass of the present invention, the interlayer film is arranged between the first laminated glass component and the second laminated glass component.

[0209] As the laminated glass component, glass plates and PET (polyethylene terephthalate) films can be cited. Laminated glass includes not only laminated glass formed by sandwiching an intermediate film between two glass plates, but also laminated glass formed by sandwiching an intermediate film between a glass plate and a PET film, etc. The laminated glass preferably has a laminated body of glass plates, and uses at least one glass plate.

[0210] Examples of the glass plate include inorganic glass and organic glass. Examples of the inorganic glass include float glass, heat absorbing glass, heat reflecting glass, polished glass, patterned glass, and wired glass. Organic glass is a synthetic resin glass used in place of inorganic glass. Examples of the organic glass include polycarbonate plates and poly(meth)acrylic resin plates. Examples of the poly(meth)acrylic resin plates include polymethyl(meth)acrylate plates.

[0211] The thickness of the laminated glass component is preferably 1 mm or more, preferably 5 mm or less, and more preferably 3 mm or less. In addition, when the laminated glass component is a glass plate, the thickness of the glass plate is preferably 0.5 mm or more, more preferably 0.7 mm or more, preferably 5 mm or less, and more preferably 3 mm or less. In the case where the laminated glass component is a PET film, the thickness of the PET film is preferably 0.03 mm or more, and preferably 0.5 mm or less.

[0212] By using the interlayer film of the present invention, the high flexural modulus of the laminated glass can be maintained even when the thickness of the laminated glass is very thin. From the viewpoint of reducing the environmental load by making the laminated glass lighter, or reducing the material of the laminated glass, or reducing the environmental load by improving the fuel cost of automobiles by making the laminated glass lighter, the thickness of the glass plate is preferably 2 mm or less, more preferably less than 2 mm, further preferably 1.8 mm or less, further preferably 1.5 mm or less, further preferably 1 mm or less, further preferably 0.8 mm or less, and particularly preferably 0.7 mm or less.

[0213] The manufacturing method of the above-mentioned laminated glass is not particularly limited. For example, an intermediate film is sandwiched between the above-mentioned first laminated glass component and the above-mentioned second laminated glass component, and the air remaining between the above-mentioned first laminated glass component, the above-mentioned second laminated glass component and the intermediate film is removed by a pressing roller or by placing it in a rubber bag for decompression and suction. Thereafter, pre-bonding is performed at about 70 to 110°C to obtain a laminate. Next, the laminate is placed in an autoclave, or pressed and pressed at about 120 to 150°C and a pressure of 1 to 1.5 MPa. In this way, laminated glass can be obtained. When manufacturing the above-mentioned laminated glass, the first layer, the second layer and the third layer can be laminated.

[0214] The above-mentioned intermediate film and the above-mentioned laminated glass can be used for automobiles, rail vehicles, aircraft, ships and buildings, etc. The above-mentioned intermediate film and the above-mentioned laminated glass can also be used for purposes other than these purposes. The above-mentioned intermediate film and the above-mentioned laminated glass are preferably intermediate films and laminated glasses for vehicles or buildings, and are more preferably intermediate films and laminated glasses for vehicles. The above-mentioned intermediate film and the above-mentioned laminated glass can be used for windshields, side window glasses, rear windshields or roof glasses of automobiles, etc. The above-mentioned intermediate film and the above-mentioned laminated glass are suitable for automobiles. The above-mentioned intermediate film is used to obtain laminated glass of automobiles.

[0215] From the viewpoint of obtaining a laminated glass with better transparency, the above-mentioned visible light transmittance of the laminated glass is preferably 65% ​​or more, and more preferably 70% or more. The visible light transmittance of the laminated glass can be measured in accordance with JIS R3211 (1998). The visible light transmittance of the laminated glass obtained by sandwiching the interlayer film for laminated glass of the present invention between two sheets of green glass (heat absorbing flat glass) with a thickness of 2 mm in accordance with JIS R3208 is preferably 70% or more. The visible light transmittance is more preferably 75% or more.

[0216] The present invention is described in more detail below with reference to the following examples, but the present invention is not limited to these examples.

[0217] Prepare the following materials.

[0218] (Polyvinyl acetal resin)

[0219] The polyvinyl acetal resins shown in Table 1 below were used. All the polyvinyl acetal resins used were acetalized with n-butyraldehyde having 4 carbon atoms. Regarding the polyvinyl acetal resin, the degree of acetalization (degree of butyralization), degree of acetylation and hydroxyl content were measured by a method in accordance with JIS K6728 "Testing methods for polyvinyl butyral". In addition, when measured by ASTM D1396-92, the same values ​​as those by the method in accordance with JIS K6728 "Testing methods for polyvinyl butyral" were shown.

[0220] (Plasticizer)

[0221] Triethylene glycol di-2-ethylhexanoate (3GO)

[0222] (UV shielding agent)

[0223] Tinuvin 326 (2-(2'-hydroxy-3'-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole, "Tinuvin 326" manufactured by BASF)

[0224] (Antioxidant)

[0225] BHT (2,6-di-tert-butyl-p-cresol)

[0226] (Example 1)

[0227] Preparation of the composition for forming the first layer:

[0228] 100 parts by weight of a polyvinyl acetal resin of the type shown in Table 1 below, 60 parts by weight of a plasticizer (3GO), 0.2 parts by weight of a UV shielding agent (Tinuvin 326), and 0.2 parts by weight of an antioxidant (BHT) were mixed to obtain a composition for forming a first layer.

[0229] Preparation of the composition for forming the second layer and the third layer:

[0230] 100 parts by weight of a polyvinyl acetal resin of the type shown in Table 1 below, 34 parts by weight of a plasticizer (3GO), 0.2 parts by weight of a UV shielding agent (Tinuvin 326), and 0.2 parts by weight of an antioxidant (BHT) were mixed to obtain a composition for forming the second layer and the third layer.

[0231] Production of intermediate film:

[0232] The composition for forming the first layer and the compositions for forming the second and third layers were coextruded using a coextruder to produce an intermediate film (thickness 780 μm) having a laminated structure of second layer (thickness 340 μm) / first layer (thickness 100 μm) / third layer (thickness 340 μm).

[0233] Preparation of laminated glass A (for measuring bending rigidity)

[0234] Prepare two cleaned and dried glass plates (transparent float glass, 25 cm long x 10 cm wide x 0.7 mm thick). Sandwich the obtained intermediate film between the two glass plates to obtain a laminate. Put the obtained laminate into a rubber bag and deaerate it at a vacuum degree of 2660 Pa (20 torr) for 20 minutes. Then, keep it at 90°C in an autoclave in a degassed state for 30 minutes and perform vacuum pressing. Place the laminate that has undergone the above pre-pressing in an autoclave at 135°C and a pressure of 1.2 MPa (12 kg / cm 2 ) for 20 minutes to obtain laminated glass A.

[0235] Preparation of laminated glass B (for measuring sound insulation)

[0236] The obtained intermediate film was cut into a size of 30 cm in length and 2.5 cm in width. Next, the intermediate film was sandwiched between two sheets of transparent glass (30 cm in length, 2.5 cm in width, and 2.5 mm in thickness) based on JIS R3208 to obtain a laminate. The laminate was placed in a rubber bag and degassed at a vacuum of 2.6 kPa for 20 minutes. Then, the laminate was transferred to an oven in a degassed state and kept at 90°C for 30 minutes for vacuum pressing to pre-press the laminate. In an autoclave, the pre-pressed laminate was pressed for 20 minutes at 135°C and a pressure of 1.2 MPa to obtain laminated glass B.

[0237] (Examples 2 to 12 and Comparative Examples 1 to 10)

[0238] The types and addition amounts of the polyvinyl acetal resin and plasticizer used in the composition for forming the first layer and the composition for forming the second layer and the third layer were set as shown in Tables 1 and 2 below, and the thicknesses of the first layer, the second layer and the third layer were set as shown in Tables 1 and 2. The interlayer film and the laminated glass were obtained in the same manner as in Example 1 except for the above. In Examples 2 to 12 and Comparative Examples 1 to 10, the same types of ultraviolet shielding agents and antioxidants as in Example 1 were added in the same amounts as in Example 1 (0.2 parts by weight relative to 100 parts by weight of the polyvinyl acetal resin).

[0239] (evaluate)

[0240] (1) Measurement of the content Y of the plasticizer in the interlayer film for laminated glass relative to 100 parts by weight of the polyvinyl acetal resin in the interlayer film for laminated glass

[0241] The interlayer film for laminated glass was cut into 0.5 cm in length and 5 cm in width. In the case of a three-layer structure formed by laminating the first layer, the second layer, and the third layer, the interlayer film for laminated glass was placed in an environment of 23±2°C and 25±5% humidity for 12 hours, and then the second layer was peeled off from the first layer, and then the third layer was peeled off from the first layer. The weight of the first layer after peeling was measured using an analytical electronic balance (GH-200 manufactured by A&D Corporation), and the weight of the first layer after peeling was set to X1 (mg). The first layer after peeling was measured using a gas chromatograph (GC-2014 manufactured by Shimadzu Corporation), and the content (R1) of the polyvinyl acetal resin in the first layer to the total amount of the polyvinyl acetal resin and the plasticizer and the content (P1) of the plasticizer in the first layer to the total amount of the polyvinyl acetal resin and the plasticizer were measured. It should be noted that the above R1 is obtained by dividing the content of the polyvinyl acetal resin in the above first layer by the total amount of the polyvinyl acetal resin and the plasticizer in the above first layer, and the above P1 is obtained by dividing the content of the plasticizer in the first layer by the total amount of the polyvinyl acetal resin and the plasticizer in the above first layer. Similarly, the weight X2 (mg) of the above second layer, the content of the polyvinyl acetal resin in the above second layer to the total amount of the polyvinyl acetal resin and the plasticizer (R2), and the content of the plasticizer in the above second layer to the total amount of the polyvinyl acetal resin and the plasticizer (P2) are measured. Similarly, the weight X3 (mg) of the above third layer, the content of the polyvinyl acetal resin in the above third layer to the total amount of the polyvinyl acetal resin and the plasticizer (R3), and the content of the plasticizer in the above third layer to the total amount of the polyvinyl acetal resin and the plasticizer (P3) are measured. In addition, the content of the polyvinyl acetal resin in the first layer is calculated as X1 (mg) × R1, the content of the polyvinyl acetal resin in the second layer is calculated as X2 (mg) × R2, and the content of the polyvinyl acetal resin in the third layer is calculated as X3 (mg) × R3, and the content of the polyvinyl acetal resin in the interlayer film for laminated glass is set to X1 (mg) × R1 + X2 (mg) × R2 + X3 (mg) × R3. Similarly, the content of the plasticizer in the first layer is calculated as X1 (mg) × P1, the content of the plasticizer in the second layer is calculated as X2 (mg) × P2, and the content of the plasticizer in the third layer is calculated as X3 (mg) × P3, and the content of the plasticizer in the interlayer film for laminated glass is set to X1 (mg) × P1 + X2 (mg) × P2 + X3 (mg) × P3. From the result, the content Y of the plasticizer in the interlayer film for laminated glass relative to 100 parts by weight of the polyvinyl acetal resin in the interlayer film for laminated glass is calculated by [{X1(mg)×P1+X2(mg)×P2+X3(mg)×P3} / {X1(mg)×R1+X2(mg)×R2+X3(mg)×R3}].It should be noted that the content of polyvinyl acetal resin (R1) and the content of plasticizer (P1) in the first layer are determined by GC measurement using the following method. 0.05 g of the peeled film is accurately weighed and dissolved in 4 ml of a mixed solution of methanol and chloroform in a weight ratio of 1:1. 0.1 ml of the mixed solution is diluted with 1.9 ml of a 1:1 mixed solution of methanol / chloroform. The diluted solution is filtered through a 0.2 μm syringe filter to prepare a solution for GC measurement. The GC measurement conditions are set as follows. The injection temperature is 280°C, and the chromatographic column used is HP-5 (. Agilent Technologies), the column temperature was set as follows: maintain at 80°C for 1 minute, then increase the temperature at 20°C / min, and maintain at 320°C for 30 seconds. The carrier gas was helium, the flow rate was 2.0ml / min, and the split ratio was 1:10. The injection volume of the sample solution was 2μl, the detector used a hydrogen flame ionization detector (FID), and the temperature of the detector was 320°C. Using the standard curve of the plasticizer prepared in advance on the same day, the content of the plasticizer in the sample solution was calculated (P1). In addition, the content of the polyvinyl alcohol acetal resin (R1) was calculated by 1-P1. The content of other additives contained in the intermediate film is also included in R1, but it can be ignored because it is extremely trace. Similarly, the second and third layers are measured.

[0242] (2) Bending rigidity

[0243] The obtained laminated glass A was used. Figure 3 The test method schematically shown measures the bending rigidity. As a measuring device, a universal material testing machine 5966 manufactured by Instron Japan Co., Ltd. with a static three-point bending test fixture 2810 is used. The measuring conditions are as follows: the measuring temperature is 20±3°C, the distance D1 is 18cm, the distance D2 is 25cm, the laminated glass is deformed in the F direction at a displacement speed of 1mm / min, the stress when a displacement of 1.5mm is applied is measured, and the bending rigidity is calculated. It should be noted that the bending rigidity is measured as follows: the bending rigidity δ(1D) of the laminated glass after 1 day after manufacturing and the bending rigidity δ(3M) of the laminated glass after being stored at 20°C for 3 months after manufacturing.

[0244] (3) Sound insulation

[0245] Vibration was applied to the laminated glass B using a vibration generator for a shock absorption experiment ("Exciter G21-0050D" manufactured by Zhenkensha), the vibration characteristics obtained were amplified using a mechanical impedance measuring device ("XG-81" manufactured by RION Corporation), and the vibration spectrum was analyzed using an FFT spectrum analyzer ("FFT Analyzer" HP3582A manufactured by Yokogawa Hewlett-Packard Company).

[0246] A graph showing the relationship between the sound frequency (Hz) and the sound transmission loss (dB) at 20°C was prepared from the loss coefficient thus obtained and the ratio of the resonant frequency of the laminated glass, and the minimum sound transmission loss (TL value) near the sound frequency of 2000 Hz was obtained. The higher the TL value, the better the sound insulation. The sound insulation was evaluated according to the following criteria.

[0247] [Sound insulation criteria]

[0248] ○: TL value is above 35dB;

[0249] ×: TL value is less than 35dB.

[0250] The details and results are shown in the following Tables 1 and 2. In addition, in the following Tables 1 and 2, the contents of the added components other than the polyvinyl acetal resin and the plasticizer are omitted.

[0251]

[0252]

Claims

1. An interlayer film for laminated glass, which has a structure of three or more layers and contains a polyvinyl acetal resin and a plasticizer, and has: The first layer contains a polyvinyl acetal resin and a plasticizer, a second layer, which is laminated on the first surface of the first layer and contains a polyvinyl acetal resin and a plasticizer, a third layer, which is laminated on a second surface of the first layer opposite to the first surface and contains a polyvinyl acetal resin and a plasticizer, The hydroxyl content of the polyvinyl acetal resin in the first layer is lower than the hydroxyl content of the polyvinyl acetal resin in the second layer, and when the absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin in the second layer and the hydroxyl content of the polyvinyl acetal resin in the first layer is denoted as XA, the absolute value XA is 9 mol% or more and 11 mol% or less, The hydroxyl content of the polyvinyl acetal resin in the first layer is lower than the hydroxyl content of the polyvinyl acetal resin in the third layer, and when the absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin in the third layer and the hydroxyl content of the polyvinyl acetal resin in the first layer is denoted as XB, the absolute value XB is 9 mol% or more and 11 mol% or less, When the content of the plasticizer in the interlayer film for laminated glass relative to 100 parts by weight of the polyvinyl acetal resin in the interlayer film for laminated glass is denoted by Y, Satisfies: Y≤-1.68XA+56, and Y≤-1.68XB+56.

2. The interlayer film for laminated glass according to claim 1, in, The content of the plasticizer in the first layer relative to 100 parts by weight of the polyvinyl acetal resin in the first layer is greater than the content of the plasticizer in the second layer relative to 100 parts by weight of the polyvinyl acetal resin in the second layer.

3. The interlayer film for laminated glass according to claim 1 or 2, in, The content of the plasticizer in the first layer relative to 100 parts by weight of the polyvinyl acetal resin in the first layer is greater than the content of the plasticizer in the third layer relative to 100 parts by weight of the polyvinyl acetal resin in the third layer.

4. The interlayer film for laminated glass according to any one of claims 1 to 3, in, The hydroxyl content of the polyvinyl acetal resin in the second layer is 32 mol % or more.

5. The interlayer film for laminated glass according to any one of claims 1 to 4, in, The hydroxyl content of the polyvinyl acetal resin in the third layer is 32 mol % or more.

6. The interlayer film for laminated glass according to any one of claims 1 to 5, in, The absolute value XA is greater than 9.3 mol %.

7. The interlayer film for laminated glass according to any one of claims 1 to 6, in, The absolute value XB is greater than 9.3 mol %.

8. The interlayer film for laminated glass according to any one of claims 1 to 7, in, The content of the plasticizer in the first layer is 55 parts by weight or more and 100 parts by weight or less relative to 100 parts by weight of the polyvinyl acetal resin in the first layer.

9. The interlayer film for laminated glass according to any one of claims 1 to 8, in, The content of the plasticizer in the second layer relative to 100 parts by weight of the polyvinyl acetal resin in the second layer and the content of the plasticizer in the third layer relative to 100 parts by weight of the polyvinyl acetal resin in the third layer are 50 parts by weight or less.

10. The interlayer film for laminated glass according to any one of claims 1 to 9, in, The content Y of the plasticizer in the interlayer film for laminated glass is 25 parts by weight or more and 40 parts by weight or less relative to 100 parts by weight of the polyvinyl acetal resin in the interlayer film for laminated glass.

11. The interlayer film for laminated glass according to any one of claims 1 to 10, in, The polyvinyl acetal resin in the first layer is polyvinyl butyral resin, The polyvinyl acetal resin in the second layer is polyvinyl butyral resin, The polyvinyl acetal resin in the third layer is polyvinyl butyral resin. 12 . The interlayer film for laminated glass according to claim 1 , which is used to obtain laminated glass by using a first glass plate having a thickness of less than 2 mm and disposing the interlayer film for laminated glass between the first glass plate and a second glass plate.

13. A laminated glass comprising: The first laminated glass component, Second laminated glass component, The interlayer film for laminated glass according to any one of claims 1 to 11, The interlayer film for laminated glass is arranged between the first laminated glass component and the second laminated glass component.

14. The laminated glass according to claim 13, in, The first laminated glass component is a first glass plate, and the thickness of the first glass plate is less than 2 mm.

Citation Information

Patent Citations

  • Interlayer for laminated glass, and laminated glass

    CN102686531A

  • Intermediate film for laminated glass, laminated glass, and method of mounting laminated glass

    CN104428267A

  • Laminate having excellent sound insulation properties

    JP2015117141A