Metal nanoparticle confinement porous organic framework composite material and preparation method thereof
The preparation of metal nanoparticles through nanosecond pulse laser bombardment method and react with the porous organic frame precursor, solving the problem of uniform distribution of metal nanoparticles in POFs pores, improving catalytic activity and stability, simplifying the preparation process, and achieving high efficiency heterogeneous catalytic application.
Patent Information
- Application Number
- CN202411043462.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The application of existing porous organic framework materials in the field of heterogeneous catalysis is limited by the agglomeration and inactivation of metal nanoparticles, and the traditional synthesis methods are lengthy and uncontrollable, resulting in insufficient catalytic activity and stability.
The nanosecond pulsed laser bombardment method is used to prepare the colloidal liquid of metal nanoparticles, and it is ultrasonic dispersed with the porous organic frame precursor to form a reaction system, and it is left to react at a specific temperature to achieve uniform distribution of metal nanoparticles in the POFs pores. The use of surfactants and reducing agents is avoided.
The high-quality uniform distribution of metal nanoparticles in POFs channels is achieved, catalytic activity and stability is improved, the preparation process is simplified, the presence of impurities is avoided, and there are broad prospects for heterogeneous catalytic application.
Smart Images

Figure CN118978653A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of new material preparation, and in particular to a method for preparing a porous organic framework material. Background Art
[0002] Porous Organic Framework (POFs) is a kind of organic polymer material composed of light elements such as C, H, N and O. It has the advantages of large specific surface area, light weight and porosity, and adjustable topology and chemical structure, and has good application prospects in the field of heterogeneous catalysis. However, although POFs materials have good porous confinement characteristics, the lack of metal catalytic sites seriously limits their effective use in the field of heterogeneous catalysis.
[0003] Transition metal and rare earth metal nanoparticles have excellent catalytic activity due to their special electronic geometry and adjustable d-band center. They are widely used in the field of heterogeneous catalysis, and the catalytic activity of metals often has a significant "size effect". Generally speaking, the smaller the metal size, the stronger the catalytic activity, but the metal must be loaded on a carrier after being nanosized to catalyze heterogeneous reactions. However, since metal nanoparticles are prone to agglomeration and inactivation during the catalytic process, their catalytic stability is seriously affected. Therefore, breaking through the bottleneck of easy agglomeration and inactivation of metals after nano-sizing is the key to obtaining high-efficiency catalysts.
[0004] Encapsulating highly active metal nanoparticles into POFs can effectively alleviate the agglomeration and deactivation of metal catalysts. The "confinement effect" between POFs and metal nanoparticles can effectively inhibit the agglomeration and deactivation of metal nanoparticles while improving the metal activity, thereby achieving a simultaneous improvement in the catalytic activity and stability of the metal. However, most of the current synthesis methods are "post-adsorption-reduction" methods, which first use acetic acid to catalyze the Schiff base reaction to prepare POFs, then adsorb the metal salt solution onto the POFs carrier, and finally use sodium borohydride and other chemical reductions to obtain metal nanoparticle confined POFs composite materials. However, the synthesis steps of this method are lengthy and the reduction process is uncontrollable. On the one hand, the reducing agent involved in the preparation process may destroy the structure of the POFs carrier; on the other hand, the obtained "surface-loaded" composite materials usually face the problems of large and uneven metal size, low catalytic activity and low metal utilization. The above factors seriously restrict the application of metal nanoparticles and their POFs composite materials in heterogeneous catalysis. Summary of the invention
[0005] The purpose of the present invention is to avoid the shortcomings of the prior art and provide a metal nanoparticle confined porous organic framework composite material and a preparation method thereof, which can achieve uniform bulk distribution of metal nanoparticles in POFs pores, give full play to the activity of nano-metal and the pore mass transfer confinement characteristics of POFs materials, and take into account both the high activity and high stability of metal catalysts.
[0006] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing a metal nanoparticle confined porous organic framework composite material, comprising the following steps:
[0007] Step 1: Prepare a colloidal mother solution containing metal nanoparticles:
[0008] The wavelength is 355~1064nm and the laser flux is 0.1~2Jpulse -1 cm -2 Nanosecond pulse lasers are used to bombard a metal target placed in a 20-40 ml solvent for 1 to 20 minutes to obtain a metal nanoparticle solution containing 0.1 to 50 mg / mL of metal nanoparticles;
[0009] Next, use a flux of 0.1 to 2 J pulse -1 cm -2 The metal nanoparticle solution is irradiated with a nanosecond pulse laser for 5-10 minutes to obtain a colloidal mother solution containing metal nanoparticles;
[0010] Wherein, the solvent is one of n-butanol, ethanol, dimethyl sulfoxide, and N,N-dimethylformamide;
[0011] Step 2: Preparation of metal nanoparticle confined porous organic framework composite materials:
[0012] Ultrasonic dispersion of a porous organic framework precursor in 20-40 ml of a colloidal mother solution containing metal nanoparticles to form a porous organic framework reaction system;
[0013] The porous organic framework reaction system is placed at a temperature of 25 to 120° C. and allowed to react for 2 to 96 hours. After the reaction is completed, the precipitate is washed alternately with N,N-dimethylformamide and ethanol at least three times, the precipitated powder is collected, and vacuum dried at 80° C. for 10 to 14 hours to obtain a metal nanoparticle confined porous organic framework composite material.
[0014] Furthermore, the metal nanoparticles are at least one of Pt, Pd, Au, Ru, Cu, Ag, Ni, Co, V, Cr, In, Ga, Er, Sm or Gd.
[0015] Furthermore, the porous organic framework precursor includes an aldehyde precursor and an amine precursor, wherein the ratio of the total amount of aldehyde groups in the aldehyde precursor to the total amount of amino groups in the amine precursor is 1 / 1.
[0016] Furthermore, the aldehyde precursor is one of terephthalaldehyde, substituted terephthalaldehyde, isophthalic acid trimeraldehyde, biphenyl dicarboxaldehyde, substituted biphenyl dicarboxaldehyde, terphenyl dicarboxaldehyde, substituted terphenyl dicarboxaldehyde and trialdehyde phloroglucinol.
[0017] Furthermore, the amine precursor is one of p-phenylenediamine, substituted p-phenylenediamine, benzyl diamine, substituted benzyl dimethylamine, terphenyl dimethylamine, substituted terphenyl dimethylamine and 1,3,5-triaminobenzene.
[0018] Furthermore, the porous organic framework of the porous organic framework material obtained from the porous organic framework precursor is POF.
[0019] The present invention also provides a metal nanoparticle confined porous organic framework composite material prepared based on the above preparation method, which is metal nanoparticles uniformly confined in the pores of the porous organic framework material.
[0020] The beneficial effects of the present invention are:
[0021] (1) The metal nanoparticle confined POFs composite material prepared by the present invention has a distinct "bulk confinement effect" and does not contain any impurities such as surfactants and reducing agents; the metal has high dispersion, uniform size and is encapsulated into the POFs pores, which has great application prospects in the field of heterogeneous catalysis.
[0022] (2) The present invention can prepare metal particle confined POFs composite materials in a green, simple, efficient and universal manner, and the in-situ encapsulation strategy involved successfully achieves high-quality confinement of metal nanoparticles in POFs pores.
[0023] (3) The metal particle confined POFs composite material prepared by the present invention has obvious "bulk encapsulation confinement" characteristics and is expected to be widely used in heterogeneous catalysis. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a high-resolution transmission electron microscopy (HRTEM) image of the Pt nanoparticle confined POF composite material Pt@POF1 prepared in Experimental Example 1 of the present invention;
[0025] Figure 2 (a) is the X-ray photoelectron spectrum (XPS) of Pt@POF1 prepared in Experimental Example 1 of the present invention;
[0026] Figure 2 (b) is a Fourier transform infrared spectrum (ATR-FTIR) of Pt@POF1 prepared in Experimental Example 1 of the present invention and POF1 prepared in Comparative Example 1;
[0027] Figure 3Powder X-ray diffraction (PXRD) spectra of Pt@POF1 prepared in Experimental Example 1 of the present invention and POF1 prepared in Comparative Example 1. DETAILED DESCRIPTION
[0028] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0029] In order to achieve the above object, the present invention provides the following specific implementation methods:
[0030] Embodiment 1:
[0031] A method for preparing a metal nanoparticle confined porous organic framework composite material comprises the following steps:
[0032] Step 1: Prepare a colloidal mother solution containing metal nanoparticles:
[0033] The wavelength is 355~1064nm and the laser flux is 0.1~2Jpulse -1 cm -2 Nanosecond pulse lasers are used to bombard a metal target placed in a 20-40 ml solvent for 1 to 20 minutes to obtain a metal nanoparticle solution containing 0.1 to 50 mg / mL of metal nanoparticles;
[0034] Among them, the metal nanoparticles are at least one of Pt, Pd, Au, Ru, Cu, Ag, Ni, Co, V, Cr, In, Ga, Er, Sm or Gd.
[0035] The solvent is one of n-butanol, ethanol, dimethyl sulfoxide, and N,N-dimethylformamide;
[0036] Next, use a flux of 0.1 to 2 J pulse -1 cm -2 The metal nanoparticle solution is irradiated with a nanosecond pulse laser for 5-10 minutes to obtain a colloidal mother solution containing metal nanoparticles;
[0037] Step 2: Preparation of metal nanoparticle confined porous organic framework composite materials:
[0038] The porous organic framework precursor is ultrasonically dispersed in 20-40 ml of a colloidal mother liquor containing metal nanoparticles to form a porous organic framework reaction system; wherein the porous organic framework precursor includes an aldehyde precursor and an amine precursor, wherein the ratio of the total amount of aldehyde groups in the aldehyde precursor to the total amount of amino groups in the amine precursor is 1 / 1.
[0039] The aldehyde precursor is one of terephthalaldehyde, substituted terephthalaldehyde, isophthalic acid trimeraldehyde, biphenyl dicarboxaldehyde, substituted biphenyl dicarboxaldehyde, terphenyl dicarboxaldehyde, substituted terphenyl dicarboxaldehyde and trialdehyde phloroglucinol.
[0040] The amine precursor is one of p-phenylenediamine, substituted p-phenylenediamine, benzylenediamine, substituted benzylenediamine, terphenylenediamine, substituted terphenylenediamine and 1,3,5-triaminobenzene.
[0041] The porous organic framework of the porous organic framework material obtained from the porous organic framework precursor is POF.
[0042] The porous organic framework reaction system is placed at a temperature of 25 to 120° C. and allowed to react for 2 to 96 hours. After the reaction is completed, the precipitate is washed alternately with N,N-dimethylformamide and ethanol at least three times, the precipitated powder is collected, and vacuum dried at 80° C. for 10 to 14 hours to obtain a metal nanoparticle confined porous organic framework composite material.
[0043] In order to further illustrate the present invention, an experimental example is provided, in which the porous organic framework material obtained from the porous organic framework precursor is abbreviated as POFX, wherein X is used to distinguish POF synthesized from any combination of aldehyde and amine precursors, and X is equal to 1, 2, 3, etc.
[0044] In this embodiment, the metal nanoparticles are Pt, Pd, V or Ga, the amine precursor is p-phenylenediamine, the aldehyde precursor is trialdehyde phloroglucinol, and the synthesized POF is POF1.
[0045] Experimental Example 1: Preparation of Pt@POF1:
[0046] (1) The wavelength is 1064nm and the laser flux is 1.2Jpulse -1 cm -2 The Pt foil placed in 20 mL of dimethyl sulfoxide was bombarded with a nanosecond pulse laser for 10 min to obtain a dimethyl sulfoxide mother solution containing Pt nanoparticles; the obtained mother solution was subjected to a 1.4 J pulse -1 cm -2 The DMSO colloidal solution containing Pt nanoparticles was obtained by secondary bombardment of the laser for 10 min.
[0047] (2) 324.42 mg of p-phenylenediamine and 420.28 mg of trialdehyde pyroglutamic acid were directly added to 40 mL of dimethyl sulfoxide colloidal solution containing Pt nanoparticles, and the mixture was allowed to react at 40 °C for 2 h. The resulting precipitate was washed alternately with N,N-dimethylformamide and ethanol for three times, and the resulting powder was vacuum dried at 80 °C for 12 h to obtain a Pt nanoparticle-confined POF1 composite material.
[0048] Experimental Example 2:
[0049] Preparation of Pd@POF1:
[0050] (1) The wavelength is 1064nm and the laser flux is 1.0Jpulse -1 cm -2 The Pd foil placed in 20 mL of N,N-dimethylformamide was bombarded with a nanosecond pulse laser for 10 min to obtain an N,N-dimethylformamide mother liquor containing Pd nanoparticles; the obtained mother liquor was subjected to a 1.4 J pulse -1 cm -2 The N,N-dimethylformamide colloidal solution containing Pd nanoparticles was obtained by secondary bombardment of the laser for 10 min.
[0051] (2) 324.42 mg of p-phenylenediamine and 420.28 mg of trialdehyde pyrogallol were directly added to 40 mL of N,N-dimethylformamide colloidal solution containing Pd nanoparticles, and the solution was allowed to react at 40 °C for 2 h. The resulting precipitate was washed alternately with N,N-dimethylformamide and ethanol for three times, and the resulting powder was vacuum dried at 80 °C for 12 h to obtain a Pd nanoparticle-confined POF1 composite material.
[0052] Experimental Example 3:
[0053] Preparation of V@POF1:
[0054] (1) The wavelength is 1064nm and the laser flux is 1.2Jpulse -1 cm -2 The V foil in 20 mL of n-butanol was bombarded with a nanosecond pulse laser for 10 min to obtain a n-butanol mother liquor containing V nanoparticles. The obtained mother liquor was subjected to a 1.4 J pulse laser. -1 cm -2 After secondary bombardment of pulsed laser for 10 min, a n-butanol colloidal solution containing V nanoparticles was obtained;
[0055] (2) 324.42 mg of p-phenylenediamine and 420.28 mg of trialdehyde pyroglucin were ultrasonically dispersed in 40 mL of n-butanol colloidal solution containing V nanoparticles, and the solution was allowed to react at 40 °C for 2 h. The resulting precipitate was washed alternately with N,N-dimethylformamide and ethanol for three times, and the resulting powder was vacuum dried at 80 °C for 12 h to obtain a V nanoparticle-confined POF1 composite material.
[0056] Experimental Example 4:
[0057] Preparation of Ga@POF1:
[0058] (1) The wavelength is 1064nm and the laser flux is 1.0Jpulse-1 cm -2 The Ga foil in 20 mL of n-butanol was bombarded with a nanosecond pulse laser for 2 min to obtain a n-butanol mother liquor containing Ga nanoparticles. The obtained mother liquor was subjected to a 1.4 J pulse laser. -1 cm -2 After secondary bombardment of pulsed laser for 10 min, a n-butanol colloidal solution containing Ga nanoparticles was obtained;
[0059] (2) 324.42 mg of p-phenylenediamine and 420.28 mg of trialdehyde pyroglutamic acid were ultrasonically dispersed in 40 mL of n-butanol colloidal solution containing Ga nanoparticles, and the mixture was allowed to react at 40 °C for 2 h. The resulting precipitate was washed alternately with N,N-dimethylformamide and ethanol for three times, and the resulting powder was vacuum dried at 80 °C for 12 h to obtain a Ga nanoparticle-confined POF1 composite material.
[0060] Embodiment 2: Same as Embodiment 1, except that:
[0061] The metal nanoparticles are Cr or Ni, the amine precursor is p-phenylenediamine, the aldehyde precursor is isophthalaldehyde, and the synthesized POF is POF2.
[0062] In order to further illustrate Example 2, the following specific experimental examples 5-6 are provided:
[0063] Experimental Example 5:
[0064] Preparation of Cr@POF2:
[0065] (1) The wavelength is 1064nm and the laser flux is 0.5Jpulse -1 cm -2 The Cr foil in 20 mL of n-butanol was bombarded with a nanosecond pulse laser for 2 min to obtain a n-butanol mother liquor containing Cr nanoparticles. The obtained mother liquor was subjected to a 1.4 J pulse laser. -1 cm -2 After secondary bombardment of pulsed laser for 10 min, a n-butanol colloidal solution containing Cr nanoparticles was obtained;
[0066] (2) 324.42 mg of p-phenylenediamine and 324.28 mg of isophthalic acid were ultrasonically dispersed in 40 mL of n-butanol colloidal solution containing Cr nanoparticles, and the mixture was allowed to react at 40 °C for 2 h. The resulting precipitate was washed alternately with N,N-dimethylformamide and ethanol for three times, and the resulting powder was vacuum dried at 80 °C for 12 h to obtain a Cr nanoparticle-confined POF2 composite material.
[0067] Experimental Example 6:
[0068] Preparation of Ni@POF2:
[0069] (1) The wavelength is 1064nm and the laser flux is 0.5Jpulse -1 cm -2 The Ni foil in 20 mL of dimethyl sulfoxide was bombarded with a nanosecond pulse laser for 2 min to obtain a dimethyl sulfoxide mother solution containing Ni nanoparticles. The obtained mother solution was subjected to a 1.4 J pulse laser. -1 cm -2 The DMSO colloidal solution containing Ni nanoparticles was obtained by secondary bombardment of the laser for 10 min.
[0070] (2) 324.42 mg of p-phenylenediamine and 324.28 mg of isophthalic acid were ultrasonically dispersed in 40 mL of dimethyl sulfoxide colloidal solution containing Ni nanoparticles, and the solution was allowed to react at 40 °C for 2 h. The resulting precipitate was washed alternately with N,N-dimethylformamide and ethanol for three times, and the resulting powder was vacuum dried at 80 °C for 12 h to obtain a Ni nanoparticle-confined POF2 composite material.
[0071] Embodiment 3: Same as Embodiment 1, except that:
[0072] The metal nanoparticles are Au or Ru, the amine precursor is p-phenylenediamine dichloride, the aldehyde precursor is trimesic acid, and the synthesized POF is POF3. In order to further illustrate Example 3, the following specific experimental examples 7-8 are provided:
[0073] Experimental Example 7:
[0074] Preparation of Au@POF3:
[0075] (1) The wavelength is 1064nm and the laser flux is 1.0Jpulse -1 cm -2 The Au foil in 20 mL of dimethyl sulfoxide was bombarded with a nanosecond pulse laser for 2 min to obtain a dimethyl sulfoxide mother liquor containing Au nanoparticles. The obtained mother liquor was subjected to a 1.4 J pulse laser. -1 cm -2 The pulsed laser was used for secondary bombardment for 10 min to obtain a dimethyl sulfoxide colloidal solution containing Au nanoparticles.
[0076] (2) 531.09 mg of dichloro-p-phenylenediamine and 324.28 mg of isophthalic acid were ultrasonically dispersed in 40 mL of dimethyl sulfoxide colloidal solution containing Au nanoparticles, and the solution was allowed to react at 40 °C for 2 h. The resulting precipitate was washed alternately with N,N-dimethylformamide and ethanol for three times, and the resulting powder was vacuum dried at 80 °C for 12 h to obtain an Au nanoparticle-confined POF3 composite material.
[0077] Experimental Example 8:
[0078] Preparation of Ru@POF3:
[0079] (1) The wavelength is 1064nm and the laser flux is 1.6Jpulse -1 cm -2 The Ru foil in 20 mL of dimethyl sulfoxide was bombarded with a nanosecond pulse laser for 2 min to obtain a dimethyl sulfoxide mother solution containing Ru nanoparticles; the obtained mother solution was subjected to a 1.4 J pulse -1 cm -2 The Ru nanoparticles were then bombarded for 10 min by a pulsed laser to obtain a dimethyl sulfoxide colloidal solution.
[0080] (2) 531.09 mg of dichloro-p-phenylenediamine and 324.28 mg of isophthalic acid were ultrasonically dispersed in 40 mL of dimethyl sulfoxide colloidal solution containing Ru nanoparticles, and the solution was allowed to react at 40 °C for 2 h. The resulting precipitate was then washed alternately with N,N-dimethylformamide and ethanol for three times, and the resulting powder was vacuum dried at 80 °C for 12 h to obtain a Ru nanoparticle-confined POF3 composite material.
[0081] Embodiment 4: Same as Embodiment 1, except that:
[0082] The metal nanoparticles are Ag, Er, Gd or Sm, the amine precursor is diphenyl diamine, the aldehyde precursor is isophthalic acid aldehyde, and the synthesized POF is POF4.
[0083] In order to further illustrate Example 4, the following specific experimental examples 9-12 are provided:
[0084] Experimental Example 9:
[0085] Preparation of Ag@POF4:
[0086] (1) The wavelength is 1064nm and the laser flux is 0.5Jpulse -1 cm -2 The Ag foil in 20 mL of dimethyl sulfoxide was bombarded with a nanosecond pulse laser for 2 min to obtain a dimethyl sulfoxide mother liquor containing Ag nanoparticles. The obtained mother liquor was subjected to a 1.4 J pulse laser. -1 cm -2 The pulsed laser was used for secondary bombardment for 10 min to obtain a dimethyl sulfoxide colloidal solution containing Ag nanoparticles.
[0087] (2) 324.72 mg of benzyl diamine and 324.28 mg of isophthalic acid were ultrasonically dispersed in 40 mL of dimethyl sulfoxide colloidal solution containing Ag nanoparticles, and the mixture was allowed to react at 40 °C for 2 h. The resulting precipitate was then washed alternately with N,N-dimethylformamide and ethanol for three times, and the resulting powder was vacuum dried at 80 °C for 12 h to obtain a Ag nanoparticle-confined POF4 composite material.
[0088] Experimental Example 10:
[0089] Preparation of Er@POF4:
[0090] (1) The wavelength is 1064nm and the laser flux is 0.5Jpulse -1 cm -2 The Er foil placed in 20 mL of dimethyl sulfoxide was bombarded with a nanosecond pulse laser for 2 min to obtain a dimethyl sulfoxide mother solution containing Er nanoparticles; the obtained mother solution was subjected to a 1.4 J pulse -1 cm -2 The pulsed laser was used for secondary bombardment for 10 min to obtain a dimethyl sulfoxide colloidal solution containing Er nanoparticles;
[0091] (2) 324.72 mg of benzyl diamine and 324.28 mg of isophthalic acid were ultrasonically dispersed in 40 mL of dimethyl sulfoxide colloidal solution containing Er nanoparticles, and the mixture was allowed to react at 40 °C for 2 h. The resulting precipitate was then washed alternately with N,N-dimethylformamide and ethanol for three times, and the resulting powder was vacuum dried at 80 °C for 12 h to obtain an Er nanoparticle-confined POF4 composite material.
[0092] Experimental Example 11:
[0093] Preparation of Gd@POF4:
[0094] (1) The wavelength is 1064nm and the laser flux is 0.5Jpulse -1 cm -2 The Gd foil in 20 mL of dimethyl sulfoxide was bombarded with a nanosecond pulse laser for 2 min to obtain a dimethyl sulfoxide mother solution containing Gd nanoparticles; the obtained mother solution was subjected to a 1.4 J pulse -1 cm -2 The pulsed laser was used for secondary bombardment for 10 min to obtain a dimethyl sulfoxide colloidal solution containing Gd nanoparticles;
[0095] (2) 324.72 mg of benzyl diamine and 324.28 mg of isophthalic acid were ultrasonically dispersed in 40 mL of dimethyl sulfoxide colloidal solution containing Gd nanoparticles, and the mixture was allowed to react at 40 °C for 2 h. The resulting precipitate was then washed alternately with N,N-dimethylformamide and ethanol for three times, and the resulting powder was vacuum dried at 80 °C for 12 h to obtain a Gd nanoparticle-confined POF4 composite material.
[0096] Experimental Example 12:
[0097] Preparation of Sm@POF4:
[0098] (1) The wavelength is 1064nm and the laser flux is 0.5Jpulse -1 cm -2 The Sm foil placed in 20 mL of dimethyl sulfoxide was bombarded with a nanosecond pulse laser for 2 min to obtain a dimethyl sulfoxide mother solution containing Sm nanoparticles; the obtained mother solution was subjected to a 1.4 J pulse -1 cm -2 The DMSO colloidal solution containing Sm nanoparticles was obtained by secondary bombardment of the solution with a pulsed laser for 10 min.
[0099] (2) 324.72 mg of benzyl diamine and 324.28 mg of isophthalic acid were ultrasonically dispersed in 40 mL of dimethyl sulfoxide colloidal solution containing Sm nanoparticles, and the mixture was allowed to react at 40 °C for 2 h. The resulting precipitate was then washed alternately with N,N-dimethylformamide and ethanol for three times, and the resulting powder was vacuum dried at 80 °C for 12 h to obtain a Sm nanoparticle-confined POF4 composite material.
[0100] In order to reflect the technical effect of the present invention, the present invention also provides the following comparative examples for comparison and explanation with the present invention:
[0101] Comparative Example 1: Preparation of pure POF1,
[0102] 324.42 mg of p-phenylenediamine and 420.28 mg of trialdehyde pyrogallol were added to 40 mL of dimethyl sulfoxide, followed by 10 mL of 6 M glacial acetic acid. The reaction was allowed to stand at 40 °C for 12 h. The resulting precipitate was washed alternately with N,N-dimethylformamide and ethanol for three times, and vacuum dried at 80 °C for 12 h to obtain POF1 material.
[0103] Comparative Example 2: Preparation of pure POF2,
[0104] 324.42 mg of p-phenylenediamine and 324.28 mg of isophthalic acid were added to 40 mL of dimethyl sulfoxide, followed by 10 mL of 6 M glacial acetic acid. The mixture was allowed to react at 40 °C for 12 h. The precipitate was washed alternately with N,N-dimethylformamide and ethanol for three times, and dried in vacuo at 80 °C for 12 h to obtain POF2 material.
[0105] Comparative Example 3: Preparation of pure POF3,
[0106] 531.09 mg of dichloro-p-phenylenediamine and 324.28 mg of isophthalic acid were added to 40 mL of dimethyl sulfoxide, followed by 10 mL of 6 M glacial acetic acid. The mixture was allowed to react at 40 °C for 12 h. The precipitate was washed alternately with N,N-dimethylformamide and ethanol for three times, and dried in vacuo at 80 °C for 12 h to obtain POF3 material.
[0107] Comparative Example 4: Preparation of pure POF4,
[0108] 324.72 mg of benzyl diamine and 324.28 mg of isophthalic acid were added to 40 mL of dimethyl sulfoxide, followed by 10 mL of 6 M glacial acetic acid. The mixture was allowed to react at 40 °C for 12 h. The precipitate was washed alternately with N,N-dimethylformamide and ethanol for three times, and dried in vacuo at 80 °C for 12 h to obtain POF4 material.
[0109] Example 5: Figure 1-3 As shown, the present invention also provides a metal nanoparticle confined porous organic framework composite material prepared based on the above preparation method, which is metal nanoparticles uniformly confined in the pores of the porous organic framework material.
[0110] Figure 1 This is a high-resolution transmission electron microscopy (HRTEM) image of the Pt nanoparticle-confined POF1 composite material (Pt@POF1) prepared in Experimental Example 1. Figure 1 It can be seen that the Pt@POF1 composite material synthesized in the present invention does not contain uneven large Pt particles, and the Pt species are evenly distributed, and the size is almost about 2 nm.
[0111] Figure 2 (a) is the X-ray photoelectron spectroscopy (XPS) of Pt@POF1 prepared in Experimental Example 1. Figure 2 (b) is the Fourier transform infrared spectrum (ATR-FTIR) of Pt@POF1 prepared in Example 1 and POF1 prepared in Comparative Example 1. Figure 2 (a) It can be seen that the valence state of Pt in the Pt@POF1 composite material prepared by the present invention is +2; Figure 2 (b) It can be seen that the 1624 cm-1 There is obvious vibration absorption of the imine bond at the position, which proves that the aldehyde and amine precursors are polymerized into imine POF1 without any catalyst.
[0112] Figure 3 The X-ray powder diffraction (XRD) spectra of Pt@POF1 prepared in Experimental Example 1 and Comparative Example 1 and POF1 prepared in Comparative Example 1 show that the method for preparing a POF material by in-situ implantation of metal nanoparticles provided by the present invention has no effect on the crystallinity of POF, and the obtained nanoparticle confined POF composite material has excellent crystallinity and ordered structure.
[0113] In summary, the metal nanoparticle confined POFs material prepared by the present invention has high purity, does not contain impurity ions, has good crystallinity, and the nanoparticles are highly evenly distributed in the POFs pores, which may have the advantages of taking into account both catalytic activity and stability in heterogeneous catalysis. In addition, the preparation method provided by the present invention is simple, universal and easy to implement, and has good potential application prospects in the field of heterogeneous catalysis.
[0114] The above description is only a preferred experimental example of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a metal nanoparticle confined porous organic framework composite material, characterized in that: The following steps are involved: Step 1: Prepare a colloidal mother solution containing metal nanoparticles: The wavelength is 355~1064nm and the laser flux is 0.1~2Jpulse -1 cm -2 Nanosecond pulse lasers are used to bombard a metal target placed in a 20-40 ml solvent for 1 to 20 minutes to obtain a metal nanoparticle solution containing 0.1 to 50 mg / mL of metal nanoparticles; Next, use a flux of 0.1 to 2 J pulse -1 cm -2 The metal nanoparticle solution is irradiated with a nanosecond pulse laser for 5-10 minutes to obtain a colloidal mother solution containing metal nanoparticles; Wherein, the solvent is one of n-butanol, ethanol, dimethyl sulfoxide, and N,N-dimethylformamide; Step 2: Preparation of metal nanoparticle confined porous organic framework composite materials: Ultrasonic dispersion of a porous organic framework precursor in 20-40 ml of a colloidal mother solution containing metal nanoparticles to form a porous organic framework reaction system; The porous organic framework reaction system is placed at a temperature of 25 to 120° C. and allowed to react for 2 to 96 hours. After the reaction is completed, the precipitate is washed alternately with N,N-dimethylformamide and ethanol at least three times, the precipitated powder is collected, and vacuum dried at 80° C. for 10 to 14 hours to obtain a metal nanoparticle confined porous organic framework composite material.
2. The method for preparing the metal nanoparticle confined porous organic framework composite material according to claim 1, characterized in that: The metal nanoparticles are at least one of Pt, Pd, Au, Ru, Cu, Ag, Ni, Co, V, Cr, In, Ga, Er, Sm or Gd.
3. The method for preparing the metal nanoparticle confined porous organic framework composite material according to claim 1, characterized in that: The porous organic framework precursor comprises an aldehyde precursor and an amine precursor, wherein the ratio of the total amount of aldehyde groups in the aldehyde precursor to the total amount of amino groups in the amine precursor is 1 / 1.
4. The method for preparing the metal nanoparticle confined porous organic framework composite material as claimed in claim 3, characterized in that: The aldehyde precursor is one of terephthalaldehyde, substituted terephthalaldehyde, isophthalic acid trimaldehyde, biphenyl dicarboxaldehyde, substituted biphenyl dicarboxaldehyde, terphenyl dicarboxaldehyde, substituted terphenyl dicarboxaldehyde and trialdehyde phloroglucinol.
5. The method for preparing the metal nanoparticle confined porous organic framework composite material as claimed in claim 3, characterized in that: The amine precursor is one of p-phenylenediamine, substituted p-phenylenediamine, benzyl diamine, substituted benzyl dimethylamine, terphenyl dimethylamine, substituted terphenyl dimethylamine and 1,3,5-triaminobenzene.
6. The method for preparing the metal nanoparticle confined porous organic framework composite material according to any one of claims 1 to 5, characterized in that: The porous organic framework of the porous organic framework material obtained from the porous organic framework precursor is POF.
7. A metal nanoparticle confined porous organic framework composite material prepared by the preparation method according to claims 1-5, characterized in that: Metal nanoparticles uniformly confined in the pores of porous organic framework materials.
Citation Information
Patent Citations
Gold@metal organic frame material nano-particle array and preparation method and application thereof
CN105750537A
Porous organic framework material as well as preparation method and application thereof
CN113105626A
Titanium-based nano composite material for microwave thermal diagnosis and treatment integration as well as preparation method and application of titanium-based nano composite material
CN115850626A
Metal nanoparticle confinement covalent organic framework material and preparation method thereof
CN118388791A
System and method for continuous wave low power laser based synthesis of metal NANO particles
IN201941029216A