Preparation method and application of iron-based polymer molecular catalyst

By preparing iron-based fog molecular catalysts with non-planar, large steric hindrance, high conjugation and rigid geometric structures, the problem of insufficient activity, selectivity and stability of existing CO2 electrocatalytic reduction catalysts is solved, and the high-efficiency depth of CO2 is achieved The effect of reducing to methanol provides a more environmentally friendly and sustainable way to utilize CO2 resources.

CN118978671AActive Publication Date: 2024-11-19NANJING UNIV OF POSTS & TELECOMM
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411062967.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

The existing CO2 electrocatalytic reduction catalysts have shortcomings in terms of activity, selectivity and stability, especially in the difficulty in efficiently reducing CO2 to methanol.

Method used

Using iron-based polyglass (FePAG) catalyst, through specific chemical structures and synthesis steps, 3,6-dibromocarbazole, bromine ethane, sodium hydroxide and tetrabutyl ammonium bromide are reacted to form substances such as Iron-based polygrid molecules with non-planar, large steric hindrance, high conjugation and rigid geometric structures are used for electrochemical reduction of CO2.

Benefits of technology

It achieves efficient and stable reduction of CO2 to methanol, improves the activity, selectivity and stability of the catalyst, and provides a more environmentally friendly and sustainable way to utilize CO2.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978671A_ABST
    Figure CN118978671A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of an iron-based polymeric molecular catalyst, and belongs to the technical field of catalysis, and the iron-based polymeric molecular catalyst has the characteristics of non-plane, large steric hindrance and high conjugation, and can reduce CO2 into methanol with high activity, high selectivity and high stability. The problems that a traditional catalyst is poor in activity, selectivity and stability in the aspect of reducing CO2 into methanol are solved. The catalyst not only can effectively catalyze the conversion and utilization of CO2 and relieve the greenhouse effect, but also can provide a more environment-friendly and sustainable way for the traditional methanol production, and provides an efficient method for the resource utilization of CO2.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysis, and in particular relates to a preparation method and application of an iron-based polylattice molecule (FePAG) catalyst. Background Art

[0002] Human activities continue to increase carbon dioxide (CO2) emissions, causing an increase in CO2 concentrations in the atmosphere, which in turn triggers the greenhouse effect, leading to global climate change and environmental problems. To meet this challenge, the use of renewable energy for CO2 electrocatalytic reduction to produce fuels and high-value-added chemicals has been considered a sustainable and zero-emission carbon cycle solution. However, the inherent chemical inertness of CO2 and the competitive hydrogen evolution reaction (HER) limit the realization of efficient CO2 conversion and high product selectivity. Therefore, researchers have been committed to developing highly active, highly selective and highly stable electrocatalysts.

[0003] At present, the main catalysts for CO2 electrocatalytic reduction include metal alloy catalysts, metal oxide catalysts, single atom catalysts, metal-organic complex catalysts, molecular catalysts, etc. Among them, molecular catalysts, such as metalloporphyrins and metal phthalocyanines, have attracted much attention because they can adjust the primary and secondary coordination spheres by manipulating the coordination environment and the stereo and electronic effects of the ligands to adjust the catalytic efficiency and product selectivity. Integrating molecular catalysts into covalent organic polymers is another strategy for designing efficient CO2 reduction electrocatalysts. In this approach, molecular catalysts exist as uniformly dispersed active sites in the covalent organic polymer framework. At the same time, by controlling the adjacent functional groups in the framework, the electronic structure of the active site can be adjusted, providing an opportunity to regulate the intrinsic catalytic properties of the catalyst. At present, although cobalt-based molecular catalysts and their combination with covalent organic polymers have been widely studied, the main product is still carbon monoxide, and there are few reports on the generation of deep reduction products such as methanol. Therefore, the development of catalysts for efficient deep reduction of CO2 remains one of the important topics of current research.

[0004] The present invention integrates unit A-type lattice molecules into an organic polymer to prepare an iron-based polylattice molecule (FePAG) catalyst, which can efficiently and stably reduce CO2 to methanol. Summary of the invention

[0005] Purpose of the invention: In order to reduce CO2 to methanol, the present invention provides a preparation method and application of an iron-based polylattice molecule (FePAG) catalyst. Based on the unique chemical structure of the molecular catalyst, the iron-based polylattice molecule (FePAG) catalyst prepared by the present invention can reduce CO2 to methanol with high activity, high selectivity and high stability, providing theoretical and technical guidance for promoting CO2 emission reduction and resource utilization.

[0006] Technical content: An iron-based polymerized molecular catalyst, the general structure of which is as follows:

[0007]

[0008] A method for preparing an iron-based polymerized molecular catalyst comprises the following steps:

[0009] Step 1: Add 3,6-dibromocarbazole, ethyl bromide, sodium hydroxide and tetrabutylammonium bromide into a three-necked flask, then add acetone, and stir in an oil bath at 60-70° C. for 1.5-3 hours to obtain 3,6-dibromoethylcarbazole;

[0010] Step 2: Put 3,6-dibromoethylcarbazole, biphenylphosphinoyl ferrocene and potassium acetate into a sealed flask, evacuate and blow nitrogen, and inject [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride and dry 1,4-dioxane into the flask under nitrogen protection, respectively, and react at 100-110° C. for 8-15 hours to obtain 9-ethyl-3,6-bis(4,4,5,5-tetramethyl-1,3,2-dioxaborolane-2-yl)-9H-carbazole;

[0011] Step 3, preparing 2,7-dibromo-9-(4-(octyloxy)phenyl)-9H-fluoren-9-ol;

[0012] Step 3.1, add Mg chips into a flask, and then add iodine particles; seal the flask, evacuate and purify with nitrogen, and slowly inject 1-bromo-4-(octyloxy)benzene and tetrahydrofuran into the flask in batches under nitrogen protection, and after the injection, reflux at 70-90° C. for 3-6 hours to obtain the Grignard reagent;

[0013] Step 3.2, then under nitrogen protection, add the prepared Grignard reagent dropwise into a reaction bottle containing 2,7-dibromofluorenone and tetrahydrofuran, and ensure that the temperature in the reaction bottle is in the range of 0 to 10° C.; after the dropwise addition is completed, reflux at 80 to 90° C. for 5 to 8 hours to obtain 2,7-dibromo-9-(4-(octyloxy)phenyl)-9H-fluoren-9-ol;

[0014] Step 4: Add 9-ethyl-3,6-bis(4,4,5,5-tetramethyl-1,3,2-dioxaborolane-2-yl)-9H-carbazole, 2,7-dibromo-9-(4-(octyloxy)phenyl)-9H-fluorene-9-ol and Pd(PPh3)4 catalyst into a three-necked flask; then, evacuate and replace the reaction system with nitrogen several times to ensure an oxygen-free environment; add a mixture of toluene and tetrahydrofuran bubbled with nitrogen and a K2CO3 / KF aqueous solution into the flask through a syringe; seal the reaction system and connect a nitrogen balloon, and stir the reaction in an oil bath at 90-100°C for 1.5-3 hours to obtain the synthon BOH;

[0015] Step 5, 4-methyl-N,N-diphenylaniline is placed in a reaction bottle, dichloromethane is added to dissolve to obtain a 4-methyl-N,N-diphenylaniline solution, and then BF3·Et2O is added thereto; BOH is dissolved in dichloromethane to obtain a BOH solution, and the BOH solution is placed in a constant pressure dropping funnel; the BOH solution is slowly added dropwise to the reaction bottle at room temperature, and stirring is continued for 5 to 10 minutes after the addition is completed to obtain compound BG;

[0016] Step 6: In a light-proof nitrogen environment in a glove box, add BG and toluene to a flask to obtain a BG solution; add bipyridine and bis(1,5-cyclooctadiene) nickel to a dry reaction tube in a light-proof nitrogen environment in a glove box, seal the tube, and gradually add 1,5-cyclooctadiene and N,N-dimethylformamide to the reaction tube with a syringe; preheat the reaction tube in a 65-75°C oil bath for 20-40 minutes, and then add the BG solution to the reaction tube in a nitrogen environment; then heat the oil bath to 80-90°C and stir to react for 4-6 days, then add a capping agent, bromobenzene, to cap the tube, and continue to react for 1-2 days to obtain a polylattice molecule PAG;

[0017] Step 7: Add the polylattice molecule PAG into a flask, followed by dichloromethane; then add the ethanol solution of FeCl3 into the flask; stir the reaction mixture at room temperature for 10 to 15 hours to obtain the iron-based polylattice molecule FePAG.

[0018] Further, in step 1, the molar ratio of ethyl bromide to 3,6-dibromocarbazole is 1:1 to 1.5:1; the molar ratio of sodium hydroxide to 3,6-dibromocarbazole is 1:2 to 1.5:1; the molar ratio of tetrabutylammonium bromide to 3,6-dibromocarbazole is 1:20 to 1:5; acetone is used as a solvent, and the concentration of 3,6-dibromocarbazole is 0.1 to 0.3M;

[0019] In step 2, the molar ratio of pinacol diboron to 3,6-dibromoethylcarbazole is 2:1-5:1; the molar ratio of potassium acetate to 3,6-dibromoethylcarbazole is 3:1-5:1; the molar ratio of [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride to 3,6-dibromoethylcarbazole is 1:20-3:20; 1,4-dioxane is used as a solvent, and the concentration of 3,6-dibromoethylcarbazole is 0.15-0.3M;

[0020] In step 3.1, the molar ratio of Mg turnings to 1-bromo-4-(octyloxy)benzene is 1:2 to 1:1; the molar ratio of I2 to 1-bromo-4-(octyloxy)benzene is 1:210 to 1:52.5; tetrahydrofuran is used as a solvent, and the concentration of 1-bromo-4-(octyloxy)benzene is 1 to 3M;

[0021] In step 3.2, the molar ratio of 2,7-dibromofluorenone to 1-bromo-4-(octyloxy)benzene in step 3.1 is 1:4 to 1:2; tetrahydrofuran is used as a solvent, and the concentration of 2,7-dibromofluorenone is 0.25 to 0.6 M;

[0022] In step 4, the molar ratio of 2,7-dibromo-9-(4-(octyloxy)phenyl)-9H-fluorene-9-ol and 9-ethyl-3,6-bis(4,4,5,5-tetramethyl-1,3,2-dioxaborolane-2-yl)-9H-carbazole is 2:1 to 4:1; the molar ratio of Pd(PPh3)4 and 9-ethyl-3,6-bis(4,4,5,5-tetramethyl-1,3,2-dioxaborolane-2-yl)-9H-carbazole is 1:7 to 1:3; the molar ratio of K2CO3 and 9-ethyl-3,6-bis(4,4,5 The molar ratio of KF to 9-ethyl-3,6-bis(4,4,5,5-tetramethyl-1,3,2-dioxaborolane-2-yl)-9H-carbazole is 1:1 to 4:1; the molar ratio of KF to 9-ethyl-3,6-bis(4,4,5,5-tetramethyl-1,3,2-dioxaborolane-2-yl)-9H-carbazole is 1:1 to 4:1; the concentration of 9-ethyl-3,6-bis(4,4,5,5-tetramethyl-1,3,2-dioxaborolane-2-yl)-9H-carbazole is 0.15 to 0.3 M; the concentration of K2CO3 / KF aqueous solution is 1.5 to 3 M;

[0023] In step 5, the molar ratio of BF3·Et2O to BOH is 7:1 to 15:1; the molar ratio of 4-methyl-N,N-diphenylaniline to BOH is 1:1 to 1.5:1; the concentration of the 4-methyl-N,N-diphenylaniline solution is 1 to 4 mM; the concentration of the BOH solution is 1 to 4 mM;

[0024] In step six, the molar ratio of bipyridine to BG is 3:1 to 5:1; the molar ratio of bis(1,5-cyclooctadiene)nickel to BG is 3:1 to 5:1; the molar ratio of 1,5-cyclooctadiene to BG is 3:1 to 5:1; the volume ratio of N,N-dimethylformamide to toluene is 1:14 to 1:3; the volume ratio of bromobenzene to toluene is 1:15 to 1:5; the concentration of BG in toluene is 0.05 to 0.2 M;

[0025] In step seven, the mass ratio of FeCl3 to PAG is 1:5 to 1:2; the volume ratio of dichloromethane to ethanol is 1:1 to 2:1.

[0026] The iron-based polylattice molecules prepared by the present invention are used to prepare a working electrode, and the working electrode is used to reduce CO2 to methanol. The preparation steps of the working electrode are as follows:

[0027] Step (1), adding the iron-based polymer molecule FePAG to ethanol, then adding the Nafion solution, and ultrasonicating for 30 minutes to fully disperse it;

[0028] Step (2), taking 100 μL of the solution prepared in step (1) and evenly applying it on carbon paper, and then drying it naturally to obtain a working electrode of an H-type electrolytic cell;

[0029] Step (3), take 100 μL of the solution prepared in step (1) and evenly apply it on the Sigracet 29BC gas diffusion layer, and then dry it naturally to obtain the working electrode of the flow-type electrolytic cell.

[0030] Furthermore, in step (1), after the iron-based polymer molecule FePAG is added to ethanol, the amount of FePAG in the ethanol is 0.005-0.02 mg / μL; the concentration of the added Nafion solution is 5 wt.%, and the volume ratio of the Nafion solution to the ethanol is 1:20-1:5;

[0031] In step (2), 100 μL of the solution prepared in step (1) is evenly dropped on carbon paper;

[0032] In step (3), 100 μL of the solution prepared in step (1) is evenly drop-coated on the Sigracet 29BC gas diffusion layer. Compared with the prior art, the present invention has the following advantages:

[0033] 1) The iron-based polylattice molecule (FePAG) prepared by the present invention has non-planar, large steric hindrance, high conjugation and rigid geometric structure characteristics. The non-planar and large steric hindrance molecular structure can effectively inhibit the aggregation of molecules and is conducive to the high exposure of active sites; the highly conjugated molecular structure promotes the efficient transfer of electrons; and the rigid geometric structure is conducive to stabilizing the active sites.

[0034] 2) The iron-based polylattice molecule (FePAG) prepared by the present invention can efficiently and stably catalyze the electrochemical reduction of CO2 to produce methanol, solving the problems of poor activity, poor selectivity and poor stability of molecular electrocatalysts in the reduction of CO2 to methanol, and has better market application prospects.

[0035] 3) The iron-based polylattice molecular catalyst prepared by the present invention can not only effectively catalyze the conversion and utilization of CO2 and alleviate the greenhouse effect, but also provide a more environmentally friendly and sustainable way for traditional methanol production and an efficient method for the resource utilization of CO2. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 The Faraday efficiency distribution diagram of CO2 reduction products of the FePAG catalyst prepared in Example 1 at different potentials in an H-type electrolyzer;

[0037] Figure 2The selectivity test results of FePAG catalyst prepared in Example 1 for CO2 reduction to produce methanol in an H-type electrolyzer;

[0038] Figure 3 The test results of the CO2 reduction stability of the FePAG catalyst prepared in Example 1 in an H-type electrolyzer;

[0039] Figure 4 The production rate of methanol by reducing CO2 with the FePAG catalyst prepared in Example 1 at different potentials in an H-type electrolyzer;

[0040] Figure 5 The Faraday efficiency and current density distribution diagram of CO2 reduction product methanol at different potentials in a flow-type electrolyzer using the FePAG catalyst prepared in Example 1;

[0041] Figure 6 The synthetic route of the iron-based polylattice molecule (FePAG) in Example 1;

[0042] Figure 6 In the figure, the compounds represented by 1-9 are: 1 is 3,6-dibromocarbazole; 2 is ethyl bromide; 3 is 3,6-dibromoethylcarbazole; 4 is biphenylboronate; 5 is 9-ethyl-3,6-bis(4,4,5,5-tetramethyl-1,3,2-dioxaborolane-2-yl)-9H-carbazole; 6 is 1-bromo-4-(octyloxy)benzene; 7 is 2,7-dibromofluorenone; 8 is 2,7-dibromo-9-(4-(octyloxy)phenyl)-9H-fluoren-9-ol; 9 is 4-methyl-N,N-diphenylaniline; and 10 is ferric chloride. DETAILED DESCRIPTION

[0043] The technical solution of the present invention is described in detail below with reference to the accompanying drawings, but the protection scope of the present invention is not limited to the embodiments.

[0044] Example 1: Preparation of FePAG

[0045] like Figure 6 As shown, the preparation steps of the iron-based polylattice molecule (FePAG) disclosed in the present invention are as follows:

[0046] Step 1, 3,6-dibromocarbazole (15g, 46.2mmol), bromoethane (5g, 46.2mmol), sodium hydroxide (1.8g, 46.2mmol), tetrabutylammonium bromide (1.5g, 4.62mmol) and acetone (308mL) were added to a three-necked flask in sequence, and refluxed and stirred in an oil bath at 65°C for 2 hours. After the reaction, the organic phase was extracted with dichloromethane. Then it was dried with anhydrous sodium sulfate, filtered, and the solvent was evaporated under reduced pressure. The crude product was separated and purified by column chromatography with 200-300 mesh silica gel to obtain compound 3,6-dibromoethylcarbazole;

[0047] Step 2: Put 3,6-dibromoethylcarbazole (3 g, 8.5 mmol), biboric acid pinacol ester (6.5 g, 25.5 mmol) and potassium acetate (3.3 g, 34 mmol) into a flask, seal it, wrap it with tin foil, and evacuate and blow nitrogen for 3 times;

[0048] Then Pd(dppf)Cl2 ([1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride) (435 mg, 0.6 mmol) was added;

[0049] Subsequently, the device was evacuated and nitrogen-filled again; dry 1,4-dioxane (43 mL) was injected into the flask under nitrogen protection and reacted at 105°C for 12 hours. After the reaction, the organic phase was extracted with dichloromethane. Then it was dried with anhydrous sodium sulfate, filtered, and the solvent was evaporated under reduced pressure. The crude product was separated and purified by column chromatography using 200-300 mesh silica gel to obtain 9-ethyl-3,6-bis(4,4,5,5-tetramethyl-1,3,2-dioxaborolane-2-yl)-9H-carbazole;

[0050] Step 3, add Mg chips (3.4g, 140mmol) to the flask, and then add I2 (254mg, 1mmol). Seal the device and evacuate and fill with nitrogen. Under nitrogen protection, slowly inject 1-bromo-4-(octyloxy)benzene (30g, 105mmol) and tetrahydrofuran (52mL) into the flask in 5 batches, injecting 6g of 1-bromo-4-(octyloxy)benzene and about 10.4mL of tetrahydrofuran in each batch. After the injection is completed, reflux at 85℃ for 4h to obtain the Grignard reagent.

[0051] Then, under nitrogen protection, the prepared Grignard reagent is added dropwise to a reaction bottle containing 2,7-dibromofluorenone (11.9 g, 35 mmol) and tetrahydrofuran (75 mL), and the temperature in the reaction bottle is ensured to be in the range of 0 to 10 ° C. The entire dropwise addition process takes 20 to 50 minutes; after the dropwise addition is completed, the reaction is refluxed at 85 ° C for 6 hours. After the reaction is completed, the reaction is quenched with a saturated ammonium chloride solution, the tetrahydrofuran solvent is removed by rotary evaporation, and then a large amount of water is added to precipitate the solid, and the inorganic salt is removed by stirring. Filter and wash with a large amount of deionized water to obtain a crude product. The crude product is separated and purified by column chromatography using 200-300 mesh silica gel to obtain 2,7-dibromo-9-(4-(octyloxy)phenyl)-9H-fluoren-9-ol.

[0052] Step 4: Add 9-ethyl-3,6-bis(4,4,5,5-tetramethyl-1,3,2-dioxaborolane-2-yl)-9H-carbazole (3 g, 6.7 mmol), 2,7-dibromo-9-(4-(octyloxy)phenyl)-9H-fluorene-9-ol (11 g, 20.2 mmol) and Pd(PPh3)4 catalyst (1.5 g, 1.3 mmol) (protect from light) into a three-necked flask.

[0053] Subsequently, the reaction system was vacuumed and nitrogen replaced several times to ensure an oxygen-free environment; a nitrogen-bubbled toluene / tetrahydrofuran mixture (volume ratio 1:1, 20.2 mL) and a K2CO3 / KF aqueous solution (molar ratio 1:1, 2 M, 13.4 mL) were injected into the flask via a syringe.

[0054] The reaction system was sealed and connected to a nitrogen balloon, and the reaction was stirred in a 95°C oil bath for 2 hours. After the reaction was completed, the organic phase was extracted with dichloromethane. Then it was dried with anhydrous sodium sulfate, filtered, and the solvent was evaporated under reduced pressure. The crude product was separated and purified by column chromatography using 200-300 mesh silica gel to obtain the synthon BOH.

[0055] Step 5, 4-methyl-N, N-diphenylaniline (69.4mg, 0.268mmol) was placed in a reaction bottle, and dichloromethane (134mL) was added to dissolve. Then BF3·Et2O (401.7mg, 2.83mmol) was added thereto, and BOH (300mg, 0.268mmol) was dissolved in dichloromethane (134mL) and placed in a constant pressure dropping funnel. The BOH solution was slowly added dropwise to the reaction bottle for about 2 hours, and stirring was continued for 5 minutes after the addition was completed. After the reaction was completed, the organic phase was extracted with dichloromethane. Then it was dried over anhydrous sodium sulfate, filtered, and the solvent was evaporated under reduced pressure. The crude product was separated and purified by column chromatography with 200-300 mesh silica gel to obtain BG.

[0056] Step 6: Preparation of polylattice molecules (PAG):

[0057] 1) In a light-proof nitrogen environment in a glove box, add BG (148 mg, 0.11 mmol) and toluene (10 mL) into a flask to obtain a BG solution;

[0058] 2) Add bipyridine (69.3 mg, 0.44 mmol) and bis(1,5-cyclooctadiene)nickel (120.7 mg, 0.44 mmol) into a dry reaction tube in a light-proof nitrogen environment in a glove box. After sealing, gradually add 1,5-cyclooctadiene (0.6 mL, 0.44 mmol) and N,N-dimethylformamide (2 mL) into the reaction tube using a syringe;

[0059] 3) Preheat the reaction tube in a 70°C oil bath for half an hour, and then transfer the BG solution in the flask to the reaction tube under nitrogen atmosphere;

[0060] 4) The oil bath was then heated to 85°C and stirred for 5 days, after which bromobenzene (1 mL) was added for end-capping and the reaction was continued for 1 day. After the reaction was completed, a 10 cm cotton column filled with neutral alumina was used to press the column with THF to remove the Ni catalyst. The DMF was then repeatedly washed with methanol to remove the DMF, and the solid was subjected to Soxhlet extraction to obtain the polylattice molecule (PAG).

[0061] Step 7: Add PAG (100 mg) to the flask, followed by dichloromethane (50 mL). Then add FeCl3 (27.3 mg) in ethanol (25 mL) to the flask. Stir the reaction mixture at room temperature for 12 hours. After the reaction is complete, evaporate the solvent under reduced pressure; then, wash with deionized water and centrifuge to remove unreacted FeCl3 to obtain FePAG.

[0062] Example 2: Preparation of working electrode based on the iron-based polylattice molecule (FePAG) in Example 1

[0063] The preparation steps of the working electrode are as follows:

[0064] (1) Preparation of H-type electrolytic cell working electrode:

[0065] Step (1), adding the FePAG complex (2 mg) to ethanol (200 μL), followed by adding 5 wt.% Nafion solution (20 μL), and ultrasonicating for 30 minutes to fully disperse it;

[0066] Step (2): Take 100 μL of the solution prepared in step (1) and evenly apply it on a piece of carbon paper (1×1 square centimeter), and then dry it naturally.

[0067] (2) Preparation of working electrodes for flow-type electrolytic cells:

[0068] Step (1), adding the FePAG complex (2 mg) to ethanol (200 μL), followed by adding 5 wt.% Nafion solution (20 μL), and ultrasonicating for 30 minutes to fully disperse it;

[0069] Step (2) Take 100 μL of the solution prepared in step (1) and evenly apply it on the Sigracet 29BC gas diffusion layer (GDL, Sigracet 29BC), and then dry it naturally.

[0070] Test Example 1: Using the H-type electrolytic cell working electrode and the flow-type electrolytic cell working electrode prepared in Example 2, CO2 was reduced to methanol. The specific test method is as follows:

[0071] (1) In the test in the H-type electrolytic cell, Ag / AgCl and platinum sheet were used as reference electrode and counter electrode respectively, and FePAG was used as working electrode. The cathode chamber and anode chamber were separated by Nafion 117 proton exchange membrane. Each chamber was filled with 20 ml of 0.5 M KHCO3 solution electrolyte. Before all electrochemical measurements, CO2 was introduced into the cathode chamber for half an hour to saturate the dissolution of CO2 in the electrolyte. During the electrolysis process, the flow rate of CO2 was controlled to 20 sccm.

[0072] (2) In the test in the flow-type electrolyzer, the iron-based polylattice molecule (FePAG) was used as the working electrode, and Ag / AgCl and iridium oxide-loaded titanium mesh (IrO2 / Ti mesh) were used as the reference electrode and the counter electrode, respectively. The cathode chamber and the anode chamber were separated by a Nafion 117 membrane. During the electrolysis process, the flow rate of CO2 was controlled to be 30sccm. 0.1M KOH+3M KCl and 1M KOH electrolytes were continuously circulated in the cathode chamber and the anode chamber, respectively, at a flow rate of 20mL / min. The electrochemical measurements were controlled and recorded using a CHI 650E potentiometer. The gas products were monitored by online gas chromatography (GC 7890B, Agilent), while the liquid products after the reaction were measured by nuclear magnetic resonance (600MHz 1 H NMR, Bruker Advance).

[0073] (3) Test results are as follows Figures 1 to 5 As shown:

[0074] Figure 1 This is the Faraday efficiency distribution diagram of CO2 reduction products under different potentials of FePAG catalyst in H-type electrolyzer. Methanol is the only liquid product, and the Faraday efficiency is the highest at -0.8V, reaching 60.5%.

[0075] Figure 2These are the selectivity test results of FePAG catalyst for CO2 reduction to produce methanol in an H-type electrolyzer. The selectivity of methanol is 98.3% at -0.8V.

[0076] Figure 3 This is the CO2 reduction stability test result of FePAG catalyst in H-type electrolyzer at -0.8V. The catalyst can work stably for 100h.

[0077] Figure 4 The production rate of methanol by reducing CO2 to FePAG catalyst at different potentials in an H-type electrolyzer is 9.8 μmol h -1 cm -2 .

[0078] Figure 5 The Faraday efficiency and current density distribution of methanol produced by CO2 reduction under different potentials in a flow-type electrolyzer over FePAG catalyst. The methanol Faraday efficiency is the highest at -0.7 V, reaching 64.2%, and the current density of methanol is 131 mA cm -2 .

[0079] As described above, although the present invention has been shown and described with reference to specific preferred embodiments, it should not be construed as limiting the present invention itself. Various changes in form and details may be made without departing from the spirit and scope of the present invention as defined in the appended claims.

Claims

1. An iron-based polylattice molecular catalyst, characterized in that: The general structure is as follows:

2. The method for preparing the iron-based polymerized molecular catalyst according to claim 1, characterized in that: The steps include: Step 1: Add 3,6-dibromocarbazole, ethyl bromide, sodium hydroxide and tetrabutylammonium bromide into a three-necked flask, then add acetone, and stir in an oil bath at 60-70° C. for 1.5-3 hours to obtain 3,6-dibromoethylcarbazole; Step 2: Put 3,6-dibromoethylcarbazole, biphenylphosphinoyl ferrocene and potassium acetate into a sealed flask, evacuate and blow nitrogen, and inject [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride and dry 1,4-dioxane into the flask under nitrogen protection, respectively, and react at 100-110° C. for 8-15 hours to obtain 9-ethyl-3,6-bis(4,4,5,5-tetramethyl-1,3,2-dioxaborolane-2-yl)-9H-carbazole; Step 3, preparing 2,7-dibromo-9-(4-(octyloxy)phenyl)-9H-fluoren-9-ol; Step 3.1, add Mg chips into a flask, and then add iodine particles; seal the flask, evacuate and purify with nitrogen, and slowly inject 1-bromo-4-(octyloxy)benzene and tetrahydrofuran into the flask in batches under nitrogen protection, and after the injection, reflux at 70-90° C. for 3-6 hours to obtain the Grignard reagent; Step 3.2, then under nitrogen protection, add the prepared Grignard reagent dropwise into a reaction bottle containing 2,7-dibromofluorenone and tetrahydrofuran, and ensure that the temperature in the reaction bottle is in the range of 0 to 10° C.; after the dropwise addition is completed, reflux at 80 to 90° C. for 5 to 8 hours to obtain 2,7-dibromo-9-(4-(octyloxy)phenyl)-9H-fluoren-9-ol; Step 4: Add 9-ethyl-3,6-bis(4,4,5,5-tetramethyl-1,3,2-dioxaborolane-2-yl)-9H-carbazole, 2,7-dibromo-9-(4-(octyloxy)phenyl)-9H-fluorene-9-ol and Pd(PPh3)4 catalyst into a three-necked flask; then, evacuate and replace the reaction system with nitrogen several times to ensure an oxygen-free environment; add a mixture of toluene and tetrahydrofuran bubbled with nitrogen and a K2CO3 / KF aqueous solution into the flask through a syringe; seal the reaction system and connect a nitrogen balloon, and stir the reaction in an oil bath at 90-100°C for 1.5-3 hours to obtain the synthon BOH; Step 5, 4-methyl-N,N-diphenylaniline is placed in a reaction bottle, dichloromethane is added to dissolve to obtain a 4-methyl-N,N-diphenylaniline solution, and then BF3·Et2O is added thereto; BOH is dissolved in dichloromethane to obtain a BOH solution, and the BOH solution is placed in a constant pressure dropping funnel; the BOH solution is slowly added dropwise to the reaction bottle at room temperature, and stirring is continued for 5 to 10 minutes after the addition is completed to obtain compound BG; Step 6: In a light-proof nitrogen environment in a glove box, add BG and toluene to a flask to obtain a BG solution; add bipyridine and bis(1,5-cyclooctadiene) nickel to a dry reaction tube in a light-proof nitrogen environment in a glove box, seal the tube, and gradually add 1,5-cyclooctadiene and N,N-dimethylformamide to the reaction tube with a syringe; preheat the reaction tube in a 65-75°C oil bath for 20-40 minutes, and then add the BG solution to the reaction tube in a nitrogen environment; then heat the oil bath to 80-90°C and stir to react for 4-6 days, then add a capping agent, bromobenzene, to cap the tube, and continue to react for 1-2 days to obtain a polylattice molecule PAG; Step 7: Add the polylattice molecule PAG into a flask, followed by dichloromethane; then add the ethanol solution of FeCl3 into the flask; stir the reaction mixture at room temperature for 10 to 15 hours to obtain the iron-based polylattice molecule FePAG.

3. The method for preparing the iron-based polymerized molecular catalyst according to claim 2, characterized in that: In step 1, the molar ratio of ethyl bromide to 3,6-dibromocarbazole is 1:1 to 1.5:1; the molar ratio of sodium hydroxide to 3,6-dibromocarbazole is 1:2 to 1.5:1; the molar ratio of tetrabutylammonium bromide to 3,6-dibromocarbazole is 1:20 to 1:5; acetone is used as a solvent, and the concentration of 3,6-dibromocarbazole is 0.1 to 0.3M; In step 2, the molar ratio of pinacol diboron to 3,6-dibromoethylcarbazole is 2:1-5:1; the molar ratio of potassium acetate to 3,6-dibromoethylcarbazole is 3:1-5:1; the molar ratio of [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride to 3,6-dibromoethylcarbazole is 1:20-3:20; 1,4-dioxane is used as a solvent, and the concentration of 3,6-dibromoethylcarbazole is 0.15-0.3M; In step 3.1, the molar ratio of Mg turnings to 1-bromo-4-(octyloxy)benzene is 1:2 to 1:1; the molar ratio of I2 to 1-bromo-4-(octyloxy)benzene is 1:210 to 1:52.5; tetrahydrofuran is used as a solvent, and the concentration of 1-bromo-4-(octyloxy)benzene is 1 to 3M; In step 3.2, the molar ratio of 2,7-dibromofluorenone to 1-bromo-4-(octyloxy)benzene in step 3.1 is 1:4 to 1:2; tetrahydrofuran is used as a solvent, and the concentration of 2,7-dibromofluorenone is 0.25 to 0.6 M; In step 4, the molar ratio of 2,7-dibromo-9-(4-(octyloxy)phenyl)-9H-fluorene-9-ol and 9-ethyl-3,6-bis(4,4,5,5-tetramethyl-1,3,2-dioxaborolane-2-yl)-9H-carbazole is 2:1 to 4:1; the molar ratio of Pd(PPh3)4 and 9-ethyl-3,6-bis(4,4,5,5-tetramethyl-1,3,2-dioxaborolane-2-yl)-9H-carbazole is 1:7 to 1:3; the molar ratio of K2CO3 and 9-ethyl-3,6-bis(4,4,5 The molar ratio of KF to 9-ethyl-3,6-bis(4,4,5,5-tetramethyl-1,3,2-dioxaborolane-2-yl)-9H-carbazole is 1:1 to 4:1; the molar ratio of KF to 9-ethyl-3,6-bis(4,4,5,5-tetramethyl-1,3,2-dioxaborolane-2-yl)-9H-carbazole is 1:1 to 4:1; the concentration of 9-ethyl-3,6-bis(4,4,5,5-tetramethyl-1,3,2-dioxaborolane-2-yl)-9H-carbazole is 0.15 to 0.3 M; the concentration of K2CO3 / KF aqueous solution is 1.5 to 3 M; In step 5, the molar ratio of BF3·Et2O to BOH is 7:1 to 15:1; the molar ratio of 4-methyl-N,N-diphenylaniline to BOH is 1:1 to 1.5:1; the concentration of the 4-methyl-N,N-diphenylaniline solution is 1 to 4 mM; the concentration of the BOH solution is 1 to 4 mM; In step six, the molar ratio of bipyridine to BG is 3:1 to 5:1; the molar ratio of bis(1,5-cyclooctadiene)nickel to BG is 3:1 to 5:1; the molar ratio of 1,5-cyclooctadiene to BG is 3:1 to 5:1; the volume ratio of N,N-dimethylformamide to toluene is 1:14 to 1:3; the volume ratio of bromobenzene to toluene is 1:15 to 1:5; the concentration of BG in toluene is 0.05 to 0.2 M; In step seven, the mass ratio of FeCl3 to PAG is 1:5 to 1:2; the volume ratio of dichloromethane to ethanol is 1:1 to 2:

1.

4. The use of the iron-based polylattice molecular catalyst according to claim 1, characterized in that: The iron-based polymer molecule is used to prepare a working electrode, and the working electrode is used to reduce CO2 into methanol.

5. The use of the iron-based polylattice molecular catalyst according to claim 4, characterized in that: The preparation steps of the working electrode are as follows: Step (1), adding the iron-based polymer molecule FePAG to ethanol, then adding the Nafion solution, and ultrasonicating for 30 minutes to fully disperse it; Step (2), taking 100 μL of the solution prepared in step (1) and evenly applying it on carbon paper, and then drying it naturally to obtain a working electrode of an H-type electrolytic cell; Step (3), take 100 μL of the solution prepared in step (1) and evenly apply it on the Sigracet 29BC gas diffusion layer, and then dry it naturally to obtain the working electrode of the flow-type electrolytic cell.

6. The use of the iron-based polymerized molecular catalyst according to claim 5, characterized in that: In step (1), after the iron-based polymer molecule FePAG is added to ethanol, the amount of FePAG in the ethanol is 0.005-0.02 mg / μL; the concentration of the added Nafion solution is 5 wt.%, and the volume ratio of the Nafion solution to the ethanol is 1:20-1:5; In step (2), 100 μL of the solution prepared in step (1) is evenly dropped on carbon paper; In step (3), 100 μL of the solution prepared in step (1) is evenly drop-coated on the Sigracet 29BC gas diffusion layer.

Citation Information

Patent Citations

  • Organic conjugated nano poly-lattice, and preparation method and applications thereof

    CN110092890A

  • Preparation method of iron-based supramolecular catalyst

    CN116640161A

  • Catalytic reaction system for converting carbon dioxide into methanol

    JP2004026667A