Cellulose-based composite aerogel and preparation method thereof

By combining magnesium-aluminum layered double hydroxide and hydrophobic Si-O-Si binder into cellulose aerogel, the poor mechanical properties and water absorption problems of cellulose aerogel are solved, and a high-quality Elastic, hydrophobic and flame retardant cellulose-based composite aerogels suitable for thermal insulation applications under extreme conditions.

CN118978749APending Publication Date: 2024-11-19CENT SOUTH UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411065133.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Because of its weak physical crosslinking, cellulose aerogel exhibits hydrophilicity, poor mechanical properties and low limit oxygen index, resulting in reduced water absorption and thermal insulation effect, structural collapse and short service life, and magnesium-aluminum layered double hydrogen The self-stacking structure of oxide nanoparticles limits mechanical properties.

Method used

Combine magnesium-aluminum layered double hydroxide and hydrophobic Si-O-Si binder into cellulose aerogel, and form a Si-O-Si bonding network through silane hydrolysis and in situ mineralization to support Mg/Al LDH nanoparticles and enhance mechanical elasticity and hydrophobicity, cellulose-based composite aerogels are prepared by freeze-drying and heat treatment.

Benefits of technology

The obtained cellulose-based composite aerogel has good high elasticity, hydrophobicity, insulation and flame retardancy, and is suitable for the thermal insulation field under extreme conditions, solving the problems of poor mechanical properties and self-stacking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978749A_ABST
    Figure CN118978749A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of composite materials, and discloses cellulose-based composite aerogel and a preparation method thereof.The cellulose-based composite aerogel is obtained by compounding magnesium-aluminum layered double hydroxide and a hydrophobic Si-O-Si adhesive into cellulose aerogel at the same time; the preparation method of the cellulose-based composite aerogel comprises the following steps: mixing silanol, a magnesium-aluminum layered double hydroxide dispersion liquid and a cellulose suspension liquid to form a precursor suspension liquid; and pouring the precursor suspension into a mold, and carrying out freeze drying and heat treatment to obtain the cellulose-based composite aerogel. Magnesium-aluminum layered double hydroxides (Mg / Al LDH) and a hydrophobic Si-O-Si adhesive are compounded into cellulose aerogel at the same time, the cellulose-based composite aerogel is prepared through a one-pot method and a directional freezing method, and the finally obtained cellulose-based composite aerogel has high elasticity, hydrophobicity, heat preservation performance and flame retardance; the material is expected to be used in the field of thermal insulation under extreme conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite materials, and in particular to a cellulose-based composite aerogel and a preparation method thereof. Background Art

[0002] As a thermal insulation material, cellulose aerogel has attracted widespread attention due to its environmental friendliness, biodegradability and low cost. However, due to the weak physical cross-linking of cellulose molecular chains, cellulose aerogels usually exhibit hydrophilicity, poor mechanical properties and a low limiting oxygen index. The water absorption of porous aerogels will significantly reduce their thermal insulation effect, because the thermal conductivity of water is much higher than that of air, and water erosion may cause its structure to collapse, thus affecting its use effect; poor mechanical properties will affect the service life of the material, and the low limiting oxygen index will affect the safety of the material.

[0003] At present, due to the large specific surface area and excellent thermodynamic properties of magnesium aluminum layered double hydroxide (Mg / AlLDH), some patents and literature have doped it in cellulose aerogels to improve flame retardancy and thermal insulation. However, Mg / Al LDH nanoparticles are small in size and have high charge density, and they tend to aggregate in solution through ab-plane stacking. This tight self-stacking structure limits stress transfer in the three-dimensional framework, resulting in poor mechanical properties, which seriously hinders their development and practical application potential.

[0004] Therefore, how to provide a cellulose-based composite aerogel with excellent hydrophobicity, thermal insulation and mechanical properties is a problem that technical personnel in this field urgently need to solve. Summary of the invention

[0005] In view of this, the present invention provides a cellulose-based composite aerogel to solve the problem that the existing cellulose aerogel exhibits hydrophilicity and has poor mechanical properties, thermal insulation and flame retardancy.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] On the one hand, the present invention provides a cellulose-based composite aerogel, wherein the cellulose-based composite aerogel is obtained by simultaneously compounding a magnesium-aluminum layered double hydroxide and a hydrophobic Si-O-Si binder into a cellulose aerogel.

[0008] On the other hand, the present invention also provides a method for preparing the above-mentioned cellulose-based composite aerogel, comprising the following steps:

[0009] (1) mixing silanol, a magnesium aluminum layered double hydroxide dispersion and a cellulose suspension to form a precursor suspension;

[0010] (2) pouring the precursor suspension into a mold, freeze-drying and heat-treating to obtain a cellulose-based composite aerogel.

[0011] Preferably, the preparation method of silanol in step (1) is as follows: methoxytrimethylsilane, vinyltriethoxysilane and an acidic solution are mixed to obtain silanol.

[0012] Preferably, the volume ratio of methoxytrimethylsilane, vinyltriethoxysilane and acidic solution is (1-2):(0.05-0.1):(3-5).

[0013] Preferably, the pH value of the acidic solution is 3-5.

[0014] Preferably, the preparation method of the magnesium aluminum layered double hydroxide dispersion in step (1) is as follows: heat-treating the magnesium aluminum layered double hydroxide and dispersing it in water, heating and stirring to obtain the magnesium aluminum layered double hydroxide dispersion.

[0015] Preferably, the heat treatment temperature is 400-500° C., and the heat treatment time is 9-11 hours.

[0016] Preferably, the heating and stirring temperature is 70-90°C and the time is 3-5h.

[0017] Preferably, in step (1), the ratio of silanol, magnesium aluminum layered double hydroxide dispersion and cellulose suspension is (0.7-1.1) mL: (0.125-0.5) mL: 5 g.

[0018] Preferably, the concentration of the magnesium aluminum layered double hydroxide dispersion is 20 mg / mL, and the concentration of the cellulose suspension is 0.3-0.6 wt %.

[0019] Preferably, the freeze-drying in step (2) is: placing the mold containing the precursor suspension on top of a metal block, cooling the metal block by liquid nitrogen to freeze the precursor suspension, and then performing freeze-drying for 24-72 hours.

[0020] Preferably, the heat treatment temperature in step (2) is 60-100° C., and the heat treatment time is 4-8 h.

[0021] The present invention provides a cellulose-based composite aerogel, which has the following beneficial effects compared with the prior art:

[0022] The present invention simultaneously compounds magnesium aluminum layered double hydroxide (Mg / Al LDH) and a hydrophobic Si-O-Si binder into a cellulose (CNF-C) aerogel, wherein the Si-O-Si group in the hydrophobic Si-O-Si binder helps to improve the mechanical elasticity of the aerogel, and the -CH3 group helps to improve the hydrophobicity of the aerogel. The Mg / Al LDH has the characteristics of flame retardancy, halogen-free and non-volatile, and helps to improve the thermal insulation and flame retardancy of the aerogel. The obtained cellulose-based composite aerogel has good high elasticity, hydrophobicity, thermal insulation and flame retardancy, and can be used in the field of thermal insulation under extreme conditions.

[0023] The cellulose-based composite aerogel prepared by the one-pot method can support Mg / Al LDH nanoparticles on a CNF-C carrier with a high surface area through a Si-O-Si bonding network formed by in-situ mineralization of silane hydrolysis, thereby effectively solving the problem of poor mechanical properties caused by self-stacking of Mg / Al LDH. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0025] Figure 1 The microstructure diagram of the cellulose-based composite aerogel of Example 1, wherein (a) is a top view and (b) is a top view;

[0026] Figure 2 Schematic diagram of the cellulose-based composite aerogel of Example 1 before and after external force compression;

[0027] Figure 3 This is a schematic diagram of the water contact angle test results of the cellulose-based composite aerogel in Example 1;

[0028] Figure 4 This is a schematic diagram of the thermal insulation test results of the cellulose-based composite aerogel in Example 1;

[0029] Figure 5 This is a schematic diagram of the flame retardancy test results of the cellulose-based composite aerogel in Example 1;

[0030] Figure 6 This is a schematic diagram of the water contact angle test results of the cellulose-based composite aerogel in Example 2;

[0031] Figure 7 Schematic diagram of the water contact angle test results of the cellulose-based composite aerogel in Example 3. DETAILED DESCRIPTION

[0032] The present invention will be described below by specific examples, and it will be appreciated by those skilled in the art that the following specific examples are only for illustrative purposes, and do not limit the scope of the present invention in any way. In addition, in the following examples, unless otherwise specified, the reagents and equipment used are all commercially available. If in the following examples, specific treatment conditions and treatment methods are not clearly described, then conditions and methods known in the art can be used to process.

[0033] In one aspect of the present invention, the present invention provides a cellulose-based composite aerogel, wherein the cellulose-based composite aerogel is obtained by simultaneously compounding a magnesium-aluminum layered double hydroxide and a hydrophobic Si-O-Si binder into a cellulose aerogel.

[0034] It should be noted that the cellulose involved in the specific implementation of this application is carboxylated cellulose nanofibers (CNF-C) purchased from the market, with the following specifications: diameter of 4-10nm, length of 1-3μm, crystal structure of cellulose type I, and carboxyl content of 1.2-3.0mmol / g. Since the present invention aims to simultaneously compound magnesium aluminum layered double hydroxide (Mg / Al LDH) and hydrophobic Si-O-Si binder into cellulose aerogel to improve the hydrophobicity, mechanical elasticity and thermal insulation performance of the aerogel, it is not limited to the cellulose of the purchased specifications in the specific use process of the present invention.

[0035] The present invention simultaneously compounds magnesium aluminum layered double hydroxide (Mg / Al LDH) and a hydrophobic Si-O-Si binder into a cellulose (CNF-C) aerogel, wherein the Si-O-Si group in the hydrophobic Si-O-Si binder helps to improve the mechanical elasticity of the aerogel, and the -CH3 group helps to improve the hydrophobicity of the aerogel. The Mg / Al LDH has the characteristics of flame retardancy, halogen-free and non-volatile, and helps to improve the thermal insulation and flame retardancy of the aerogel. The obtained cellulose-based composite aerogel has good high elasticity, hydrophobicity, thermal insulation and flame retardancy, and can be used in the field of thermal insulation under extreme conditions.

[0036] In another aspect of the present invention, the present invention provides a method for preparing the above-mentioned cellulose-based composite aerogel, comprising the following steps:

[0037] Step S100: Mix silanol, magnesium aluminum layered double hydroxide dispersion and cellulose suspension to form a precursor suspension.

[0038] The preparation method of silanol is as follows: methoxytrimethylsilane (MTMS), vinyltriethoxysilane (VTES) and an acidic solution are mixed in a volume ratio of (1-2): (0.05-0.1): (3-5), stirred and hydrolyzed to obtain silanol. Preferably, the pH value of the acidic solution is 3-5, for example, pH=3, pH=4 or pH=5, and the acidic solution can be CH3COOH or HCl.

[0039] Alternatively, the preparation method of silanol is: add 1-2 mL of methyltrimethoxysilane (MTMS) and 50-100 μL of vinyltriethoxysilane (VTES) to 3-5 mL of CH3COOH or HCl (pH=4) solution, and stir for 2 h to hydrolyze and form silanol.

[0040] The preparation method of magnesium aluminum layered double hydroxide dispersion is as follows: heat-treat magnesium aluminum layered double hydroxide at 400-500° C. for 9-11 hours, then disperse the heat-treated material in water, heat and stir at 70-90° C. for 3-5 hours to obtain magnesium aluminum layered double hydroxide dispersion.

[0041] Optionally, the heat treatment temperature can be 400°C, 450°C, 500°C, etc., and the heat treatment time can be 9h, 10h, 11h, etc. The heating and stirring speed is 500-800rpm, for example, 500rpm, 600rpm, 800rpm, etc., the heating and stirring temperature can be 70°C, 80°C, 90°C, etc., and the heating and stirring time can be 3h, 4h, 5h, etc.

[0042] The ratio of silanol, magnesium aluminum layered double hydroxide dispersion and cellulose suspension is (0.7-1.1) mL: (0.125-0.5) mL: 5 g. Preferably, the concentration of magnesium aluminum layered double hydroxide dispersion is 20 mg / mL, and the concentration of cellulose suspension is 0.3-0.6 wt%.

[0043] The present invention adopts a one-pot preparation method, and the Si-O-Si bonding network formed by in-situ mineralization of silane hydrolysis can support Mg / Al LDH nanoparticles on a CNF-C carrier with a high surface area, thereby effectively solving the problem of poor mechanical properties caused by self-stacking of Mg / Al LDH; in addition, the Si-O-Si group helps to improve the mechanical elasticity of the aerogel, the -CH3 group helps to improve the hydrophobicity of the aerogel, and the Mg / Al LDH has the characteristics of flame retardancy, halogen-free and non-volatility, which helps to improve the thermal insulation and flame retardancy of the aerogel.

[0044] Step S200: pouring the precursor suspension into a mold, freeze-drying and heat-treating to obtain a cellulose-based composite aerogel.

[0045] In this step, freeze drying is as follows: placing a mold on top of the metal block so that the bottom of the mold contacts the top of the metal block, and using liquid nitrogen to cool the metal block for 24-72 hours, for example, 24 hours, 48 ​​hours, 72 hours, etc.

[0046] The heat treatment is as follows: the freeze-dried material is heat treated in an oven at a temperature of 60-100° C. for 4-8 hours.

[0047] The present invention adopts a bottom-up freeze-drying method and directional freeze-drying, which can finely control the growth of ice crystals and adjust the microstructure of the aerogel. This layered engineering structure is conducive to effective stress and heat transfer.

[0048] The present invention is further described below by means of specific embodiments.

[0049] Example 1

[0050] Mg / Al LDH was heat treated at 450 °C for 600 min, and the heat-treated material was dispersed in ultrapure water and magnetically stirred at 600 rpm and 80 °C for 4 h to form a uniform Mg / Al LDH dispersion (20 mg mL -1 ); 1 mL of MTMS and 50 μL VTES were added to 3 mL of CH3COOH solution and stirred for 2 h to hydrolyze and form silanol.

[0051] 800 μl of silanol and 0.25 mL of 20 mg mL -1 The Mg / Al LDH dispersion was added to 5 g of 0.3 wt% CNF-C suspension in turn and stirred at room temperature for 1 h to form a uniform precursor suspension. An appropriate amount of the precursor suspension was poured into a mold so that the bottom of the mold was in contact with the top of the copper block. The precursor suspension in the mold was directionally frozen by cooling the copper block with liquid nitrogen, and the frozen material was then freeze-dried for 72 h. The obtained aerogel was heat-treated in an oven at 80 ° C for 4 h to obtain a cellulose-based composite aerogel.

[0052] Example 2

[0053] Mg / Al LDH was heat treated at 450 °C for 600 min, and the heat-treated material was dispersed in ultrapure water and magnetically stirred at 600 rpm and 80 °C for 4 h to form a uniform Mg / Al LDH dispersion (20 mg mL -1 ); 1 mL of MTMS and 50 μL VTES were added to 3 mL of CH3COOH solution and stirred for 2 h to hydrolyze and form silanol.

[0054] 700 μl of silanol and 0.125 mL of 20 mg mL -1The Mg / Al LDH dispersion was sequentially added to 5 g of 0.3 wt % CNF-C suspension and stirred at room temperature for 1 h to form a uniform precursor suspension.

[0055] An appropriate amount of the precursor suspension was poured into the mold so that the bottom of the mold was in contact with the top of the copper block. The precursor suspension in the mold was directionally frozen by cooling the copper block with liquid nitrogen, and then the frozen material was freeze-dried for 72 hours. The obtained aerogel was heat-treated in an oven at 80°C for 4 hours to obtain a cellulose-based composite aerogel.

[0056] Example 3

[0057] Mg / Al LDH was heat treated at 450 °C for 600 min, and the heat-treated material was dispersed in ultrapure water and magnetically stirred at 600 rpm and 80 °C for 4 h to form a uniform Mg / Al LDH dispersion (20 mg mL -1 ); 1 mL of MTMS and 50 μL VTES were added to 3 mL of CH3COOH solution and stirred for 2 h to hydrolyze and form silanol.

[0058] 1100 μl of silanol and 0.5 mL of 20 mg mL -1 The Mg / Al LDH dispersion was sequentially added to 5 g of 0.6 wt % CNF-C suspension and stirred at room temperature for 1 h to form a uniform precursor suspension.

[0059] An appropriate amount of the precursor suspension was poured into the mold so that the bottom of the mold was in contact with the top of the copper block. The precursor suspension in the mold was directionally frozen by cooling the copper block with liquid nitrogen, and then the frozen material was freeze-dried for 72 hours. The obtained aerogel was heat-treated in an oven at 80°C for 4 hours to obtain a cellulose-based composite aerogel.

[0060] The present invention conducted various performance tests on the cellulose-based composite aerogels prepared in Examples 1-3. The test process and results are as follows:

[0061] (I) Microscopic morphology characterization of cellulose-based composite aerogels

[0062] Scanning electron microscopy (SEM) was used to observe the microscopic morphology of the cellulose-based composite aerogel. The aerogel was cut with a blade and adhered to the conductive glue, and then the top view and side view were taken.

[0063] Figure 1 This is a scanning electron microscope image of the cellulose-based composite aerogel prepared in Example 1. As shown in the figure, the top view of the aerogel presents a honeycomb structure, and the side view presents a layered structure.

[0064] (II) Elastic properties of cellulose-based composite aerogels

[0065] A camera is used to capture the height changes of the cellulose-based composite aerogel before and after compression by a weight to determine its elasticity.

[0066] Figure 2 This is a schematic diagram of the cellulose-based composite aerogel prepared in Example 1 before and after external force compression. It can be seen from the figure that the aerogel is compressed into a thin sheet under external force and then returns to its original shape after the external force is released, indicating that the aerogel has excellent elastic properties.

[0067] (III) Hydrophobic properties of cellulose-based composite aerogels

[0068] The contact angle of the cellulose-based composite aerogel was tested using an optical contact angle meter (JC2000D1, Data Physics Instruments), and the volume of the water droplet was approximately 3 μL.

[0069] Figure 3 , Figure 6 , Figure 7 Schematic diagrams of water contact angles of cellulose-based composite aerogels prepared in Examples 1 to 3. As can be seen from the figure, the water contact angles of cellulose-based composite aerogels prepared in Examples 1 to 3 are 140.49°, 133.99°, and 128.49°, respectively, indicating that the cellulose-based composite aerogels have good hydrophobicity.

[0070] (IV) Thermal insulation properties of cellulose-based composite aerogels

[0071] The cellulose-based composite aerogel was placed on a constant temperature heating plate at 392℉ (200℃) and heated continuously for 20 minutes to test the thermal insulation performance of the cellulose-based composite aerogel.

[0072] Figure 4 This is a test chart of the cellulose-based composite aerogel prepared in Example 1 after continuous heating for 20 minutes. The initial temperature of the upper surface is 124.6℉. After heating for 20 minutes, the upper surface temperature is only 138.9℉, which is very different from the temperature of the lower surface, indicating that the cellulose-based composite aerogel blocks heat transfer and has good thermal insulation performance.

[0073] (V) Flame retardant properties of cellulose-based composite aerogels

[0074] The cellulose-based composite aerogel is placed in a butane flame and burned, and the flame retardant properties of the aerogel are determined by judging whether the aerogel self-extinguishes after the butane flame is removed.

[0075] Figure 5This is a schematic diagram of the flame retardancy test of the cellulose-based composite aerogel prepared in Example 1. As can be seen from the figure, after the cellulose-based composite aerogel is removed from the butane flame, the flame on the cellulose-based composite aerogel is extinguished, indicating that the cellulose-based composite aerogel has good flame retardancy.

[0076] In summary, the present invention simultaneously compounds magnesium aluminum layered double hydroxide (Mg / Al LDH) and hydrophobic Si-O-Si binder into cellulose aerogel, and prepares cellulose-based composite aerogel by a one-pot method and a directional freezing method. The final cellulose-based composite aerogel has high elasticity, hydrophobicity, thermal insulation and flame retardancy, and is expected to be used in the field of thermal insulation under extreme conditions.

[0077] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A cellulose-based composite aerogel, characterized in that: The cellulose-based composite aerogel is obtained by simultaneously compounding magnesium-aluminum layered double hydroxide and a hydrophobic Si-O-Si binder in a cellulose aerogel.

2. A method for preparing the cellulose-based composite aerogel according to claim 1, characterized in that: The following steps are involved: (1) mixing silanol, a magnesium aluminum layered double hydroxide dispersion and a cellulose suspension to form a precursor suspension; (2) pouring the precursor suspension into a mold, freeze-drying and heat-treating to obtain a cellulose-based composite aerogel.

3. The method for preparing the cellulose-based composite aerogel according to claim 2, characterized in that: The preparation method of silanol in step (1) is as follows: methoxytrimethylsilane, vinyltriethoxysilane and an acidic solution are mixed to obtain silanol.

4. The method for preparing the cellulose-based composite aerogel according to claim 3, characterized in that: The volume ratio of methoxytrimethylsilane, vinyltriethoxysilane and acidic solution is (1-2):(0.05-0.1):(3-5).

5. The method for preparing the cellulose-based composite aerogel according to claim 4, characterized in that: The pH value of the acidic solution is 3-5.

6. The method for preparing the cellulose-based composite aerogel according to claim 2, characterized in that: The preparation method of the magnesium aluminum layered double hydroxide dispersion in step (1) is as follows: The magnesium aluminum layered double hydroxide is heat-treated and dispersed in water, and heated and stirred to obtain a magnesium aluminum layered double hydroxide dispersion.

7. The method for preparing the cellulose-based composite aerogel according to claim 6, characterized in that: The heat treatment temperature is 400-500°C and the heat treatment time is 9-11h; The heating and stirring temperature is 70-90°C and the time is 3-5h.

8. The method for preparing the cellulose-based composite aerogel according to any one of claims 2 to 7, characterized in that: In step (1), the ratio of silanol, magnesium aluminum layered double hydroxide dispersion and cellulose suspension is (0.7-1.1) mL: (0.125-0.5) mL: 5 g; The concentration of the magnesium aluminum layered double hydroxide dispersion is 20 mg / mL, and the concentration of the cellulose suspension is 0.3-0.6 wt %.

9. The method for preparing the cellulose-based composite aerogel according to claim 2, characterized in that: The freeze drying in step (2) is as follows: placing the mold containing the precursor suspension on top of a metal block, cooling the metal block with liquid nitrogen to freeze the precursor suspension, and then performing freeze drying for 24-72 hours.

10. The method for preparing the cellulose-based composite aerogel according to claim 2, characterized in that: The heat treatment temperature in step (2) is 60-100° C., and the heat treatment time is 4-8 hours.

Citation Information

Cited By

  • Hybrid aerogel, hybrid aerogel coating and aerogel super-hydrophobic flame-retardant insulation board thereof

    CN120137401A