AgBiS2 nanocrystalline ink, preparation method and application in photoelectric device

By dissolving Ag/Bi metal precursor and thiol molecules in polar organic solvents, reacting with sulfur sources and organic amines, AgBiS2 nanocrystalline ink is generated, which solves the problems of cumbersome process, high cost and poor stability in the prior art, and realizes the problem of cumbersome process, high cost and poor stability. It has efficient nanocrystalline ink preparation and photoelectric properties regulation, and is suitable for batch printing and preparation of large-area optoelectronic devices.

CN118978827AActive Publication Date: 2024-11-19SUZHOU UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411000376.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-19
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

The existing AgBiS2 nanocrystalline ink preparation process is cumbersome, costly and poor stability, and there are defective regeneration problems during nanocrystalline ligand exchange, which limits its application in optoelectronic devices.

Method used

Dissolve Ag/Bi metal precursor and thiol molecules in a polar organic solvent, react with sulfur source and organic amine to form AgBiS2 nanocrystal mother liquor, and obtain nanocrystal powder through precipitation and drying, and finally disperse into colloidal ink. Direct synthesis method achieves high dispersion and stability of nanocrystals.

Benefits of technology

It realizes the high dispersion and stability of AgBiS2 nanocrystals, improves the ability to regulate photoelectric properties, and is suitable for large-area batch printing and preparation. The stability of nanocrystal ink can be maintained for more than three months, and is suitable for efficient solar cell devices. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978827A_ABST
    Figure CN118978827A_ABST
Patent Text Reader

Abstract

The invention discloses AgBiS2 nanocrystalline ink, a preparation method and application of the AgBiS2 nanocrystalline ink in photoelectric devices. In a polar organic solvent, silver and bismuth metals are used as cation sources, sulfydryl molecules are introduced as a synergistic passivator, and one-step sulfur source injection is adopted to initiate a reaction, so that the AgBiS2 nanocrystal is obtained. The photoelectric property of the AgBiS2 nanocrystal is regulated and controlled by adjusting the charge ratio of the halide precursor, the AgBiS2 nanocrystal is used as a photoactive layer of a photoelectric device, especially the initial application in a solar cell is realized, and the photoelectric conversion efficiency can reach 7.66%. The sulfur bismuth silver nanocrystal prepared based on direct synthesis is excellent in quality, the stability of the nanocrystal solution is good, and the nanocrystal solution is not agglomerated after being stored for more than ten months; more than 10 g of AgBiS2 nanocrystals can be prepared in batches at a time, the cost is low, and large-scale production and application are facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for synthesizing and preparing green and non-toxic AgBiS2 nanocrystalline ink with excellent colloid stability and application in optoelectronic devices, belonging to the technical field of functional materials. Background Art

[0002] Silver bismuth sulfide (AgBiS2) nanocrystals have attracted widespread attention due to their ultra-high absorption coefficient. Thanks to their abundant raw materials, non-toxicity, and low cost, they are considered to be promising non-toxic substitutes for traditional cadmium-based and lead-based semiconductor nanocrystals, becoming a new type of "green" nano-photoelectric material to build ultra-thin and ultra-flexible optoelectronic devices.

[0003] When the AgBiS2 nanocrystal film is used as the active layer of the optoelectronic device, the solution-phase ligand exchange method avoids the cumbersome process of preparing nanocrystalline conductive films by solid-phase ligand exchange after traditional synthesis, and the nanocrystalline ink after ligand exchange can be applied in one step. In addition, the high ligand exchange rate in the solution phase is conducive to narrower band tail states and low defect state density, thereby reducing the open circuit voltage loss of the device (see literature: Adv. Energy Mater. 2023, 2302579, Adv. Energy Mater. 2022, 2200700), which provides the possibility for printable and large-area preparation applications. However, this method is still based on AgBiS2 nanocrystals wrapped with oleic acid ligands synthesized by hot injection in a non-polar solvent system, and the defect regeneration problem in the ligand exchange process cannot be avoided. At the same time, the high ligand exchange rate in the solution phase makes batch preparation difficult, and the nanocrystalline ink after ligand exchange can only be stably stored for one week, which is not conducive to its further application.

[0004] Chinese invention patent CN 115893488 A discloses a method for synthesizing AgBiS2 nanocrystals in one step at low temperature[]. Pure phase AgBiS2 nanocrystals were prepared, simplifying the material preparation process. However, this method still needs to be further explored in terms of material property regulation and device application. Summary of the invention

[0005] In view of the shortcomings of the prior art nanocrystalline ink, such as complicated preparation process, high cost, poor ink stability, and defect regeneration during nanocrystal ligand exchange, the present invention provides a AgBiS2 nanocrystalline ink with high colloid quality, low direct synthesis cost and suitable for batch preparation, a preparation method and its application in optoelectronic devices.

[0006] The technical solution to achieve the purpose of the present invention is to provide a method for preparing AgBiS2 nanocrystalline ink, comprising the following steps: 1) dissolving a Ag / Bi metal precursor and a thiol molecule in a polar organic solvent to obtain a reaction precursor; the molar ratio of the Ag / Bi metal precursor to the thiol molecule is 1:1 to 6:1; the Ag / Bi metal precursor comprises an Ag metal compound and a Bi metal compound, and the molar ratio of Ag to Bi element is 1:1 to 10:1; 2) Mixing the sulfur source, the organic amine and the reaction precursor, reacting for 1 to 150 minutes at a temperature of -20°C to 150°C to obtain a mother solution of AgBiS2 nanocrystals; 3) adding an anti-solvent to the obtained AgBiS2 nanocrystal mother liquor, and performing precipitation and drying treatment to obtain AgBiS2 nanocrystal powder; 5) Dispersing the nanocrystalline powder in a solvent to obtain nanocrystalline ink with continuously adjustable AgBiS2 concentration.

[0007] The polar organic solvent of the present invention has a dielectric constant of 20 to 90, and a range of solvent donor number of 14 to 18 kcal / mol; it includes N, N-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, butyronitrile, propylene carbonate, γ-valerolactone, and n-butylamine. The anti-solvent includes anhydrous ethanol, isopropanol, methanol, methyl acetate, ethyl acetate, toluene, n-hexane, and n-octane; the solvent includes N, N-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, acetonitrile, butyronitrile, propylene carbonate, γ-valerolactone, water, and acetone.

[0008] The Ag metal compound of the present invention includes silver iodide, silver bromide, silver chloride, silver acetate, silver thiocyanate, and silver nitrate; the Bi metal compound includes bismuth iodide, bismuth bromide, bismuth chloride, bismuth acetate, bismuth nitrate, and triphenyl bismuth. The thiol molecule includes 3-chloro-1-propanethiol, 4-chlorothiophenol, mercaptobenzoic acid, mercaptoethanol, furfuryl mercaptan, 1,4-phenyldithiol, 3-aminothiophenol, 4-aminothiophenol, 4-(trifluoromethyl)thiophenol, 1,2-ethanedithiol, and o-phenylthiol.

[0009] The technical solution of the present invention also includes an AgBiS2 nanocrystalline ink obtained according to the above preparation method.

[0010] The application of the AgBiS2 nanocrystalline ink described in the technical solution of the present invention is to form a film by spin coating, scraping, dip coating, and inkjet printing, and is used as a photoactive layer of a photoelectric device. The photoelectric device includes a solar cell and a photodetector.

[0011] The structure of the solar cell includes upright or inverted; the upright structure is conductive glass / electron transport layer / AgBiS2 absorption layer / hole transport layer / molybdenum trioxide / silver electrode in sequence, and the inverted structure is conductive glass / hole transport layer / AgBiS2 absorption layer / electron transport layer / silver electrode in sequence.

[0012] The principle of the present invention is: the precursor is improved by introducing thiol molecules in situ, which effectively improves the dispersibility of the synthesized nanocrystals compared with the one-step low-temperature synthesis of AgBiS2 nanocrystals in the prior art, and can achieve long-term stability of the dispersion of the nanocrystals in polar solvents. At the same time, in a multi-component nanocrystal system, component control is crucial to the material properties. The present invention can directly change the precursor feed molar ratio by introducing thiol molecules in situ, realize the optimization and regulation of the components of the synthesized AgBiS2 nanocrystals, and thus change the photoelectric properties of the nanocrystals.

[0013] The present invention adopts a method of dissolving a metal precursor in a polar phase, and in situ introduces a short-chain thiol molecule to improve the dispersion of the precursor and the synthesized nanocrystals, thereby realizing the direct synthesis of ternary AgBiS2 nanocrystals, obtaining AgBiS2 nanocrystal ink stably dispersed in a polar solvent, and applying it to solar cell devices. The present invention provides a method for scalably preparing AgBiS2 nanocrystal ink, which is suitable for batch printing preparation of large-area optoelectronic devices in the future, and has important significance for the development and application of AgBiS2 nanocrystals.

[0014] Compared with the prior art, the present invention has the following beneficial effects: 1. The technical solution provided by the present invention has a relatively large steric hindrance formed by the thiol ligand with a thiol group, which regulates the dipole interaction between the nanocrystals and the DMF solvent, and improves the dispersibility and stability of the colloidal nanocrystals. The efficiency of the solar cell device prepared by the AgBiS2 nanocrystal ink after storage for 3 months can still reach the level of fresh ink, which is suitable for the mass printing preparation of large-area optoelectronic devices in the future.

[0015] 2. The present invention changes the composition of nanocrystals by the synthetic feed ratio, thereby achieving the regulation of the photoelectric properties of the nanocrystals and realizing the batch preparation of AgBiS2 nanocrystals. More than 10 g of AgBiS2 nanocrystals can be obtained in a single reaction, and the nanocrystals have a high phase purity.

[0016] 3. The present invention adopts a direct synthesis method to prepare AgBiS2 nanocrystals, prepares AgBiS2 nanocrystal ink by dispersion in polar solvents, and obtains a conductive nanocrystal film in one step, making it an ideal candidate material for application in high-efficiency AgBiS2 nanocrystal solar cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is the XRD diagram of nanocrystals synthesized by using silver iodide (AgI) and bismuth iodide (BiI3) metal precursors in different proportions in Example 1.

[0018] Figure 2This is a TEM image of nanocrystals synthesized using different proportions of metal precursors of silver iodide (AgI) and bismuth iodide (BiI3) in Example 1.

[0019] Figure 3 This is an EDS elemental analysis diagram of AgBiS2 nanocrystals prepared by synthesizing silver iodide (AgI) and bismuth iodide (BiI3) in different proportions as metal precursors in Example 1 of the present invention.

[0020] Figure 4 The reaction temperature in Example 2 is room temperature (RT), 50°C, 80°C, 100°C, 125°C, and 150°C, and the corresponding UV-visible absorption spectra are obtained.

[0021] Figure 5 These are the corresponding EDS spectra obtained in Example 3 at different Ag-Bi:CBT ratios (1:1, 2:1, 3:1, 4:1, 6:1).

[0022] Figure 6 TEM images of the purified nanocrystals in Example 4 at different reaction times (1 to 150 minutes).

[0023] Figure 7 This is the XRD diagram of nanocrystals obtained by using different silver and bismuth compounds in Example 4.

[0024] Figure 8 This is the XRD pattern of AgBiS2 nanocrystals synthesized by using 3-chloro-1-propanethiol as the thiol functional molecule in Example 5 of the present invention.

[0025] Fig. 9 This is the JV diagram corresponding to the solar cell device prepared by synthesizing AgBiS2 nanocrystals as the photoactive layer using different ratios of silver iodide (AgI) and bismuth iodide (BiI3) metal precursors in Example 1 of the present invention.

[0026] Fig.10 This is the absorption diagram of the nanocrystal solution provided in Example 1 when stored for different time periods.

[0027] Fig.11 This is the XRD diagram of the nanocrystals obtained by expanding the reaction by forty times when the AgI:BiI3 ratio is 4:1 in Example 8 of the present invention. DETAILED DESCRIPTION

[0028] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.

[0029] The raw materials and equipment used below, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used below, unless otherwise specified, are all conventional methods in the art.

[0030] The present invention proposes a method for preparing AgBiS2 nanocrystals and their application. In an embodiment of the present invention, the AgBiS2 nanocrystals are prepared by a direct synthesis method, in which a metal precursor dissolved in a polar solvent is mixed with a sulfur source under the action of an organic amine to react to generate stable colloidal AgBiS2 nanocrystals, which are then used to prepare solar cells. Embodiment 1

[0031] This embodiment provides a method for preparing AgBiS2 nanocrystals by direct synthesis. Silver iodide (AgI) and bismuth iodide (BiI3) Ag-Bi metal precursors dissolved in polar solvents are mixed with a sulfur source under the action of organic amines to react and generate stable colloidal AgBiS2 nanocrystals; in this embodiment, the molar amount of AgI is regulated so that the ratio of Ag:Bi put into the reaction system is adjustable within the range of 1:1 to 10:1, and multiple AgBiS2 nanocrystal samples are obtained. The specific steps are as follows: 1) Dissolve AgI, Ag-Bi metal precursors of BiI3 and thiol molecules in a polar organic solvent to obtain a reaction precursor I. In this step, the reaction precursor I is AgI and BiI3 dissolved in an organic solvent DMF (5 mL), with a fixed molar amount of bismuth iodide (0.5 mmol), and the molar amount of AgI is regulated in the range of 1:1 to 10:1 (the specific ratios are 1:1, 2:1, 3:1, 4:1, 6:1 and 10:1, respectively). In this embodiment, the constant ratio of Ag-Bi:4-chlorobenzenethiol is maintained at 2:1, and 6 samples of reaction precursor I with different Ag:Bi ratios are obtained by dissolving at 100°C.

[0032] 2) Organic amine dissolves the sulfur source as reaction precursor II. Ag-Bi:S (N'N-diphenylthiourea) is a constant molar ratio of 2:1. The sulfur source is weighed and dispersed in 1 mL of butylamine to prepare 6 parts of reaction precursor II.

[0033] 3) Precursor II (N'N-diphenylthiourea dissolved in butylamine) was mixed with each precursor I respectively, and the mixture was allowed to react for 20 minutes and then cooled to room temperature.

[0034] 4) The nanocrystals are precipitated from the reaction mother liquor using methyl acetate as an anti-solvent at a volume ratio of 1:6 between the nanocrystal mother liquor and methyl acetate, and then the AgBiS2 nanocrystal powder is obtained by drying.

[0035] See attached Figure 1 , 2 and 3 are respectively the X-ray diffraction pattern (XRD), transmission electron microscope image (TEM) and energy dispersive X-ray spectroscopy (EDS) of the nanocrystals prepared in this example.

[0036] The solution selected in this embodiment has a ratio of AgI:BiI3 of 4:1 and is stored in a nitrogen atmosphere at a temperature of 25°C. The absorption stability curve is shown in Fig.10 ,In the figure, curve I is a fresh solution, curve II is three months, and curve III is ten months.,The results show that the colloid has excellent stability. Embodiment 2

[0037] This embodiment adopts a direct synthesis method to prepare AgBiS2 nanocrystals, by mixing a metal precursor dissolved in a polar solvent and a sulfur source under the action of an organic amine, and initiating a reaction under different reaction temperature conditions to generate stable colloidal AgBiS2 nanocrystals, comprising the following steps: 1) Dissolve AgI, BiI3 and thiol molecules in a polar organic solvent to obtain a reaction precursor I. In this step, 2 mmol AgI, 0.5 mmol BiI3 and 1.25 mmol 4-chlorobenzenethiol are dissolved in the organic solvent DMF (5 mL) of the reaction precursor I; prepare multiple samples and dissolve them at different temperatures from room temperature to 150°C, and the specific temperatures are room temperature (RT), 50°C, 80°C, 100°C, 125°C and 150°C to obtain 6 reaction precursors I.

[0038] 2) Take 1.25 mmol of N'N-diphenylthiourea and disperse it in 1 mL of butylamine to prepare 6 parts of precursor II.

[0039] 3) Precursor II (N'N-diphenylthiourea dissolved in butylamine) was mixed with metal precursor I samples prepared at different temperatures, and the mixture was cooled to room temperature after reacting for 20 minutes.

[0040] 4) Using methyl acetate as an anti-solvent, the nanocrystals are precipitated from the reaction mother liquor at a volume ratio of 1:5 to 1:10 between the nanocrystal mother liquor and methyl acetate, and the AgBiS2 nanocrystal powder is obtained by drying.

[0041] See attached Figure 4 , which is the UV-visible absorption spectra of the purified nanocrystal samples under different reaction temperature conditions provided in this embodiment. Embodiment 3

[0042] AgBiS2 nanocrystals are prepared by direct synthesis method, which includes the following steps: mixing a metal precursor dissolved in a polar solvent and a sulfur source under the action of an organic amine, and inducing a reaction under different ratios of Ag-Bi:4-chlorobenzenethiol (CBT) to generate stable colloidal AgBiS2 nanocrystals. 1) Dissolve AgI, BiI3Ag-Bi metal precursor and thiol molecule in polar organic solvent to obtain reaction precursor I. In this step, 2 mmol AgI and 0.5 mmol BiI3 are dissolved in DMF (5 mL), an organic solvent of reaction precursor I, and CBT is weighed respectively, and 5 parts of reaction precursor I are obtained by dissolving at 100°C according to different ratios of Ag-Bi:CBT of 1:1 to 6:1, and the specific ratios are 1:1, 2:1, 3:1, 4:1, and 6:1.

[0043] 2) Take 1.25 mmol of N'N-diphenylthiourea and disperse it in 1 mL of butylamine to obtain intermediate precursor II.

[0044] 3) Precursor II (1.25 mmol N'N-diphenylthiourea dissolved in butylamine) was mixed with reaction precursor I with different Ag-Bi:CBT ratios and allowed to react for 20 minutes before cooling to room temperature.

[0045] 4) Using methyl acetate as an anti-solvent, the nanocrystals are precipitated from the reaction mother liquor in a volume ratio of 1:6 between the nanocrystal mother liquor and methyl acetate, and the AgBiS2 nanocrystal powder is obtained by drying.

[0046] See attached Figure 5 , are the corresponding EDS spectra obtained in this embodiment using different Ag-Bi:CBT ratios (1:1, 2:1, 3:1, 4:1, 6:1). Embodiment 4

[0047] AgBiS2 nanocrystals are prepared by a direct synthesis method, which includes the following steps: mixing a metal precursor dissolved in a polar solvent and a sulfur source under the action of an organic amine, and inducing a reaction under different reaction times to generate stable colloidal AgBiS2 nanocrystals. 1) Dissolve AgI, BiI3 metal precursors and thiol molecules in a polar organic solvent to obtain a reaction precursor I. In this step, 2 mmol AgI, 0.5 mmol BiI3, and 1.25 mmol 4-chlorobenzenethiol are dissolved in the reaction precursor I organic solvent DMF (5 mL) at 100°C to obtain the reaction precursor I. Five samples of the reaction precursor I are prepared according to the above method.

[0048] 2) Disperse 1.25 mmol of N'N-diphenylthiourea in 1 mL of butylamine to obtain precursor II.

[0049] 3) Precursor II (N'N-diphenylthiourea dissolved in butylamine) was mixed with reaction precursor I respectively. The reaction time of each sample was 10min, 20min, 40min, 70min, and 150min respectively, and then cooled to room temperature.

[0050] 4) The nanocrystals in each sample were precipitated from the reaction mother liquor using methyl acetate anti-solvent at a volume ratio of 1:6 between the nanocrystal mother liquor and methyl acetate, and then dried to obtain AgBiS2 nanocrystal powder.

[0051] See attached Figure 6 , are TEM images of AgBiS2 nanocrystals prepared in this example using different reaction times. Embodiment 5

[0052] AgBiS2 nanocrystals are prepared by a direct synthesis method, and different Ag metal compounds (such as one or more of silver iodide, silver bromide AgBr, silver chloride AgCl, silver acetate AgAc, silver thiocyanate AgSCN, and silver nitrate AgNO3) and Bi metal compounds (such as one or more of bismuth iodide, bismuth bromide, bismuth chloride, bismuth acetate, and bismuth nitrate) are selected. The metal precursor dissolved in a polar solvent and the sulfur source under the action of an organic amine are mixed to initiate a reaction to generate stable colloidal AgBiS2 nanocrystals, which includes the following steps: 1) Dissolve the Ag / Bi metal precursor and the thiol molecule in a polar organic solvent to obtain a reaction precursor I. In this step, the reaction precursor I is prepared by dissolving 2 mmol of an Ag metal compound (AgI, AgBr, AgCl, AgSCN, AgAc, AgNO3, respectively, in this embodiment), 0.5 mmol of a Bi metal compound (BiI3, BiBr3, respectively, in this embodiment), and 1.25 mmol of 4-chlorothiophenol in an organic solvent DMF (5 mL), and dissolving at 100°C to obtain 7 portions of the reaction precursor I.

[0053] 2) Take 1.25 mmol of N'N-diphenylthiourea and disperse it in 1 mL of butylamine to obtain precursor II. A total of 7 parts were prepared.

[0054] 3) Precursor II (N'N-diphenylthiourea dissolved in butylamine) was mixed with the reaction precursor I sample, and the reaction was continued for 20 minutes before cooling to room temperature.

[0055] 4) The nanocrystals are precipitated from the reaction mother liquor using methyl acetate as an anti-solvent at a volume ratio of 1:6 between the nanocrystal mother liquor and methyl acetate, and then the AgBiS2 nanocrystal powder is obtained by drying.

[0056] See attached Figure 7 , which is the XRD pattern of AgBiS2 nanocrystals prepared by selecting different Ag / Bi metal precursors in this embodiment. Embodiment 6

[0057] AgBiS2 nanocrystals are prepared by a direct synthesis method, wherein a metal precursor dissolved in a polar solvent is mixed with a sulfur source under the action of an organic amine. In this embodiment, different thiol molecules are used, and the thiol molecules can be selected from one or more of 3-chloro-1-propanethiol, 4-chlorothiophenol, mercaptobenzoic acid, and mercaptoethanol, to initiate a reaction to generate stable colloidal AgBiS2 nanocrystals, comprising the following steps: 1) Dissolve AgI, BiI3 and thiol molecules in a polar organic solvent to obtain a reaction precursor I. In this step, 2 mmol AgI, 0.5 mmol BiI3, and 1.25 mmol thiol molecules (3-chloro-1-propanethiol in this embodiment) are dissolved in the reaction precursor I organic solvent DMF (5 mL) at 100°C to obtain 1 portion of reaction precursor I.

[0058] 2) Take 1.25 mmol of N'N-diphenylthiourea and disperse it in 1 mL of butylamine to obtain precursor II, and prepare 1 portion.

[0059] 3) Precursor II (N'N-diphenylthiourea dissolved in butylamine) was mixed with reaction precursor I and allowed to react for 20 minutes before cooling to room temperature.

[0060] 4) The nanocrystals are precipitated from the reaction mother liquor using methyl acetate as an anti-solvent at a volume ratio of 1:6 between the nanocrystal mother liquor and methyl acetate, and then the AgBiS2 nanocrystal powder is obtained by drying.

[0061] See attached Figure 8 , is the XRD pattern of AgBiS2 nanocrystals prepared in this embodiment using 3-chloro-1-propylsulfide as the thiol molecule. Embodiment 7

[0062] This embodiment provides an AgBiS2 nanocrystalline solar cell having a structure of ITO / SnO2 / AgBiS2 / PTAA / MoO3 / Ag.

[0063] The specific preparation method is: according to the technical scheme of Example 1, the molar ratio of AgI:BiI3 is 2:1, 3:1, 4:1, and 6:1 to prepare nanocrystals, and then dispersed in the polar solvent DMF to obtain 4 parts of stable colloidal nanocrystal ink.

[0064] Tin oxide (SnO2) nanoparticle solution, AgBiS2 nanocrystal ink, PTAA were spin-coated on the cleaned ITO conductive glass substrate, and then 3nm molybdenum trioxide and 120nm silver were evaporated.

[0065] The optimized mass volume concentration of AgBiS2 nanocrystal ink is 120 mg / ml, the optimized rotation speed is 2000 rpm, the duration is 45 seconds, and the annealing temperature and time of the nanocrystal film are annealing at 125°C for 5 minutes.

[0066] See attached Fig. 9 , are JV curves of solar cells prepared using nanocrystals with AgI:BiI3 precursor feed molar ratios of 2:1, 3:1, 4:1, and 6:1 as the photoactive layer in this embodiment. Embodiment 8

[0067] This embodiment provides a method for directly synthesizing and preparing AgBiS2 nanocrystals in batches.

[0068] AgBiS2 nanocrystals are prepared by a direct synthesis method, which includes the following steps: mixing a metal precursor dissolved in a polar solvent with a sulfur source under the action of an organic amine to initiate a reaction to generate stable colloidal AgBiS2 nanocrystals: 1) Dissolve AgI, BiI3 and thiol molecules in a polar organic solvent to obtain a reaction precursor I. The feed of the reaction precursor I is as follows: 80 mmol AgI, 20 mmol BiI3 and 50 mmol 4-chlorothiophenol are dissolved in 150 mL DMF, and the reaction precursor I is obtained by dissolving at 100°C.

[0069] 2) Disperse 50 mmol of N'N-diphenylthiourea in 30 mL of butylamine to obtain precursor II.

[0070] 3) Inject precursor II (N'N-diphenylthiourea dissolved in butylamine) into the reaction precursor I, react at 100°C for 20 minutes and then cool to room temperature.

[0071] 4) The nanocrystals were precipitated from the reaction mother liquor using methyl acetate as an anti-solvent at a volume ratio of 1:6 between the nanocrystal mother liquor and methyl acetate, and then the nanocrystals were dried to obtain 10.46 g of AgBiS2 nanocrystal powder.

[0072] Compared with other embodiments, this embodiment simultaneously increases the feed ratio of the reaction process by nearly forty times, and can obtain more than 10g of AgBiS2 nanocrystalline powder in one preparation, thus realizing batch preparation.

[0073] See attached Fig.11 , is the XRD diagram of AgBiS2 nanocrystals prepared in batches in this embodiment.

Claims

1. A method for preparing AgBiS2 nanocrystalline ink, characterized in that The steps include: 1) dissolving a Ag / Bi metal precursor and a thiol molecule in a polar organic solvent to obtain a reaction precursor; the molar ratio of the Ag / Bi metal precursor to the thiol molecule is 1:1 to 6:1; the Ag / Bi metal precursor comprises an Ag metal compound and a Bi metal compound, and the molar ratio of Ag to Bi element is 1:1 to 10:1; 2) Mixing the sulfur source, the organic amine and the reaction precursor, reacting for 1 to 150 minutes at a temperature of -20°C to 150°C to obtain a mother solution of AgBiS2 nanocrystals; 3) adding an anti-solvent to the obtained AgBiS2 nanocrystal mother liquor, and performing precipitation and drying treatment to obtain AgBiS2 nanocrystal powder; 5) Dispersing the nanocrystalline powder in a solvent to obtain nanocrystalline ink with continuously adjustable AgBiS2 concentration.

2. The method for preparing AgBiS2 nanocrystalline ink according to claim 1, characterized in that: The dielectric constant of the polar organic solvent is 20-90, and the range of the solvent donor number is 14-18 kcal / mol.

3. The method for preparing AgBiS2 nanocrystalline ink according to claim 1, characterized in that: The Ag metal compound includes silver iodide, silver bromide, silver chloride, silver acetate, silver thiocyanate, and silver nitrate; the Bi metal compound includes bismuth iodide, bismuth bromide, bismuth chloride, bismuth acetate, bismuth nitrate, and triphenyl bismuth.

4. The method for preparing AgBiS2 nanocrystalline ink according to claim 1, characterized in that: The thiol molecules include 3-chloro-1-propanethiol, 4-chlorothiophenol, mercaptobenzoic acid, mercaptoethanol, furfuryl mercaptan, 1,4-phenyldithiol, 3-aminothiophenol, 4-aminothiophenol, 4-(trifluoromethyl)thiophenol, 1,2-ethanedithiol, and o-phenylthiol.

5. The method for preparing AgBiS2 nanocrystalline ink according to claim 1, characterized in that: The anti-solvent includes anhydrous ethanol, isopropanol, methanol, methyl acetate, ethyl acetate, toluene, n-hexane, and n-octane; the solvent includes N,N-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, acetonitrile, butyronitrile, propylene carbonate, γ-valerolactone, water, and acetone.

6. The method for preparing a AgBiS2 nanocrystalline ink according to claim 1 or 2, characterized in that: The polar organic solvent includes N, N-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, butyronitrile, propylene carbonate, γ-valerolactone, and n-butylamine.

7. An AgBiS2 nanocrystalline ink obtained by the preparation method according to claim 1.

8. The use of the AgBiS2 nanocrystalline ink according to claim 7, characterized in that: The film is formed by spin coating, blade coating, dip coating and inkjet printing and is used as the photoactive layer of optoelectronic devices.

9. The use of an AgBiS2 nanocrystalline ink according to claim 8, characterized in that: The photoelectric device comprises a solar cell and a photoelectric detector.

10. The use of AgBiS2 nanocrystalline ink according to claim 9, characterized in that: The structure of the solar cell includes upright or inverted; the upright structure is conductive glass / electron transport layer / AgBiS2 absorption layer / hole transport layer / molybdenum trioxide / silver electrode in sequence, and the inverted structure is conductive glass / hole transport layer / AgBiS2 absorption layer / electron transport layer / silver electrode in sequence.

Citation Information

Patent Citations

  • Preparation method of AgBiS2 quantum dot superlattice and photoelectric detector thereof

    CN114774114A

  • Preparation method of ternary metal chalcogenide nanocrystalline

    CN115744976A

  • Method for low-temperature one-step synthesis of AgBiS2 nanocrystals

    CN115893488A

  • AgBiS2 quantum dot based on liquid-phase ligand exchange and preparation method of solar cell of AgBiS2 quantum dot