Method for controlling hydrogen content in high-strength steel rail steel
By optimizing the steel smelting process, including converter smelting, LF furnace refining, RH vacuum treatment, continuous casting and slow stacking cooling, combined with online baking, argon blowing treatment and tundish baking, the problem of controlling the hydrogen content of steel rails was solved, achieving stable control of hydrogen content and reducing production costs.
Patent Information
- Application Number
- CN202411041623.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
Existing technologies are insufficient to effectively control the hydrogen content in rails, leading to increased hydrogen embrittlement, which affects the safety and reliability of rails. Furthermore, existing processes and equipment are unable to meet stricter hydrogen content requirements, resulting in a high rate of product downgrading and reclassification.
By optimizing the steelmaking process, including converter smelting, LF furnace refining, RH vacuum treatment, continuous casting and slow cooling, combined with online baking, argon blowing and tundish baking, the hydrogen content of molten steel and tundish is controlled, and the composition of tundish materials is optimized to achieve stable control of hydrogen content.
It effectively reduced the fluctuation of hydrogen content during the steel smelting process, met the strict requirements of high-strength steel rails for hydrogen content, reduced the steel modification rate, and achieved a reduction in production costs.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steel smelting, and in particular relates to a method for controlling the hydrogen content in high-strength rail steel. Background Art
[0002] At present, the transportation steel industry has entered a critical period of quality improvement. As the basic supporting material for railway transportation, rails have developed from low strength, small cross-section, and light load to high speed, high strength, large cross-section, and heavy load. The sensitivity to defects such as cracks has increased significantly. Hydrogen in solid steel can easily lead to hydrogen-induced defects such as white spots and cracks, resulting in "hydrogen embrittlement", which has become the origin of defects such as cracks, greatly increasing the risk of brittle fracture of rails.
[0003] Domestic and foreign rail manufacturers mainly use vacuum dehydrogenation and slow cooling processes to reduce the internal hydrogen content of rails to achieve rail hydrogen ≤2.0ppm to ensure the rail's resistance to hydrogen embrittlement. However, during the laying and service of rails, rail head core damage and rail breakage accidents caused by hydrogen-induced cracks occur from time to time. As rails develop towards heavier, stronger, and purer steel, the requirements for rail hydrogen embrittlement resistance are further improved. Some manufacturers control rail hydrogen to ≤1.5ppm or even lower, but there is still a blank in the research on the critical hydrogen content of white spots in rails. The control of rail hydrogen content is more based on relevant rail production standards at home and abroad, and lacks theoretical guidance on the diffusion behavior of rail hydrogen. The increase in hydrogen content requirements will increase the dehydrogenation burden on the process and equipment. The current average vacuum dehydrogenation efficiency of rail production at home and abroad is 70%. By controlling the processing time, the hydrogen content after vacuum treatment can be 1.0-2.0ppm. Combined with the slow cooling process, the hydrogen content of the rail can be controlled at 1.0-2.0ppm. However, if the hydrogen content of the rail is controlled at ≤1.5ppm or even lower, the domestic and foreign rail production process and equipment capabilities will not be able to guarantee full satisfaction, and the product downgrade and re-judgment rate caused by excessive hydrogen content will increase significantly.
[0004] Therefore, in order to support the safety and reliability of the railway transportation industry and ensure the stability and controllability of hydrogen in the rail production process, it is particularly important to carry out research and application of key technologies for efficient and stable control of hydrogen in rail steel. Summary of the invention
[0005] In view of this, the object of the present invention is to provide a method for controlling the hydrogen content in high-strength rail steel, which can reduce the fluctuation of hydrogen content in the steelmaking process and meet the strict requirements of high-strength rails on hydrogen content, thereby further reducing the steel billet modification rate caused by hydrogen content fluctuations and achieving a reduction in production costs.
[0006] The present invention provides a method for controlling the hydrogen content in high-strength rail steel, comprising the following steps:
[0007] a) Converter smelting:
[0008] Steelmaking raw materials are smelted in the converter, and the alloys used in the smelting process are baked online before entering the converter;
[0009] b) LF furnace refining and RH vacuum treatment:
[0010] After the converter taps out steel, the molten steel is sent to the LF furnace for refining, and the refined molten steel is sent to the RH vacuum furnace for vacuum treatment. During the vacuum treatment, argon blowing is carried out throughout the process.
[0011] c) Continuous Casting:
[0012] The molten steel after vacuum treatment is sent to the continuous casting platform for casting; before continuous casting begins, the tundish for continuous casting is baked at a temperature of 100-1400°C for 4-5 hours; the tundish dry material used in continuous casting has a MgO content of ≥80wt%, a SiO2 content of ≤3wt%, an Al2O3 content of ≤3wt%, and a H2O content of ≤0.5wt%; during the continuous casting process, the tundish covering agent, carbonized rice husk and crystallizer protective slag used are baked before use at a temperature of 50-80°C for 36-48 hours; during the continuous casting process, the hydrogen content of the molten steel in the tundish is controlled at 0.88-0.93ppm;
[0013] d) Stacking slow cooling:
[0014] The ingots obtained by continuous casting are cut to length, then stacked and slowly cooled to obtain high-strength rail steel.
[0015] Preferably, in step a), the temperature of the online baking is 200-300° C.; and the time of the online baking is 0.5-1 h.
[0016] Preferably, in step b), the argon flow rate of the argon blowing treatment is 50 to 80 L / min.
[0017] Preferably, in step b), the vacuum treatment process specifically includes:
[0018] After the refined molten steel is fed into the RH vacuum furnace, the vacuum degree is drawn to the target value, and the furnace is treated at the target vacuum degree for a period of time. Argon blowing is performed throughout the vacuum treatment process. After the vacuum treatment is completed, the vacuum is broken, and then the argon blowing treatment is continued for a period of time.
[0019] Preferably, the target value of the vacuum degree is ≤1 mbar; and the time taken to draw the vacuum degree to the target value is ≤3 min.
[0020] Preferably, the treatment time at the target vacuum degree is 13 to 18 minutes.
[0021] Preferably, the argon flow rate of the continued argon blowing treatment is 120-150 L / min.
[0022] Preferably, the argon blowing treatment is continued for 8 to 10 minutes.
[0023] Preferably, in step d), the stacking temperature of the stacking slow cooling is 350-450°C.
[0024] Preferably, in step d), the slow cooling time of the stack is ≥ 32 h.
[0025] Compared with the prior art, the present invention provides a method for controlling the hydrogen content in high-strength rail steel, comprising the following steps: a) converter smelting: the steelmaking raw materials are smelted in the converter, and the alloy used in the smelting process is baked online before entering the converter; b) LF furnace refining and RH vacuum treatment: after the converter taps out steel, the molten steel is sent to the LF furnace for refining, and the refined molten steel is sent to the RH vacuum furnace for vacuum treatment; during the vacuum treatment, argon blowing treatment is performed throughout the process; c) continuous casting: the molten steel after vacuum treatment is sent to the continuous casting platform for casting; before the continuous casting starts, the continuous casting tundish is baked at a baking temperature of 100 to 1400°C , the baking time is 4 to 5 hours; the MgO content of the dry material of the tundish used in continuous casting is ≥80wt%, the SiO2 content is ≤3wt%, the Al2O3 content is ≤3wt%, and the H2O content is ≤0.5wt%; during the continuous casting process, the tundish covering agent, carbonized rice husk and crystallizer protective slag used are first baked before use, the baking temperature is 50 to 80°C, and the baking time is 36 to 48 hours; during the continuous casting process, the hydrogen content of the molten steel in the tundish is controlled at 0.88 to 0.93ppm; d) Stacking and slow cooling: the ingot obtained by continuous casting is cut to a fixed length, and then stacked and slowly cooled to obtain high-strength rail steel. The method provided by the present invention can effectively reduce the hydrogen content fluctuation in the steel smelting process by optimizing the process steps and process conditions of steel smelting, meet the strict requirements of high-strength rails on hydrogen content, thereby further reducing the steel billet modification rate caused by hydrogen content fluctuations, and achieving a reduction in production costs. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] The present invention provides a method for controlling the hydrogen content in high-strength rail steel, comprising the following steps:
[0028] a) Converter smelting: Steelmaking raw materials are smelted in a converter;
[0029] b) LF furnace refining and RH vacuum treatment: After the converter taps out, the molten steel is sent to the LF furnace for refining, and the refined molten steel is sent to the RH vacuum furnace for vacuum treatment;
[0030] c) Continuous casting: The molten steel after vacuum treatment is sent to the continuous casting platform for casting;
[0031] d) Stacking and slow cooling: The ingots obtained by continuous casting are cut to length and then stacked and slowly cooled to obtain high-strength rail steel.
[0032] In the method provided by the present invention, in step a), the alloy used in the smelting process is baked online before entering the converter, and molten steel is added during the converter tapping process; the online baking temperature is preferably 200-300°C, specifically 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C, 290°C or 300°C; the online baking time is preferably 0.5-1h, specifically 0.5h, 0.55h, 0.6h, 0.65h, 0.7h, 0.75h, 0.8h, 0.85h, 0.9h, 0.95h or 1h.
[0033] In the method provided by the present invention, in step b), LF refers to ladle furnace; RH refers to ruhstahl hausen process, which is a vacuum degassing method commonly used in steelmaking.
[0034] In the method provided by the present invention, in step b), the slag-melting time of LF refining is preferably ≥15 min; and the outlet temperature of the molten steel after LF refining is preferably controlled at 1550°C to 1570°C.
[0035] In the method provided by the present invention, in step b), argon blowing treatment is carried out throughout the vacuum treatment process; the argon gas flow rate of the argon blowing treatment is 50-80 L / min, specifically 50 L / min, 52 L / min, 55 L / min, 57 L / min, 60 L / min, 62 L / min, 65 L / min, 67 L / min, 70 L / min, 72 L / min, 75 L / min, 77 L / min or 80 L / min.
[0036] In the method provided by the present invention, in step b), the specific process of the vacuum treatment preferably includes: after the refined molten steel is fed into the RH vacuum furnace, the vacuum degree is pumped to the target value, and the treatment is carried out at the target vacuum degree for a period of time, and argon blowing treatment is carried out throughout the vacuum treatment process; after the vacuum treatment is completed, the vacuum is broken, and then the argon blowing treatment is continued for a period of time. Among them, the target value of the vacuum degree is preferably ≤1mbar, and can be specifically 0.1mbar, 0.2mbar, 0.3mbar, 0.4mbar, 0.5mbar, 0.6mbar, 0.7mbar, 0.8mbar, 0.9mbar or 1mbar; the time taken to pump the vacuum degree to the target value is preferably ≤3min, and can be specifically 1min, 1.5min, 2min, 2.5min or 3min; the treatment time at the target vacuum degree is preferably 13 to 18min, and can be specifically 13min, 13.5min, 14min. , 14.5min, 15min, 15.5min, 16min, 16.5min, 17min, 17.5min or 18min; the argon flow rate of the continued argon blowing treatment is preferably 120-150L / min, specifically 120L / min, 125L / min, 130L / min, 135L / min, 140L / min, 145L / min or 150L / min; the time of the continued argon blowing treatment is preferably 8-10min, specifically 8min, 8.5min, 9min, 9.5min or 10min.
[0037] In the method provided by the present invention, in step c), before continuous casting begins, the tundish for continuous casting is baked. The baking temperature is 100-1400°C, specifically 100°C, 200°C, 300°C, 400°C, 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C, 1100°C, 1200°C, 1300°C or 1400°C; the baking time is 4-5h, specifically 4h, 4.1h, 4.2h, 4.3h, 4.4h, 4.5h, 4.6h, 4.7h, 4.8h, 4.9h or 5h. In the specific embodiments provided by the present invention, the baking is preferably divided into three stages, wherein the baking temperature of the first stage is preferably 100-300°C, specifically 200°C, and the baking time of the first stage is preferably 1-1.25h; the baking temperature of the second stage is preferably 400-600°C, specifically 500°C, and the baking time of the second stage is preferably 2-2.5h; the baking temperature of the third stage is preferably 1000-1200°C, specifically 1100°C, and the baking time of the third stage is preferably 1-1.25h.
[0038] In the method provided by the present invention, in step c), the MgO content of the dry material in the tundish used for continuous casting is ≥80wt%, specifically 80wt%, 81wt%, 82wt%, 83wt%, 84wt%, 85wt%; the SiO2 content of the dry material in the tundish used is ≤3wt%, specifically 2wt%, 2.1wt%, 2.2wt%, 2.3wt%, 2.4wt%, 2.5wt%, 2.6wt%, 2.7wt%, 2.8wt%, 2.9wt% or 3wt%; the dry material in the tundish used is ≤3wt%, specifically 2wt%, 2.1wt%, 2.2wt%, 2.3wt%, 2.4wt%, 2.5wt%, 2.6wt%, 2.7wt%, 2.8wt%, 2.9wt% or 3wt%; The Al2O3 content is ≤3wt%, specifically 2wt%, 2.1wt%, 2.2wt%, 2.3wt%, 2.4wt%, 2.5wt%, 2.6wt%, 2.7wt%, 2.8wt%, 2.9wt% or 3wt%; the H2O content of the dry material in the tundish is ≤0.5wt%, specifically 0.05wt%, 0.1wt%, 0.15wt%, 0.2wt%, 0.25wt%, 0.3wt%, 0.35wt%, 0.4wt%, 0.45wt% or 0.5wt%.
[0039] In the method provided by the present invention, in step c), the tundish covering agent, carbonized rice husk and mold protection slag used in the continuous casting process are first baked before use. The baking temperature is 50-80°C, specifically 50°C, 52°C, 55°C, 57°C, 60°C, 62°C, 65°C, 67°C, 70°C, 72°C, 75°C, 77°C or 80°C; the baking time is 36-48h, specifically 36h, 37h, 38h, 39h, 40h, 41h, 42h, 43h, 44h, 45h, 46h, 47h or 48h.
[0040] In the method provided by the present invention, in step c), during the continuous casting process, the hydrogen content of the molten steel in the tundish is controlled at 0.88-0.93 ppm, specifically 0.88 ppm, 0.89 ppm, 0.9 ppm, 0.91 ppm, 0.92 ppm or 0.93 ppm.
[0041] In the method provided by the present invention, in step d), the stacking temperature of the stack slow cooling is preferably 350-450°C, specifically 350°C, 360°C, 370°C, 380°C, 390°C, 400°C, 410°C, 420°C, 430°C, 440°C or 450°C; the slow cooling time of the stack slow cooling is preferably ≥32h, more preferably 32-48h, specifically 32h, 34h, 36h, 38h, 40h, 42h, 44h, 46h or 48h.
[0042] The method provided by the present invention can effectively reduce the fluctuation of hydrogen content in the steelmaking process by optimizing the process steps and process conditions of steelmaking, meet the strict requirements of high-strength rails on hydrogen content, thereby further reducing the steel billet modification rate caused by hydrogen content fluctuations and achieving a reduction in production costs.
[0043] For the purpose of greater clarity, the present invention is described in detail with reference to the following examples and comparative examples.
[0044] Example 1
[0045] For a 120t ladle, when producing heavy rail steel, the process steps are:
[0046] (1) Steelmaking raw materials are smelted in a converter; the alloy used in the smelting process is baked online in the silo before entering the converter. The baking temperature is 200°C and the baking time is 1 hour. After the baking is completed, molten steel is added during the converter tapping process.
[0047] (2) After the converter is tapped, the molten steel is sent to the LF furnace for refining. The LF refining slag-removing time is ≥15min, and the temperature of the molten steel out of the LF refining station is controlled at 1550℃~1570℃; the refined molten steel is sent to the RH vacuum furnace for vacuum treatment; after the molten steel enters the vacuum furnace, it takes 2min to draw the vacuum degree to 1.0mbar, and maintain the vacuum degree of 0.8mbar for 13min. During the vacuum treatment process, argon blowing is carried out throughout the process, and the argon flow rate is controlled at 80L / min; after the vacuum treatment is completed, the vacuum is broken, and then the argon flow rate is adjusted to 150L / min, and the argon blowing treatment is continued for 10min.
[0048] (3) The molten steel after vacuum treatment is sent to the continuous casting platform for casting; before the continuous casting starts, the continuous casting tundish is baked, and the baking system is divided into three stages: the baking temperature of the first stage is 200°C and the baking time is 1h, the baking temperature of the second stage is 500°C and the baking time is 2h, and the baking temperature of the third stage is 1100°C and the baking time is 1h; the tundish dry material used has a MgO content of 80wt%, a SiO2 content of 3wt%, an Al2O3 content of 3wt%, and a H2O content of 0.5wt%; during the continuous casting process, the tundish covering agent, carbonized rice husk and crystallizer protective slag used are baked before use, and the baking temperature is controlled at 50°C and the baking time is controlled at 36h; during the continuous casting process, an automatic hydrogen determination instrument is used for online hydrogen determination, and the hydrogen content of the molten steel in the tundish is 0.93ppm.
[0049] (4) The ingots were cut to size and then stacked. The stacking temperature was controlled at 350°C and the stacking slow cooling time was 32 hours. The hydrogen content of the obtained high-strength rail ingots was 0.83 ppm.
[0050] Example 2
[0051] For a 120t ladle, when producing heavy rail steel, the process steps are:
[0052] (1) Steelmaking raw materials are smelted in a converter; the alloy used in the smelting process is baked online in the silo before entering the converter. The baking temperature is 200°C and the baking time is 1 hour. After the baking is completed, molten steel is added during the converter tapping process.
[0053] (2) After the converter is tapped, the molten steel is sent to the LF furnace for refining. The LF refining slag-removing time is ≥15min, and the temperature of the molten steel out of the LF refining station is controlled at 1550℃~1570℃; the refined molten steel is sent to the RH vacuum furnace for vacuum treatment; after the molten steel enters the vacuum furnace, it takes 2.5min to draw the vacuum degree to 0.8mbar, and maintain the vacuum degree of 0.8mbar for 15min. During the vacuum treatment process, argon blowing is carried out throughout the process, and the argon flow rate is controlled at 65L / min; after the vacuum treatment is completed, the vacuum is broken, and then the argon flow rate is adjusted to 130L / min, and the argon blowing treatment is continued for 9min.
[0054] (3) The molten steel after vacuum treatment is sent to the continuous casting platform for casting; before the continuous casting starts, the continuous casting tundish is baked, and the baking system is divided into three stages: the baking temperature of the first stage is 200°C and the baking time is 1h, the baking temperature of the second stage is 500°C and the baking time is 2h, and the baking temperature of the third stage is 1100°C and the baking time is 1h; the tundish dry material used has a MgO content of 82wt%, a SiO2 content of 2.8wt%, an Al2O3 content of 2.5wt%, and a H2O content of 0.5wt%; during the continuous casting process, the tundish covering agent, carbonized rice husk and crystallizer protective slag used are baked before use, and the baking temperature is controlled at 60°C and the baking time is controlled at 38h; during the continuous casting process, an automatic hydrogen determination instrument is used for online hydrogen determination, and the hydrogen content of the molten steel in the tundish is 0.91ppm.
[0055] (4) The ingots were cut to size and then stacked. The stacking temperature was controlled at 350°C and the stacking slow cooling time was 32 hours. The hydrogen content of the obtained high-strength rail ingots was 0.80 ppm.
[0056] Example 3
[0057] For a 120t ladle, when producing heavy rail steel, the process steps are:
[0058] (1) Steelmaking raw materials are smelted in a converter; the alloy used in the smelting process is baked online in the silo before entering the converter. The baking temperature is 250°C and the baking time is 1 hour. After the baking is completed, molten steel is added during the converter tapping process.
[0059] (2) After the converter is tapped, the molten steel is sent to the LF furnace for refining. The LF refining slag-removing time is ≥15min, and the temperature of the molten steel out of the LF refining station is controlled at 1550℃~1570℃; the refined molten steel is sent to the RH vacuum furnace for vacuum treatment; after the molten steel enters the vacuum furnace, it takes 3min to draw the vacuum degree to 0.7mbar, and maintain the vacuum degree of 0.7mbar for 18min. During the vacuum treatment process, argon blowing is carried out throughout the process, and the argon flow rate is controlled at 50L / min; after the vacuum treatment is completed, the vacuum is broken, and then the argon flow rate is adjusted to 120L / min, and the argon blowing treatment is continued for 8min.
[0060] (3) The molten steel after vacuum treatment is sent to the continuous casting platform for casting; before the continuous casting starts, the continuous casting tundish is baked, and the baking system is divided into three stages: the baking temperature of the first stage is 200°C and the baking time is 1h, the baking temperature of the second stage is 500°C and the baking time is 2h, and the baking temperature of the third stage is 1100°C and the baking time is 1h; the tundish dry material used has a MgO content of 82wt%, a SiO2 content of 2.8wt%, an Al2O3 content of 2.5wt%, and a H2O content of 0.5wt%; during the continuous casting process, the tundish covering agent, carbonized rice husk and crystallizer protective slag used are baked before use, and the baking temperature is controlled at 60°C and the baking time is controlled at 38h; during the continuous casting process, an automatic hydrogen determination instrument is used for online hydrogen determination, and the hydrogen content of the molten steel in the tundish is 0.89ppm.
[0061] (4) The ingots were cut to size and then stacked. The stacking temperature was controlled at 350°C and the stacking slow cooling time was 32 hours. The hydrogen content of the obtained high-strength rail ingots was 0.78 ppm.
[0062] Comparative Example 1
[0063] For a 120t ladle, when producing heavy rail steel, the process steps are:
[0064] (1) Steelmaking raw materials are smelted in a converter; the alloys used in the smelting process are not baked online before entering the converter.
[0065] (2) After the converter is tapped, the molten steel is sent to the LF furnace for refining. The LF refining slag-removing time is ≥15min, and the temperature of the molten steel out of the LF refining station is controlled at 1550℃~1570℃; the refined molten steel is sent to the RH vacuum furnace for vacuum treatment; after the molten steel enters the vacuum furnace, it takes 2min to draw the vacuum degree to 1.0mbar, and maintain the vacuum degree of 0.8mbar for 13min. During the vacuum treatment process, argon blowing is carried out throughout the process, and the argon flow rate is controlled at 80L / min; after the vacuum treatment is completed, the vacuum is broken, and then the argon flow rate is adjusted to 150L / min, and the argon blowing treatment is continued for 10min.
[0066] (3) The molten steel after vacuum treatment is sent to the continuous casting platform for casting; before the continuous casting starts, the continuous casting tundish is baked, and the baking system is divided into three stages: the baking temperature of the first stage is 200°C and the baking time is 1h, the baking temperature of the second stage is 500°C and the baking time is 2h, and the baking temperature of the third stage is 1100°C and the baking time is 1h; the tundish dry material used has an MgO content of 80wt%, an SiO2 content of 3wt%, an Al2O3 content of 3wt%, and an H2O content of 0.5wt%; during the continuous casting process, the tundish covering agent, carbonized rice husk and crystallizer protective slag used are baked before use, and the baking temperature is controlled at 50°C and the baking time is controlled at 36h; during the continuous casting process, an automatic hydrogen determination instrument is used for online hydrogen determination, and the hydrogen content of the molten steel in the tundish is 1.09ppm.
[0067] (4) The ingots were cut to size and then stacked. The stacking temperature was controlled at 350°C and the stacking slow cooling time was 32 hours. The hydrogen content of the obtained high-strength rail ingots was 1.01 ppm.
[0068] Comparative Example 2
[0069] For a 120t ladle, when producing heavy rail steel, the process steps are:
[0070] (1) Steelmaking raw materials are smelted in a converter; the alloy used in the smelting process is baked online in the silo before entering the converter. The baking temperature is 200°C and the baking time is 1 hour. After the baking is completed, molten steel is added during the converter tapping process.
[0071] (2) After the converter is tapped, the molten steel is sent to the LF furnace for refining. The LF refining slag-making time is ≥15min, and the temperature of the molten steel out of the LF refining station is controlled at 1550℃~1570℃; the refined molten steel is sent to the RH vacuum furnace for vacuum treatment; after the molten steel enters the vacuum furnace, it takes 2min to draw the vacuum degree to 1.0mbar, and maintain the vacuum degree of 0.8mbar for 13min. No argon blowing is performed during the vacuum treatment process; after the vacuum treatment is completed, the vacuum is broken, and then the argon flow rate is adjusted to 150L / min, and the argon blowing treatment is continued for 10min.
[0072] (3) The molten steel after vacuum treatment is sent to the continuous casting platform for casting; before the continuous casting starts, the continuous casting tundish is baked, and the baking system is divided into three stages: the baking temperature of the first stage is 200°C and the baking time is 1h, the baking temperature of the second stage is 500°C and the baking time is 2h, and the baking temperature of the third stage is 1100°C and the baking time is 1h; the tundish dry material used has a MgO content of 80wt%, a SiO2 content of 3wt%, an Al2O3 content of 3wt%, and a H2O content of 0.5wt%; during the continuous casting process, the tundish covering agent, carbonized rice husk and crystallizer protective slag used are baked before use, and the baking temperature is controlled at 50°C and the baking time is controlled at 36h; during the continuous casting process, an automatic hydrogen determination instrument is used for online hydrogen determination, and the hydrogen content of the molten steel in the tundish is 1.06ppm.
[0073] (4) The ingots were cut to size and then stacked. The stacking temperature was controlled at 350°C and the stacking slow cooling time was 32 hours. The hydrogen content of the obtained high-strength rail ingots was 0.99 ppm.
[0074] Comparative Example 3
[0075] For a 120t ladle, when producing heavy rail steel, the process steps are:
[0076] (1) Steelmaking raw materials are smelted in a converter; the alloy used in the smelting process is baked online in the silo before entering the converter. The baking temperature is 200°C and the baking time is 1 hour. After the baking is completed, molten steel is added during the converter tapping process.
[0077] (2) After the converter is tapped, the molten steel is sent to the LF furnace for refining. The LF refining slag-removing time is ≥15min, and the temperature of the molten steel out of the LF refining station is controlled at 1550℃~1570℃; the refined molten steel is sent to the RH vacuum furnace for vacuum treatment; after the molten steel enters the vacuum furnace, it takes 2min to draw the vacuum degree to 1.0mbar, and maintain the vacuum degree of 0.8mbar for 13min. During the vacuum treatment process, argon blowing is carried out throughout the process, and the argon flow rate is controlled at 80L / min; after the vacuum treatment is completed, the vacuum is broken, and then the argon flow rate is adjusted to 150L / min, and the argon blowing treatment is continued for 10min.
[0078] (3) The molten steel after vacuum treatment is sent to the continuous casting platform for casting; before the continuous casting starts, the continuous casting tundish is baked, and the baking system is divided into three stages: the baking temperature of the first stage is 200°C and the baking time is 0.5h, the baking temperature of the second stage is 500°C and the baking time is 1h, and the baking temperature of the third stage is 1100°C and the baking time is 0.5h; the tundish dry material used has a MgO content of 80wt%, a SiO2 content of 3wt%, an Al2O3 content of 3wt%, and a H2O content of 0.5wt%; during the continuous casting process, the tundish covering agent, carbonized rice husk and crystallizer protective slag used are baked before use, and the baking temperature is controlled at 50°C and the baking time is controlled at 18h; during the continuous casting process, an automatic hydrogen determination instrument is used for online hydrogen determination, and the hydrogen content of the molten steel in the tundish is 1.18ppm.
[0079] (4) The ingots were cut to size and then stacked. The stacking temperature was controlled at 350°C and the stacking slow cooling time was 32 hours. The hydrogen content of the obtained high-strength rail ingots was 1.07 ppm.
[0080] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for controlling the hydrogen content in high-strength rail steel, characterized in that: The following steps are involved: a) Converter smelting: Steelmaking raw materials are smelted in the converter, and the alloys used in the smelting process are baked online before entering the converter; b) LF furnace refining and RH vacuum treatment: After the converter taps out steel, the molten steel is sent to the LF furnace for refining, and the refined molten steel is sent to the RH vacuum furnace for vacuum treatment. During the vacuum treatment, argon blowing is carried out throughout the process. c) Continuous Casting: The molten steel after vacuum treatment is sent to the continuous casting platform for casting; before continuous casting begins, the tundish for continuous casting is baked at a temperature of 100-1400°C for 4-5 hours; the tundish dry material used in continuous casting has a MgO content of ≥80wt%, a SiO2 content of ≤3wt%, an Al2O3 content of ≤3wt%, and a H2O content of ≤0.5wt%; during the continuous casting process, the tundish covering agent, carbonized rice husk and crystallizer protective slag used are baked before use at a temperature of 50-80°C for 36-48 hours; during the continuous casting process, the hydrogen content of the molten steel in the tundish is controlled at 0.88-0.93ppm; d) Stacking slow cooling: The ingots obtained by continuous casting are cut to length, then stacked and slowly cooled to obtain high-strength rail steel.
2. The method according to claim 1, characterized in that In step a), the temperature of the online baking is 200-300° C.; the time of the online baking is 0.5-1 hour.
3. The method according to claim 1, characterized in that In step b), the argon flow rate of the argon blowing treatment is 50 to 80 L / min.
4. The method according to claim 1, characterized in that: In step b), the vacuum treatment process specifically includes: After the refined molten steel is fed into the RH vacuum furnace, the vacuum degree is drawn to the target value, and the furnace is treated at the target vacuum degree for a period of time. Argon blowing is performed throughout the vacuum treatment process. After the vacuum treatment is completed, the vacuum is broken, and then the argon blowing treatment is continued for a period of time.
5. The method according to claim 4, characterized in that The target value of the vacuum degree is ≤1 mbar; and the time taken to draw the vacuum degree to the target value is ≤3 min.
6. The method according to claim 4, characterized in that The treatment time at the target vacuum degree is 13 to 18 minutes.
7. The method according to claim 4, characterized in that The argon flow rate of the continued argon blowing treatment is 120-150 L / min.
8. The method according to claim 4, characterized in that The time for continuing the argon blowing treatment is 8 to 10 minutes.
9. The method according to claim 1, characterized in that: In step d), the stacking temperature of the stacking slow cooling is 350-450°C.
10. The method according to claim 1, characterized in that In step d), the slow cooling time of the stack is ≥ 32 h.