CrmN / TixAlyN / AlaCrbSicVdNe nano-composite coating, preparation method thereof and tool comprising CrmN / TixAlyN / AlaCrbSicVdNe nano-composite coating

Through the CrmN/TixAlyN/AlaCrbSicVdNe nanocomposite coating structure, the problems of insufficient binding force and thermal stability of the existing CrN/TiAlN/AlCrSiVN composite coating in high temperature environment are solved, and high hardness, wear resistance and lubricating performance are achieved. Comprehensive lift, suitable for high-temperature cutting tools.

CN118979228APending Publication Date: 2024-11-19TARFILM HI-TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411073253.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing CrN/TiAlN/AlCrSiVN composite coating has excellent performance in hardness, wear resistance and thermal stability, but its binding force with the substrate is low, unable to work for a long time in a high temperature environment, and insufficient thermal stability.

Method used

The CrmN/TixAlyN/AlaCrbSicVdNe nanocomposite coating structure is adopted, which includes a CrmN transition layer and a TixAlyN/AlaCrbSicVdNe composite multilayer with a periodic structure. The composition and structure of the coating are optimized through arc ion plating technology to improve hardness and bonding. Force and lubrication performance.

Benefits of technology

It achieves excellent hardness, bonding and toughness in high temperature environments, while taking into account lubricating performance, improving the thermal stability and anti-friction and wear performance of the coating, reducing the wear rate, and replacing the effect of some lubricating fluid, reducing the Pollution and environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979228A_ABST
    Figure CN118979228A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of physical vapor deposition nano composite coatings. In particular to a CrmN / TixAlyN / AlaCrbSicVdNe nano composite coating and a preparation method of the CrmN / TixAlyN / AlaCrbSicVdNe nano composite coating. The invention further relates to a tool comprising the CrmN / Ti < x > Al < y > N / Al Cr SicV < d > N < e > nano composite coating. According to the CrmN / TixAlyN / AlaCrbSicVdNe nano-composite coating prepared by the method disclosed by the invention, the characteristics of high wear resistance and thermal stability of the AlaCrbSicVdNe layer, excellent hardness and toughness of the TixAlyN layer, high adhesive force of the CrmN transition layer and the like are comprehensively utilized; therefore, the nano-composite coating disclosed by the invention has excellent lubricating property while having relatively good comprehensive mechanical properties such as hardness, binding force and toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of physical vapor deposition nanocomposite coatings. Specifically, the present invention relates to Cr m N / Ti x Al y N / A a Cr b Si c V d N e The present invention also relates to a nanocomposite coating and a preparation method thereof. m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coatings for tools. Background Art

[0002] With the rapid development of modern manufacturing industry, hard coating has been paid much attention as an important research direction of materials science, and is widely used in the fields of machinery, medicine, textile, microelectronics and aviation. Hard coating is a layer or layers of coating with a thickness of several microns deposited on a substrate. Under the condition that the substrate remains unchanged, hard coating can make the parts coated with it have better performance and longer service life. For example, cutting tools will have improved cutting performance after depositing a hard film layer. In addition to improving the cutting quality of cutting tools and greatly reducing their processing costs, hard coating can also greatly improve their hardness and toughness.

[0003] Cutting tool coating technology has evolved over time and can be divided into multi-component coatings, gradient coatings, nano-composite coatings, nano-multilayer coatings, etc. The various properties of the coatings have also been steadily improved and can be applied in various cutting processing environments.

[0004] Cutting tool coatings can generally be deposited using physical vapor deposition technology. Physical vapor deposition technology is now quite mature, mainly including the process of using a large current to evaporate the target material or bombarding the target surface with additional particles so that the target particles are sputtered onto the substrate surface to achieve deposition. Physical vapor deposition technology mainly includes evaporation, magnetron sputtering (MS), arc ion plating (AIP) and electron beam physical vapor deposition technology.

[0005] The AlCrSiTiN coating containing elements of aluminum (Al), chromium (Cr), silicon (Si), titanium (Ti) and nitrogen (N) can be formed by the physical vapor deposition technology, and the coating is one of the coatings with various excellent mechanical properties. Replacing the Ti element in the AlCrSiTiN coating with the vanadium (V) element can form a small amount of vanadium-containing nitride, thereby increasing the hardness, toughness and friction resistance of the coating.

[0006] Composite coating structures have been proven to effectively improve the performance of coatings, such as TiAlN / AlCrN, AlCrSiN / AlCrN composite coatings disclosed in the prior art. AlCrN coatings prepared by cathodic arc ion plating technology have the advantages of high hardness and strong toughness, but their thermal stability is poor and they cannot work for a long time in an environment above 800°C.

[0007] AlCrSiVN coating is currently a coating with excellent hardness, wear resistance, thermal stability and other aspects, but its bonding strength with the substrate is low; TiAlN, as a transition layer of many nitride coatings, has good bonding strength between coatings, excellent hardness and toughness; and CrN coating has high adhesion. Their combination may bring about a coating with higher comprehensive performance.

[0008] However, the comprehensive performance of the CrN / TiAlN / AlCrSiVN composite coating structure still needs to be further optimized. Summary of the invention

[0009] Purpose of the Invention

[0010] In view of the problems existing in the prior art described in the above background technology part, the object of the present invention is to provide a Cr m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coating and preparation method thereof. In addition, the present invention also aims to provide a nanocomposite coating comprising the Cr m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coatings for tools.

[0011] Technical Solution

[0012] In order to achieve the above-mentioned purpose of the present invention, the present invention provides the following technical solutions

[0013] Scheme 1: A Cr bonded to the substrate surface m N / Ti x Al y N / A a Cr b Si c V d N e The nanocomposite coating comprises Cr deposited on the surface of the substrate. m N transition layer, and deposited on the Cr m Ti with one or more periodic structures on the surface of the N transition layer x Al y N / A a Cr b Si c V d N e Composite multilayer, wherein the Ti x Al y N / A a Cr b Si c V d N e One period of the composite multilayer contains the inner layer of Ti x Al y N layer and outer Al a Cr b Si c V d N e layer,

[0014] in

[0015] m is from about 0.99 to about 1.01;

[0016] x is from about 0.29 to about 0.31, y is from about 0.69 to about 0.71, and the sum of x+y is about 1;

[0017] a is from about 0.20 to about 0.25; b is from about 0.13 to about 0.17; c is from about 0.05 to about 0.10; d is from about 0.05 to about 0.10, e is from about 0.40 to about 0.50, and the sum of a+b+c+d+e is about 1.

[0018] Scheme 2: Cr according to Scheme 1 above m N / Ti x Al y N / A a Cr b Si c Vd N e Nanocomposite coating, wherein the Cr m The thickness of the N transition layer is in the range of about 0.4 to about 0.6 μm.

[0019] Scheme 3: Cr according to Scheme 1 or 2 above m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coating, wherein the Ti x Al y N / A a Cr b Si c V d N e The total thickness of one period of the composite multilayer is in the range of about 0.9 to about 1.1 μm.

[0020] Scheme 4: Cr according to any one of Schemes 1 to 3 above m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coating, wherein the Ti x Al y The thickness of the N layer is in the range of about 0.4 to about 0.6 μm.

[0021] Scheme 5: Cr according to any one of Schemes 1 to 3 above m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coating, wherein the Al a Cr b Si c V d N e The thickness of the layer is in the range of about 0.4 to about 0.6 μm.

[0022] Scheme 6: Cr according to any one of Schemes 1 to 5 above m N / Ti x Al y N / A a Crb Si c V d N e The nanocomposite coating, wherein the substrate is selected from any one of cemented carbide, high-speed steel and corundum.

[0023] Scheme 7: Cr according to any one of Schemes 1 to 6 above m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coating, wherein the Ti having a periodic structure x Al y N / A a Cr b Si c V d N e The number of periods of the composite multilayer is 1, 2, 3 or 4.

[0024] Scheme 8: Cr according to any one of Schemes 1 to 7 m N / Ti x Al y N / A a Cr b Si c V d N e The nanocomposite coating comprises AlN, CrN, VN phases with a face-centered cubic structure, an AlN phase with a close-packed hexagonal structure, and an amorphous phase of Si nitride.

[0025] Scheme 9: Cr according to any one of Schemes 1 to 8 above m N / Ti x Al y N / A a Cr b Si c V d N e A nanocomposite coating, wherein the nanocomposite coating has one or more of the following properties:

[0026] The hardness is in the range of about 29.4 ± about 1.5 GPa,

[0027] The elastic modulus is in the range of about 384.4 ± about 12.3 GPa,

[0028] The bonding force reaches about 54N or more.

[0029] The hardness / elastic modulus ratio reaches above about 0.0765, and

[0030] The coefficient of friction is less than about 0.6, preferably less than about 0.56.

[0031] Scheme 10: A method for preparing Cr according to any one of the above schemes 1 to 9 m N / Ti x Al y N / A a Cr b Si c V d N e A method for nanocomposite coating, wherein the method comprises the following steps:

[0032] Step 1: Depositing the Cr on the substrate surface by arc ion plating m N transition layer; and

[0033] Step 2: In the Cr m The Ti x Al y The N layer and the Al a Cr b Si c V d N e layer.

[0034] Scheme 11: The preparation method according to Scheme 10, wherein the method further comprises step 3: in the Al obtained in step 2 a Cr b Si c V d N e The Ti layer is further deposited on the surface by arc ion plating. x Al y The N layer and the Al a Cr b Si c V d N e Layer one or more times.

[0035] Scheme 12: A preparation method according to any one of schemes 10 to 11 above, wherein the deposited Cr m The N transition layer process includes:

[0036] In the case of continuously introducing nitrogen gas at a flow rate of about 600 to about 800 sccm into an arc ion plating deposition chamber under a nitrogen atmosphere, the pressure in the deposition chamber is controlled to be about 0.8 to about 1.1 Pa, the temperature is controlled to be about 460 to about 490° C., and the temperature of the substrate in the deposition chamber is controlled to be about 470 to about 500° C., and the Cr target is turned on to perform the arc ion plating deposition for about 25 to about 35 minutes to form the Cr m N transition layer, wherein the target current of the Cr target is set to about 80 to about 100 A, the bias voltage of the Cr target is set to about -80 to about -120 V, and the distance between the Cr target and the substrate is set to about 24 to about 26 cm.

[0037] Scheme 13: A preparation method according to any one of schemes 10 to 12 above, wherein the deposited Ti x Al y The N-layer process includes:

[0038] In the case of continuously introducing nitrogen gas with a flow rate of about 600 to about 800 sccm into the arc ion plating deposition chamber under a nitrogen atmosphere, the pressure in the deposition chamber is controlled to be about 0.8 to about 1.1 Pa, the temperature is controlled to be about 460 to about 490° C., and the Cr-containing gas in the deposition chamber is controlled to be about 0.8 to about 1.1 Pa. m The temperature of the substrate of the N transition layer is about 470 to about 500° C., and the TiAl target is turned on to perform the arc ion plating deposition for about 55 to about 65 minutes to form the TiAl transition layer. x Al y N layer, wherein the atomic ratio of Ti:Al in the TiAl target is about (32-34):(66-68), the target current of the TiAl target is set to about 90 to about 110A, the bias voltage of the TiAl target is set to about -80 to about -120V, and the distance between the TiAl target and the substrate is set to about 24 to about 26cm.

[0039] Scheme 14: A preparation method according to any one of schemes 10 to 13 above, wherein the deposited Al a Cr b Si c V d N e The layer process includes:

[0040] In the case of continuously introducing nitrogen gas with a flow rate of about 600 to about 800 sccm into the arc ion plating deposition chamber under a nitrogen atmosphere, the pressure in the deposition chamber is controlled to be about 0.8 to about 1.1 Pa, the temperature is controlled to be about 460 to about 490° C., and the Cr-containing gas in the deposition chamber is controlled to be about 0.8 to about 1.1 Pa. m N transition layer and the Ti x Al yThe temperature of the substrate of the N layer is about 470 to about 500° C., and the AlCrSi target and the V target are simultaneously turned on to perform the arc ion plating deposition for about 25 to about 35 minutes to form the Al a Cr b Si c V d N e layer, wherein the atomic ratio of Al:Cr:Si in the AlCrSi target is about (59-61):(29-31):10, and the target currents of the AlCrSi target and the V target are both set to about 80 to about 120 A, the bias voltages of the AlCrSi target and the V target are both set to about -80 to about -120 V, and the distances between the AlCrSi target and the V target and the substrate are both set to about 24 to about 26 cm.

[0041] Scheme 15: A preparation method according to any one of Schemes 10 to 14, wherein the method comprises step 3: adding the Al obtained in step 2 a Cr b Si c V d N e The Ti layer is further deposited on the surface by arc ion plating. x Al y The N layer and the Al a Cr b Si c V d N e Layer 1, 2 or 3 times.

[0042] Scheme 16: A tool, preferably a cutting tool, wherein the tool comprises the Cr according to any one of Schemes 1 to 9 above. m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coating or Cr prepared by the preparation method according to any one of the above schemes 10 to 15 m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coating.

[0043] Technical Effects

[0044] Cr prepared by the method of the present inventionm N / Ti x Al y N / A a Cr b Si c V d N e The nanocomposite coating comprehensively utilizes the Al a Cr b Si c V d N e The high wear resistance and thermal stability of the Ti x Al y The excellent hardness and toughness of the N layer and the Cr m The high adhesion and other characteristics of the N transition layer enable the composite coating of the present invention to have good comprehensive mechanical properties such as hardness, bonding strength and toughness while also having excellent lubrication properties.

[0045] Specifically,

[0046] The Cr of the present invention m N / Ti x Al y N / A a Cr b Si c V d N e The nanocomposite coating comprises AlN, CrN, VN phases of face-centered cubic structure and AlN phases of close-packed hexagonal structure, which account for the main part, and Si nitride amorphous phases, which account for the minor part. The amorphous phases of the minor part may at least partially wrap the crystalline phases of the major part in some cases. The amorphous phases contained in the composite coating have the performance of blocking crack generation and inhibiting the movement of dislocations, thereby improving the toughness and wear resistance of the composite coating of the present invention, so that the coating has suitable hardness, bonding force, thermal stability and anti-friction and wear performance. Specifically, the hardness of the nanocomposite coating of the present invention is within the range of about 29.4±1.5GPa, the elastic modulus is within the range of about 384.4±12.3GPa, the bonding force can reach about 54N or more, the ratio of hardness / elastic modulus reaches about 0.0765 or more, and the friction coefficient is less than about 0.6, preferably less than about 0.56. The composite coating of the present invention has good hardness, bonding force and toughness while also taking into account excellent lubrication performance.

[0047] The Cr of the present invention m N / Ti x Al y N / A a Cr b Si c V dN e The nanocomposite coating has an introduced V element, thereby forming a vanadium-containing nitride, which has excellent resistance to high-temperature friction. The addition of V inhibits the growth of columnar crystals in the coating, and generates a vanadium oxide lubricating phase during the friction process, so that the composite coating has an excellent lubrication effect in a high-temperature environment and can reduce its wear rate.

[0048] The Cr of the present invention m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coatings have good lubricating effects and can replace some lubricating fluids in the production process to achieve lubrication effects, thus avoiding pollution and playing an important role in protecting the ecological environment.

[0049] The Cr of the present invention m N / Ti x Al y N / A a Cr b Si c V d N e The preparation method of the nanocomposite coating has high process repeatability. m N / Ti x Al y N / A a Cr b Si c V d N e The surface of the nanocomposite coating is dense and smooth. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] In order to more clearly illustrate the technical solutions in the specific embodiments of the present invention, the drawings used in the specific embodiments will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0051] Figure 1 The Cr m N / Ti x Al y N / A a Cr b Si c V d N e Schematic diagram of the structure of the nanocomposite coating.

[0052] Figure 2 Cr in Example 1 of the present invention m N / Ti x Al y N / A a Cr b Si c V d N e XRD diffraction patterns of nanocomposite coatings.

[0053] FIG3(a) is a graph showing Cr in Example 1 of the present invention. m N / Ti x Al y N / A a Cr b Si c V d N e Scanning electron microscopy image of the nanocomposite coating surface.

[0054] 3(b) to (f) are scanning electron microscope images of the surfaces of the nanocomposite coatings of Comparative Examples 1 to 5 of the present invention, respectively.

[0055] Figure 4 Cr in Example 1 of the present invention m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coating and Cr of Comparative Example 1 m N / Ti x Al y N / A a Cr b Si c Ti d N e Plot of average friction coefficient of nanocomposite coatings.

[0056] Reference numerals: 1 - matrix; 2 - Cr m N transition layer; 3——Ti x Al y N layer; 4——Al a Cr b Si c V d N e layer. DETAILED DESCRIPTION

[0057] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention and the accompanying drawings. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without paying creative work belong to the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.

[0058] In the description of the present invention, the terms "upper", "lower", "inside", "outside" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the present invention and do not require that the present invention must be constructed and operated in a specific orientation. Therefore, they should not be understood as limitations on the present invention.

[0059] The endpoints and any values ​​of the scope disclosed in the present invention are not limited to the precise scope or value, and these scopes or values ​​should be understood to include values ​​close to these scopes or values. The term "about" used in the present invention means that the modified numeral can fluctuate within the range of ±20%, ±15%, ±10%, ±5% or ±2% of the numeral. For numerical ranges, the endpoint values ​​of each scope, the endpoint values ​​of each scope and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in the present invention.

[0060] According to a first aspect of the present invention, there is provided a Cr m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coating, the Cr m N / Ti x Al y N / A a Cr b Si c V d N e The nanocomposite coating is bonded to the surface of the substrate.

[0061] As attached Figure 1 As shown in FIG. , the Cr of the first aspect of the present invention m N / Ti x Al y N / A a Cr b Si c Vd N e The nanocomposite coating comprises a substrate 1, a Cr m N transition layer 2, and the Cr m Ti with one or more periodic structures on the surface of N transition layer 2 x Al y N / A a Cr b Si c V d N e Composite multilayer, the Ti x Al y N / A a Cr b Si c V d N e One period of the composite multilayer contains the inner layer of Ti x Al y N layer 3 and outer Al a Cr b Si c V d N e Layer 4. Here, in the Ti x Al y N / A a Cr b Si c V d N e In one cycle of the composite multilayer, the inner layer refers to the Ti layer that is relatively closer to the substrate. x Al y N layer 3, the outer layer refers to the Al a Cr b Si c V d N e Layer 4. Here, the "Ti having one or more periodic structures x Al y N / A a Cr b Si c V d N e "Composite multilayer" means that the Ti x Al y N / A a Cr b Si c V d N e The composite multilayer can exist alone in the form of an outer layer 4 stacked on an inner layer 3 in the Cr mN transition layer 2, or repeatedly present in the Cr m N transition layer 2.

[0062] In the first aspect of the present invention, Cr m N / Ti x Al y N / A a Cr b Si c V d N e In the nanocomposite coating, the settings of various parameters are as follows:

[0063] m is from about 0.99 to about 1.01, for example about 1.00;

[0064] x is about 0.29 to about 0.31, for example about 0.30; y is about 0.69 to about 0.71, for example about 0.70; and x+y is about 1;

[0065] a is from about 0.20 to about 0.25, for example, about 0.205, about 0.21, about 0.215, about 0.22, about 0.225, about 0.23, about 0.235, about 0.24, or about 0.245; b is from about 0.13 to about 0.17, for example, about 0.135, about 0.14, about 0.145, about 0.15, about 0.155, about 0.16, or about 0.165; c is from about 0.05 to about 0.10, for example, about 0.055, about 0.06, about 0.065, about 0.07, about 0.075 , about 0.08, about 0.085, about 0.09 or about 0.095; d is about 0.05 to about 0.10, for example, about 0.055, about 0.06, about 0.065, about 0.07, about 0.075, about 0.08, about 0.085, about 0.09 or about 0.095; e is about 0.40 to about 0.50, for example, about 0.41, about 0.42, about 0.43, about 0.44, about 0.45, about 0.46, about 0.47, about 0.48 or about 0.49; and a+b+c+d+e is about 1.

[0066] Here, in Cr m N transition layer 2 and Ti x Al y The values ​​of m, x and y in the N layer 3 need to be kept within the above-defined ranges. These values ​​outside the defined ranges may have adverse effects on the hardness, bonding force and friction and wear properties of the composite coating of the present invention.

[0067] In addition, in the Al a Cr b Si c V d N eIn layer 4, based on the total number of atoms, the atomic proportion of Al is about 20 to about 25 at%, the atomic proportion of Cr is about 13 to about 17 at%, the atomic proportion of Si is about 5 to about 10 at%, the atomic proportion of V is about 5 to about 10 at%, and the atomic proportion of N is about 40 to about 50 at%.

[0068] Here, the atomic proportion fraction of Al and the atomic proportion fraction of Cr have an important influence on the hardness and bonding strength of the coating. Outside the above-defined range, the hardness and bonding strength of the coating may not meet the requirements. The atomic proportion fraction of Si has an important influence on the hardness of the coating. Outside the above-defined range, the hardness of the coating may not meet the requirements. The atomic proportion fraction of V has an important influence on the friction coefficient of the coating. Outside the above-defined range, the friction coefficient of the coating may not meet the requirements.

[0069] The alternating Ti x Al y N layer 3 and Al a Cr b Si c V d N e Layer 4 can effectively improve the film-base bonding strength and thermal stability of the nanocomposite coating of the first aspect of the present invention. Here, when the tool containing the coating undergoes operations such as chip cutting, such as when undergoing a thermal friction and wear tester test in the embodiment of the present invention, the coating may reach a very high temperature, such as exceeding about 450°C, at which time the coating can still maintain the required mechanical properties, which to a certain extent reflects that the composite coating has excellent thermal stability. The Ti x Al y The N layer 3 can also optimize the deposition environment, a Cr b Si c V d N e The deposition of layer 4 provides better bonding strength and can prevent the Ti element from penetrating into the substrate under high temperature environment. In the present invention, the nanocomposite coating of the present invention has both good mechanical properties and self-lubricating properties through the introduction of the nanocomposite structure and the V element.

[0070] In the first aspect of the present invention, Cr m N / Ti x Al y N / A a Cr b Si c V d N e In a preferred embodiment of the nanocomposite coating, the Cr mThe thickness of the N transition layer 2 is in the range of about 0.4 to about 0.6 μm, for example, about 0.45 μm, about 0.50 μm or about 0.55 μm; x Al y The thickness of the N layer 3 is in the range of about 0.4 to about 0.6 μm, for example, about 0.45 μm, about 0.50 μm or about 0.55 μm; a Cr b Si c V d N e The thickness of the layer 4 is in the range of about 0.4 to about 0.6 μm, for example, about 0.45 μm, about 0.50 μm or about 0.55 μm; x Al y N layer 3 and an Al a Cr b Si c V d N e The total thickness of the composite coating composed of layer 4 is in the range of about 0.9 to about 1.1 μm, for example, about 0.95 μm, about 1.00 μm or about 1.05 μm. m N transition layer 2, Ti x Al y N layer 3 and Al a Cr b Si c V d N e If the thickness of layer 4 is not within the required range, the comprehensive performance of the composite coating may not meet the requirements of the present invention.

[0071] In the first aspect of the present invention, Cr m N / Ti x Al y N / A a Cr b Si c V d N e In the nanocomposite coating, the substrate is not particularly limited, but in a preferred embodiment, it can be selected from any one of cemented carbide, high speed steel and corundum.

[0072] In the first aspect of the present invention, Cr m N / Ti x Al y N / A a Cr b Si c V d N e In another preferred embodiment of the nanocomposite coating, the Ti having a periodic structurex Al y N / A a Cr b Si c V d N e The number of periods of the composite multilayer may be, for example, 1, 2, 3 or 4 or more.

[0073] In the first aspect of the present invention, Cr m N / Ti x Al y N / A a Cr b Si c V d N e In another preferred embodiment of the nanocomposite coating, the composite coating contains AlN, CrN, VN phases with a face-centered cubic structure and an AlN phase with a close-packed hexagonal structure, which account for the main part, and amorphous nitrides of Si, which account for a minor part. The amorphous phase, which accounts for a certain amount of the minor part, may at least partially wrap the crystalline phase, which accounts for the main part, in some cases. The nanocomposite coating of the present invention is a composite nanocoating, and the composite of each coating is not a clearly layered superposition, and there will also be element diffusion between the layers. Therefore, when there is a certain Si content in each layer, a Si3N4 amorphous phase may be formed. The amorphous phase contained in the coating has the ability to prevent cracks from occurring and inhibit the movement of dislocations, thereby improving the toughness and wear resistance of the composite coating of the present invention, so that the coating has suitable hardness, bonding strength, thermal stability and anti-friction and wear properties.

[0074] The Cr in the first aspect of the present invention m N / Ti x Al y N / A a Cr b Si c V d N e The nanocomposite coating typically has one or more of the following properties: a hardness in the range of about 29.4 ± about 1.5 GPa, an elastic modulus in the range of about 384.4 ± about 12.3 GPa, a bonding force of about 54 N or more, a hardness / elastic modulus ratio of about 0.0765 or more, and a friction coefficient of less than about 0.6, preferably less than about 0.56.

[0075] According to a second aspect of the present invention, the present invention provides a method for preparing the Cr m N / Ti x Al y N / A a Cr b Si c Vd N e The method for preparing a nanocomposite coating comprises steps 1 and 2 and an optional step 3.

[0076] The step 1 comprises depositing the Cr on the substrate surface by arc ion plating m N transition layer 2.

[0077] In a preferred embodiment, the deposited Cr m The N transition layer 2 process includes:

[0078] In the case where nitrogen gas with a flow rate of about 600 to about 800 sccm (e.g., about 700 sccm) is continuously introduced into an arc ion plating deposition chamber under a nitrogen atmosphere, the pressure in the deposition chamber is controlled to be about 0.8 to about 1.1 Pa (e.g., about 0.9 Pa or about 1.0 Pa), the temperature is controlled to be about 460 to about 490° C. (e.g., about 470° C. or about 480° C.), and the temperature of the substrate in the deposition chamber is controlled to be about 470 to about 500° C. (e.g., about 480° C. or about 490° C.), the Cr target is turned on to perform the arc ion plating deposition for about 25 to about 35 minutes (e.g., about 30 minutes) to form the Cr m N transition layer 2, wherein the target current of the Cr target is set to about 80 to about 100 A (e.g., about 90 A), the bias voltage of the Cr target is set to about -80 to about -120 V (e.g., about -100 V), and the distance between the Cr target and the substrate is set to about 24 to about 26 cm (e.g., about 25 cm).

[0079] Cr obtained from step 1 m The thickness of the N transition layer 2 is in the range of about 0.4 to about 0.6 μm, for example, about 0.5 μm, and m is in the range of about 0.99 to about 1.01, for example, about 1.00.

[0080] The step 2 comprises: m The Ti x Al y N layer 3 and the Al a Cr b Si c V d N e Layer 4.

[0081] In a preferred embodiment, the deposited Ti x Al y The N-layer 3 process includes:

[0082] In the case where nitrogen gas with a flow rate of about 600 to about 800 sccm (e.g., about 700 sccm) is continuously introduced into an arc ion plating deposition chamber under a nitrogen atmosphere, the pressure in the deposition chamber is controlled to be about 0.8 to about 1.1 Pa (e.g., about 0.9 Pa or about 1.0 Pa), the temperature is controlled to be about 460 to about 490° C. (e.g., about 470° C. or about 480° C.), and the Cr-containing molten metal in the deposition chamber is controlled to be about 0.5 to about 1.0 μm. m The temperature of the substrate of the N transition layer 2 is about 470 to about 500° C. (for example, about 480° C. or about 490° C.), and the TiAl target is turned on to perform the arc ion plating deposition for about 55 to about 65 minutes (for example, about 60 minutes) to form the TiAl x Al y N layer 3, wherein the atomic ratio of Ti:Al in the TiAl target is about (32-34):(66-68), for example, about 33:67, the target current of the TiAl target is set to about 90 to about 110 A (for example, about 100 A), the bias voltage of the TiAl target is set to about -80 to about -120 V (for example, about -100 V), and the distance between the TiAl target and the substrate is set to about 24 to about 26 cm (for example, about 25 cm).

[0083] Ti obtained from step 2 x Al y The thickness of the N layer 3 is in the range of about 0.4 to about 0.6 μm, and x is in the range of about 0.29 to about 0.31, such as about 0.30, and y is in the range of about 0.69 to about 0.71, such as about 0.70, wherein x+y is about 1.

[0084] In another preferred embodiment, the deposited Al a Cr b Si c V d N e The Tier 4 process includes:

[0085] In the case where nitrogen gas with a flow rate of about 600 to about 800 sccm (e.g., about 700 sccm) is continuously introduced into an arc ion plating deposition chamber under a nitrogen atmosphere, the pressure in the deposition chamber is controlled to be about 0.8 to about 1.1 Pa (e.g., about 0.9 Pa or about 1.0 Pa), the temperature is controlled to be 460 to 490° C. (e.g., about 470° C. or about 480° C.), and the temperature of the substrate in the deposition chamber is controlled to be 470 to 500° C. (e.g., about 480° C. or about 490° C.), and an AlCrSi target and a V target are simultaneously turned on to perform the arc ion plating deposition for 25 to 35 minutes (e.g., about 30 minutes) to form the AlCrSi target. a Cr b Si c V d Ne Layer 4, wherein the atomic ratio of Al:Cr:Si in the AlCrSi target is about (59-61):(29-31):10, for example, about 60:30:10, and the target currents of the AlCrSi target and the V target are both set to 80 to 120 A (for example, about 100 A), the bias voltages of the AlCrSi target and the V target are both set to -80 to -120 V (for example, about -100 V), and the distances between the AlCrSi target and the V target and the substrate are both set to 24 to 26 cm (for example, about 25 cm).

[0086] Al obtained from step 2 a Cr b Si c V d N e The thickness of layer 4 is in the range of about 0.4 to about 0.6 μm, for example about 0.5 μm, and a is in the range of about 0.20 to about 0.25, b is in the range of about 0.13 to about 0.17, c is in the range of about 0.05 to about 0.10; d is in the range of about 0.05 to about 0.10, and e is in the range of about 0.40 to about 0.50, wherein a+b+c+d+e is about 1.

[0087] The optional step 3 comprises adding the Al obtained in step 2 a Cr b Si c V d N e The Ti layer 4 is further deposited in sequence by arc ion plating. x Al y N layer 3 and the Al a Cr b Si c V d N e Layer 4 one or more times.

[0088] The Ti deposited in step 3 x Al y N layer 3 process and deposition of Al a Cr b Si c V d N e The process of layer 4 is identical to the process of depositing the corresponding layer in step 2.

[0089] In a preferred embodiment of the present invention, step 3 is performed after step 2, and in step 3, the Ti x Al y N layer 3 and the Al a Cr b Sic V d N e The number of layer 4 can be 1, 2 or 3 times.

[0090] According to a third aspect of the present invention, the present invention provides a tool, preferably a cutting tool, wherein the tool comprises Cr according to the first aspect of the present invention. m N / Ti x Al y N / A a Cr b Si c V d N e The nanocomposite coating or the Cr prepared according to the preparation method of the second aspect of the present invention m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coating.

[0091] The present invention contains the Cr m N / Ti x Al y N / A a Cr b Si c V d N e During the use of tools with nano-composite coatings, the friction coefficient increases rapidly in a short period of time due to the roughness of the coating surface in the initial stage under the influence of wear particles; in the middle stage, due to the solid lubricant contained in the coating, the temperature rises during friction, and the V element on the surface easily reacts with oxygen in the air to generate VO lubricating phase oxide, which has a lubricating effect on the coating, and the friction coefficient remains stable for a considerable period of time.

[0092] The present invention is further described in detail below with reference to specific embodiments and comparative examples.

[0093] The coating machine used in the following examples and comparative examples is a coating machine obtained from Shenyang VLEAD Company, and the ion sputtering targets used include Ti target, V target, TiAl target (the atomic ratio of Ti:Al is about 33:67 or 40:60) and AlCrSi target (the atomic ratio of Al:Cr:Si is about 6:3:1). The targets are all obtained from Suzhou Liujiu New Materials Co., Ltd.

[0094] Example 1 :

[0095] The Cr of the present invention is deposited on the substrate by the following process:m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coating.

[0096] Substrate pretreatment:

[0097] Use cemented carbide as the substrate. The cemented carbide substrate is ground and polished, and sandpaper of different meshes (300 mesh, 600 mesh, 850 mesh, 1200 mesh, 1500 mesh) is used in turn to polish the substrate surface to a smooth and flat surface without obvious defects, and then the substrate is polished to a mirror effect with a metallographic polisher assisted by diamond powder. The substrate surface after treatment is neat and mirror-like, without obvious scratches and pits. The treated substrate is placed in an acetone solution for ultrasonic cleaning for about 20 minutes to ensure that there is no oil stain or stain on the substrate surface. Then the substrate cleaned with acetone is cleaned in ultrapure water and anhydrous ethanol for about 10 minutes in turn. Finally, the substrate cleaned with ethanol is placed on the turntable of the coating machine, and the distance between the substrate surface and the target material used is about 25 cm. After wiping the target material with anhydrous ethanol again, close the deposition chamber door of the coating machine.

[0098] Vacuuming + heating:

[0099] Open the roughing pump and roughing valve to pump the pressure in the deposition chamber to below 3 Pa, turn on the molecular pump, and after the molecular pump speed stabilizes, open the fine pump and fine valve to pump the pressure in the deposition chamber to 3×10 -3 Turn on the heating module, raise the temperature in the deposition chamber to above about 480°C, and control the pressure in the deposition chamber to be stable at about 3×10 -3 Below Pa.

[0100] Etching and cleaning:

[0101] Open the argon gas channel and introduce argon gas at a flow rate of about 450 sccm into the deposition chamber. Control the pressure in the deposition chamber to about 0.3 Pa. Turn on the Ti target, set the Ti target current to about 80 A, set the etching negative bias to about -120 V, and perform ion etching cleaning for about 120 minutes.

[0102] Cr m N / Ti x Al y N / A a Cr b Si c V d N e Deposition of Nanocomposite Coatings:

[0103] During the deposition process, the argon gas channel was opened to introduce argon gas at a flow rate of about 50 sccm into the deposition chamber, and the nitrogen gas channel was opened to introduce nitrogen gas at a flow rate of about 700 sccm into the deposition chamber.

[0104] The pressure in the deposition chamber was controlled to be about 0.8 to about 1.1 Pa, the temperature was controlled to be about 475° C., and the substrate temperature was controlled to be about 485° C. The Cr target was turned on, the Cr target current was set to about 100 A, the etching negative bias voltage was set to about -100 V, and Cr was deposited. m N transition layer 2 is about 30 minutes.

[0105] Turn off the Cr target, control the pressure in the deposition chamber to about 0.8 to about 1.1 Pa, the temperature to about 480°C, and control the substrate temperature to about 485°C. Turn on the TiAl target. Set the TiAl target current to about 100A, the etching negative bias voltage to about -100V, and deposit TiAl. x Al y N layer about 60 minutes.

[0106] The TiAl target was turned off, and the pressure in the deposition chamber was controlled to be about 0.8 to about 1.1 Pa, the temperature was controlled to be about 480°C, and the substrate temperature was controlled to be about 485°C. The AlCrSi target and the V target were turned on at the same time, and the target currents of the AlCrSi target and the V target were set to about 100 A, and the negative etching bias voltage was set to about -100 V. Al was deposited. a Cr b Si c V d N e Layer for about 30 minutes.

[0107] Continue to alternately deposit Ti x Al y N layer and Al a Cr b Si c V d N e Layer. Deposited Ti x Al y N layer and Al a Cr b Si c V d N e There are four cycles in total, Ti x Al y N layer and Al a Cr b Si c V d N e The coating thickness of one period of the layers was about 1 μm, and the total thickness was about 4 μm.

[0108] End of deposition:

[0109] Turn off the ion sputtering target, close the argon and nitrogen gas channels, turn off the bias voltage, turn off the heating module, let the deposition chamber stand to room temperature, and remove the vacuum state.

[0110] Remove the Cr m N / Ti x Al y N / A a Cr b Si c V d N e The cemented carbide substrate of the nanocomposite coating is analyzed, wherein Cr m N transition layer 2, Ti x Al y N layer 3 and Al a Cr b Si c V d N e The thickness of layer 4 is about 0.5 μm, m is about 1.00; x is about 0.30, y is about 0.70; a is about 0.225, b is about 0.15, c is about 0.075, d is about 0.075, and e is about 0.475.

[0111] The Cr obtained in Example 1 m N / Ti x Al y N / A a Cr b Si c V d N e The nanocomposite coating was subjected to X-ray diffraction analysis to obtain the following information: Figure 2 The XRD pattern shown in Figure 2 It can be seen that in Example 1 of the present invention, Cr m N / Ti x Al y N / A a Cr b Si c V d N e There are polycrystalline nanocomposite coatings, mostly with face-centered cubic structures, mainly composed of AlN, CrN and VN phases. There is no Si3N4 phase in the spectrum, which may be due to the crystallization temperature of silicon nitride being above 1000℃, while the temperature used in the experiment to prepare the coating is 480℃, which does not cause Si3N4 to crystallize, so Si3N4 may exist in the coating as an amorphous phase. The phases in the spectrum all preferentially grow along the (111)(211) crystal planes.

[0112] The Cr obtained in Example 1 m N / Ti x Al y N / A a Cr b Si c V d N e The surface of the nanocomposite coating was photographed by scanning electron microscope to obtain the surface morphology shown in Figure 3 of the specification. As can be seen from Figure 3, the surface of the composite coating of Example 1 of the present invention is relatively flat and dense.

[0113] The Cr obtained in Example 1 was subjected to a thermal friction and wear tester. m N / Ti x Al y N / A a Cr b Si c V d N e The friction coefficient of the nanocomposite coating was measured, and it was determined that the friction coefficient of the composite coating of Example 1 was still within the range of about 0.53±0.02 when the temperature reached above 450°C.

[0114] The Cr obtained in Example 1 was stained by a nanoindenter. m N / Ti x Al y N / A a Cr b Si c V d N e The hardness and elastic modulus of the nanocomposite coating were measured, and it was determined that the hardness of the composite coating of Example 1 was about 29.4±about 1.5 GPa, and the elastic modulus was about 384.4±about 12.3 GPa.

[0115] The Cr obtained in Example 1 was scratched by a large load scratch tester. m N / Ti x Al y N / A a Cr b Si c V d N e The bonding strength of the nanocomposite coating was measured, and it was determined that the bonding strength of the composite coating of Example 1 was at least about 54N.

[0116] The above test results are shown in Table 1 below.

[0117] Comparative Example 1:

[0118] The Cr of Comparative Example 1 was deposited on the substrate using a process similar to that of Example 1. mN / Ti x Al y N / A a Cr b Si c Ti d N e The nanocomposite coating was prepared by replacing the V target used in Example 1 with a Ti target. m N / Ti x Al y N / A a Cr b Si c Ti d N e In the nanocomposite coating, Cr m N transition layer, Ti x Al y N layer and Al a Cr b Si c Ti d N e The thickness of the layers were all about 0.5 μm, m was about 1.00; x was about 0.30, y was about 0.70; a was about 0.225, b was about 0.15, c was about 0.075, d was about 0.075, and e was about 0.475.

[0119] Comparative Example 2:

[0120] The Cr of Comparative Example 2 was deposited on the substrate using a process similar to that of Example 1. m N / Ti x Al y N / A a Cr b Si c V d N e The nanocomposite coating was prepared by replacing the TiAl target (Ti:Al=33:67) used in Example 1 with a TiAl target (Ti:Al=40:60). m N / Ti x Al y N / A a Cr b Si c V d N e In the nanocomposite coating, Cr m N transition layer, Ti x Al y N layer and Al a Cr b Si c Ti d Ne The thickness of the layers were all about 0.5 μm, m was about 1.00; x was about 0.50, y was about 0.50; a was about 0.225, b was about 0.15, c was about 0.075, d was about 0.075, and e was about 0.475.

[0121] Comparative Example 3:

[0122] The Cr of Comparative Example 3 was deposited on the substrate using a process similar to that of Example 1. m N / A a Cr b Si c V d N e The nanocomposite coating, except that the Ti deposition in Example 1 is not performed x Al y N-layer steps, and Al a Cr b Si c V d N e The deposition of the layer was performed only once. m N / A a Cr b Si c V d N e In the nanocomposite coating, Cr m N transition layer and Al a Cr b Si c V d N e The thickness of the layers were all about 0.5 μm, m was about 1.00; a was about 0.225, b was about 0.15, c was about 0.075, d was about 0.075, and e was about 0.475.

[0123] Comparative Examples 4 and 5:

[0124] The Cr of Comparative Examples 4 and 5 was deposited on the substrate using a process similar to that of Example 1. m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coating, except that the target current of the V target used in Comparative Examples 4 and 5 is set to about 120A and about 80A, respectively, and the etching negative bias is set to about -100V and about -80V, respectively, so that:

[0125] Cr of Comparative Example 4 m N / Tix Al y N / A a Cr b Si c V d N e In the nanocomposite coating, Cr m N transition layer, Ti x Al y N layer and Al a Cr b Si c V d N e The thickness of the layers are all about 0.5 μm, m is about 1.00; x is about 0.30, y is about 0.70; a is about 0.225, b is about 0.15, c is about 0.075; d is about 0.125; and e is about 0.425;

[0126] Cr of Comparative Example 5 m N / Ti x Al y N / A a Cr b Si c V d N e In the nanocomposite coating, Cr m N transition layer, Ti x Al y N layer and Al a Cr b Si c V d N e The thickness of the layers were all about 0.5 μm, m was about 1.00; x was about 0.30, y was about 0.70; a was about 0.225, b was about 0.15, c was about 0.075; d was about 0.025; and e was about 0.525.

[0127] The surfaces of the nanocomposite coatings obtained in Comparative Examples 1-5 were photographed by scanning electron microscope to obtain surface morphology (see FIG3 ). Pits appeared on part of the surfaces of the composite coatings of Comparative Examples 1-5 of the present invention.

[0128] The friction coefficient, hardness, elastic modulus and bonding force of the nanocomposite coatings obtained from Comparative Examples 1-5 were measured by a thermal friction and wear tester, a nanoindenter and a high-load scratch tester. The measurement results are shown in Table 1 below.

[0129] Table 1: Comparison of hardness, elastic modulus, toughness, bonding force and friction coefficient of the composite coating of Example 1 of the present invention and the composite coating of Comparative Examples 1-5

[0130] Example No. Hardness H(GPa) Elastic modulus E(GPa) H / E Binding force (N) Friction coefficient Example 1 29.4±1.5 384.4±12.3 0.0765 54 0.53±0.02 Comparative Example 1 31.4±1.3 443.2±15.4 0.0708 44 0.62±0.02 Comparative Example 2 28.1±2.1 383.4±17.4 0.0733 47 0.68±0.02 Comparative Example 3 29.2±1.8 388.3±12.9 0.0752 45 0.62±0.02 Comparative Example 4 27.3±1.1 369.9±14.3 0.0738 51 0.59±0.02 Comparative Example 5 28.7±1.6 402.5±11.1 0.0713 39 0.64±0.02

[0131] It can be seen from the above table that, compared with the composite coating of comparative example 1, the hardness H and elastic modulus E of the composite coating of embodiment 1 of the present invention are reduced. This is because the soft VN is dissolved in the CrN lattice, and the soft phase increases.

[0132] However, it is known that the ratio of hardness H to elastic modulus E can characterize the toughness of the coating material to a certain extent, and the larger the ratio, the better the toughness of the coating material. The H / E values ​​of the composite coating of Example 1 of the present invention are all higher than those of the composite coatings of Comparative Examples 1 to 5, indicating that the composite coating of Example 1 of the present invention not only ensures a certain level of hardness, but also takes into account the coordination of toughness.

[0133] The bonding strength of the composite coating of Example 1 of the present invention is also higher than that of the composite coatings of Comparative Examples 1 to 5. This is because Ti x Al y The N layer has a strong film-base bonding strength with other coatings and Cr m The N transition layer adjusts the thermal expansion coefficient between the substrate and the coating.

[0134] Cr in Example 1 of the present invention m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coating and Cr of Comparative Example 1 m N / Ti x Al y N / A a Cr b Si c Ti d N e The average friction coefficient of the nanocomposite coating is Figure 4 As shown in Figure 4 It can be seen that the anti-friction ability of the composite coating of Example 1 of the present invention is much higher than that of Comparative Example 1. This is because the addition of the V element enables the nano-composite coating system to continuously generate a sub-lubricating phase during the friction test, thereby reducing the friction coefficient.

[0135] In addition, since the Cr in Example 1 of the present invention m N / Ti x Al y N / A a Cr b Si c V d N eThe specific combination of the various coatings of the nanocomposite coating can still provide better self-lubricating properties than comparative examples 1 to 5 in a high temperature (above about 450° C.) environment, although a large amount of heat is released during the tool cutting process.

[0136] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the above embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions claimed to be protected by the present invention.

Claims

1. A Cr bonded to the surface of the substrate m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coating, characterized in that The nanocomposite coating comprises Cr deposited on the surface of the substrate. m N transition layer, and deposited on the Cr m Ti with one or more periodic structures on the surface of the N transition layer x Al y N / A a Cr b Si c V d N e Composite multilayer, wherein the Ti x Al y N / A a Cr b Si c V d N e One period of the composite multilayer contains the inner layer of Ti x Al y N layer and outer Al a Cr b Si c V d N e layer, in m=0.99-1.01; x=0.29-0.31, y=0.69-0.71, and x+y=1; a=0.20-0.25; b=0.13-0.17; c=0.05-0.10; d=0.05-0.10, e=0.40-0.50, and a+b+c+d+e=1.

2. The Cr according to claim 1 m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coating, characterized in that The Cr m The thickness of the N transition layer is in the range of 0.4 to 0.6 μm, and / or The Ti x Al y N / A a Cr b Si c V d N e The total thickness of one period of the composite multilayer is in the range of 0.9 to 1.1 μm, where The Ti x Al y The thickness of the N layer is in the range of 0.4 to 0.6 μm, and / or The Al a Cr b Si c V d N e The thickness of the layer is in the range of 0.4 to 0.6 μm.

3. The Cr according to claim 1 m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coating, characterized in that The substrate is selected from any one of cemented carbide, high speed steel and corundum.

4. The Cr according to claim 1 m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coating, characterized in that The Ti with periodic structure x Al y N / A a Cr b Si c V d N e The number of periods of the composite multilayer is 1, 2, 3 or 4.

5. Cr according to any one of claims 1 to 4 m N / Ti x Al y N / A a Cr b Si cV d N e Nanocomposite coating, characterized in that The composite coating comprises AlN, CrN and VN phases with a face-centered cubic structure, an AlN phase with a close-packed hexagonal structure, and a Si nitride amorphous phase.

6. Cr according to any one of claims 1 to 4 m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coating, characterized in that The nanocomposite coating has one or more of the following properties: hardness within the range of 29.4±1.5 GPa, elastic modulus within the range of 384.4±12.3 GPa, bonding force above 54 N, hardness / elastic modulus ratio above 0.0765, and friction coefficient less than 0.

6.

7. A method for preparing Cr according to any one of claims 1 to 6 m N / Ti x Al y N / A a Cr b Si c V d N e A method for nanocomposite coating, characterized in that, The method comprises the following steps: Step 1: Depositing the Cr on the substrate surface by arc ion plating m N transition layer; Step 2: In the Cr m The Ti x Al y The N layer and the Al a Cr b Si c V d N e Layer; and Optional step 3: In the Al obtained in step 2 a Cr b Si c V d N e The Ti layer is further deposited on the surface by arc ion plating. x Al y The N layer and the Al a Cr b Si c V d N e Layer one or more times.

8. The preparation method according to claim 7, characterized in that: The Cr deposition m The N transition layer process includes: In the case of continuously introducing nitrogen gas with a flow rate of 600 to 800 sccm into the arc ion plating deposition chamber under a nitrogen atmosphere, the pressure in the deposition chamber is controlled to be 0.8 to 1.1 Pa, the temperature is controlled to be 460 to 490° C., and the temperature of the substrate in the deposition chamber is controlled to be 470 to 500° C., and the Cr target is turned on to perform the arc ion plating deposition for 25 to 35 minutes to form the Cr m N transition layer, wherein the target current of the Cr target is set to 80 to 100 A, the bias voltage of the Cr target is set to -80 to -120 V, and the distance between the Cr target and the substrate is set to 24 to 26 cm; and / or The Ti is deposited x Al y The N-layer process includes: In the case of continuously introducing nitrogen gas with a flow rate of 600 to 800 sccm into the arc ion plating deposition chamber under a nitrogen atmosphere, the pressure in the deposition chamber is controlled to be 0.8 to 1.1 Pa and the temperature is controlled to be 460 to 490° C., and the Cr-containing m The temperature of the substrate of the N transition layer is 470 to 500° C., and the TiAl target is turned on to perform the arc ion plating deposition for 55 to 65 minutes to form the TiAl transition layer. x Al y N layer, wherein the atomic ratio of Ti:Al in the TiAl target is (32-34):(66-68), the target current of the TiAl target is set to 90 to 110A, the bias voltage of the TiAl target is set to -80 to -120V, and the distance between the TiAl target and the substrate is set to 24 to 26cm; and / or The Al a Cr b Si c V d N e The layer process includes: In the case of continuously introducing nitrogen gas with a flow rate of 600 to 800 sccm into the arc ion plating deposition chamber under a nitrogen atmosphere, the pressure in the deposition chamber is controlled to be 0.8 to 1.1 Pa and the temperature is controlled to be 460 to 490° C., and the Cr-containing m N transition layer and the Ti x Al y The temperature of the N layer substrate is 470 to 500° C., and the AlCrSi target and the V target are simultaneously turned on to perform the arc ion plating deposition for 25 to 35 minutes to form the Al a Cr b Si c V d N e layer, wherein the atomic ratio of Al:Cr:Si in the AlCrSi target is (59-61):(29-31):10, and the target currents of the AlCrSi target and the V target are both set to 80 to 120 A, the bias voltages of the AlCrSi target and the V target are both set to -80 to -120 V, and the distances between the AlCrSi target and the V target and the substrate are both set to 24 to 26 cm.

9. The preparation method according to claim 7 or 8, characterized in that: The method comprises performing step 3 after step 2, wherein step 3 comprises: a Cr b Si c V d N e The Ti layer is further deposited on the surface by arc ion plating. x Al y The N layer and the Al a Cr b Si c V d N e Layer 1, 2 or 3 times.

10. A tool, preferably a cutting tool, characterized in that The tool comprises Cr according to any one of claims 1 to 6 m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coating or Cr prepared by the preparation method according to any one of claims 7 to 9 m N / Ti x Al y N / A a Cr b Si c V d N e Nanocomposite coating.

Citation Information

Cited By

  • CrmNn / AlxCryNz / TiaAlbTacBdNe nano-composite coating, preparation method thereof and tool comprising CrmNn / AlxCryNz / TiaAlbTacBdNe nano-composite coating

    CN120888870A