Production process of stainless steel seamless steel pipe
By synergistically acting tetrabutyl titanate, ammonium persulfate and oxalic acid in the modified steel pipe treatment solution, the problem of insufficient adhesion of the galvanized layer of stainless steel seamless steel pipe is solved, and the adhesion and bacterial inhibition of the galvanized layer are significantly improved. Performance extends service life and improves the overall performance of the product.
Patent Information
- Application Number
- CN202411077422.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing stainless steel seamless steel pipes are insufficiently adhesive during galvanizing treatment, resulting in corrosion resistance and service life.
The modified steel pipe treatment solution, including water, tetrabutyl titanate, ammonium persulfate and oxalic acid, is used to form a thin film and a micro-rough structure through surface treatment, which enhances the adhesion of the galvanized layer and has antibacterial properties.
It significantly improves the adhesion and antibacterial properties of the galvanized layer, extends the service life of stainless steel seamless steel pipes, and improves the comprehensive performance and market competitiveness of the product.
Smart Images

Figure CN118979249A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of stainless steel seamless pipes, in particular to a production process of stainless steel seamless pipes. Background Art
[0002] Galvanized stainless steel seamless pipes, as the preferred material for modern domestic water delivery systems, play a vital role in ensuring the purity and safety of water due to their excellent corrosion resistance, high strength and seamless structure. This type of steel pipe has undergone precise galvanizing treatment, which not only effectively resists the corrosion of chloride ions, microorganisms and other chemicals in the water, prolongs the service life of the pipe, but also ensures the cleanliness and hygiene of the water during long-term delivery.
[0003] The disclosure discloses a large-diameter seamless stainless steel pipe production process with the publication number CN115478268A, which is used to solve the problems that the existing large-diameter seamless stainless steel pipe is prone to pitting corrosion when in contact with chemicals, and the performance is reduced after corrosion, which does not meet the application requirements of large equipment. In addition, due to the large size of large-diameter composite pipes, the installation is very laborious, and the assembly and welding processes are difficult. The disclosure specifically relates to a large-diameter seamless stainless steel pipe production process; in the production process, anti-rust liquid is sprayed on the inner and outer walls of the large-diameter seamless stainless steel pipe blank, so that the large-diameter seamless stainless steel pipe has good corrosion resistance, ensuring that the large-diameter seamless stainless steel pipe can be used safely for a long time and reducing the number of maintenance and replacement of the large-diameter seamless stainless steel pipe.
[0004] When existing seamless stainless steel pipes are galvanized, the galvanized layer is difficult to adhere firmly because the surface of the seamless stainless steel pipe usually has high smoothness and stable chemical properties. Due to insufficient adhesion of the galvanized layer, the galvanized layer may fall off during use, affecting the corrosion resistance and service life of the steel pipe. Summary of the invention
[0005] 1. Technical issues to be resolved
[0006] In view of the deficiencies in the prior art, the present invention provides a production process for a stainless steel seamless steel pipe, which can significantly improve the coating adhesion of the stainless steel seamless steel pipe during the galvanizing process.
[0007] (II) Technical solution
[0008] To achieve the above object, the present invention provides the following technical solution: a production process of a seamless stainless steel pipe, specifically comprising the following steps:
[0009] a. Clean the stainless steel seamless pipe to remove surface oil and impurities;
[0010] b. Immerse the cleaned stainless steel seamless pipe in a modified steel pipe treatment solution for surface treatment, wherein the modified steel pipe treatment solution comprises: 80-90 parts by weight of water, 5-10 parts by weight of tetrabutyl titanate, 3-5 parts by weight of ammonium persulfate, and 0.5-1 parts by weight of oxalic acid;
[0011] c. Drying after surface treatment;
[0012] d. Galvanize the treated seamless stainless steel pipe.
[0013] Preferably, the proportion of water in the modified steel pipe treatment solution is 85 parts by weight.
[0014] Preferably, the proportion of tetrabutyl titanate in the modified steel pipe treatment solution is 7 parts by weight.
[0015] Preferably, the proportion of ammonium persulfate in the modified steel pipe treatment solution is 4 parts by weight.
[0016] Preferably, the proportion of oxalic acid in the modified steel pipe treatment solution is 0.7 parts by weight.
[0017] Preferably, the surface treatment time is 10-20 minutes.
[0018] Preferably, the drying temperature is 100-120°C.
[0019] Preferably, the preparation of the modified steel pipe treatment solution comprises the following steps:
[0020] S1. Raw material preparation: water: 80-90 parts by weight, tetrabutyl titanate: 5-10 parts by weight, ammonium persulfate: 3-5 parts by weight, and oxalic acid: 0.5-1 parts by weight;
[0021] S2. Add ammonium persulfate to a predetermined amount of water under stirring and continue stirring until it is completely dissolved;
[0022] S3, gradually adding oxalic acid to the above solution, and continuing to stir until the oxalic acid is completely dissolved;
[0023] S4. While stirring, slowly add tetrabutyl titanate to ensure uniform dispersion and prevent local over-concentration;
[0024] S5. Continue stirring the solution for at least 10 minutes to ensure that all components are fully mixed.
[0025] (III) Beneficial effects
[0026] Compared with the prior art, the present invention provides a production process for a seamless stainless steel pipe, which has the following beneficial effects:
[0027] 1. Through the treatment of the modified steel pipe treatment solution, the modified steel pipe treatment solution used in the present invention effectively changes the physical and chemical properties of the stainless steel surface through the synergistic effect of tetrabutyl titanate, ammonium persulfate and oxalic acid, so that the galvanized layer can be more firmly attached to the surface of the steel pipe. Tetrabutyl titanate is one of the main components. Tetrabutyl titanate can form a thin film on the surface of the steel pipe, improve the surface roughness and activity, thereby enhancing the adhesion of the galvanized layer. Ammonium persulfate is oxidizing and can slightly oxidize the surface of the steel pipe to further increase the surface adhesion performance. Oxalic acid can remove oxides and dirt on the surface, improve the surface cleanliness, and further improve the adhesion effect of the galvanized layer.
[0028] 2. By adding tetrabutyl titanate, the film formed by tetrabutyl titanate on the surface of the steel pipe has natural antibacterial properties and can inhibit the growth and reproduction of bacteria. After the modified steel pipe is treated with the solution, a micron-level rough structure is formed on the surface of the steel pipe. This structure can prevent the attachment and growth of bacteria and achieve an antibacterial effect. Since the antibacterial performance is achieved by changing the physical and chemical properties of the surface, rather than relying on volatile or leached antibacterial agents, it has better long-term stability and durability. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a flow chart of a production process of a stainless steel seamless steel pipe;
[0030] Figure 2 The present invention is a flowchart of the preparation process of a modified steel pipe treatment solution in the production process of a stainless steel seamless steel pipe. DETAILED DESCRIPTION
[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0032] Tetrabutyl titanate is used as a raw material for preparing a modified steel pipe treatment solution in the present invention. Tetrabutyl titanate (TBT) is an important organic titanium compound widely used in the fields of chemical synthesis and material surface modification. In the present invention, tetrabutyl titanate is used as a key component of the modified steel pipe treatment solution, and by forming a uniform film on the surface of a stainless steel seamless steel pipe, the roughness and chemical activity of the steel pipe surface are greatly improved. This film not only enhances the adhesion of the galvanized layer, but also gives the stainless steel seamless steel pipe excellent antibacterial properties due to its unique physical and chemical properties. In addition, tetrabutyl titanate can synergize with other components during the treatment process to effectively remove impurities and oxides on the surface of the steel pipe, further improving the effect of the surface treatment. Therefore, the application of tetrabutyl titanate in the present invention not only solves the shortcomings of traditional surface treatment methods, but also opens up new application prospects for stainless steel seamless steel pipes.
[0033] Using ammonium persulfate as the raw material for preparing the modified steel pipe treatment solution, ammonium persulfate (APS) is a strong oxidant, commonly used in chemical synthesis, polymerization initiator and surface treatment and other fields. In the stainless steel seamless steel pipe production process of the present invention, ammonium persulfate, as an important component of the modified steel pipe treatment solution, effectively removes oxides and other impurities on the steel pipe surface through its strong oxidation, and increases the cleanliness and activity of the surface. The oxidizing ability of ammonium persulfate forms a microscopic rough structure on the steel pipe surface, which not only helps the firm attachment of the zinc coating, but also inhibits the attachment and growth of bacteria to a certain extent. In addition, the use of ammonium persulfate is simple and efficient, not only can significantly improve the surface state of the steel pipe in a short time, but also will not introduce harmful substances, meet environmental protection requirements. Therefore, the application of ammonium persulfate in the present invention not only improves the zinc coating adhesion performance, but also indirectly enhances the antibacterial performance of the steel pipe, significantly improves the comprehensive performance and service life of the product.
[0034] Oxalic acid is used as the raw material for preparing the modified steel pipe treatment solution. Oxalic acid is an organic acid widely used in the fields of metal cleaning, rust removal and bleaching. In the stainless steel seamless steel pipe production process of the present invention, oxalic acid, as one of the key components of the modified steel pipe treatment solution, plays an important cleaning and activation role. Oxalic acid can effectively remove oxides and oil stains on the surface of the steel pipe, making the surface cleaner and providing an ideal substrate for the subsequent galvanizing process. Through oxalic acid treatment, the chemical properties of the steel pipe surface are optimized, and the adhesion of the galvanized layer is significantly improved. In addition, the use of oxalic acid can also improve the microstructure of the steel pipe surface, enhance its antibacterial properties, and prevent the attachment and reproduction of bacteria. The application of oxalic acid is not only simple and efficient, but also environmentally friendly and safe, and no harmful substances are introduced. Therefore, the application of oxalic acid in the present invention not only improves the surface quality and galvanizing adhesion performance of the stainless steel seamless steel pipe, but also unexpectedly gives it an antibacterial function, significantly improving the added value and market competitiveness of the product.
[0035] For the adhesion test of the galvanized layer, the method described in GB / T 5210-1985 "Determination of adhesion of coatings - Pull-off method" is used. The coating sample is fixed on the test device with an adhesive, and then a tensile force is applied until the coating is separated from the substrate. The required tensile force value is measured to evaluate the adhesion performance. This method can provide quantitative adhesion strength data.
[0036] The antibacterial performance test of stainless steel seamless pipes adopts the relevant standards of GB / T 3621-2018. These standards specify in detail the test methods and evaluation criteria for the antibacterial rate and antibacterial effect of stainless steel materials, ensuring the accuracy and reliability of the test results.
[0037] When testing the antibacterial performance of seamless stainless steel pipes, commonly used testing methods include microbial culture method, quantitative sterilization test and simulated field test, etc. The microbial culture method places the steel pipe sample in a culture medium containing specific pathogens (such as Escherichia coli, Staphylococcus aureus, etc.), and after a certain period of cultivation, the colony count before and after treatment is compared to calculate the antibacterial rate, thereby evaluating its antibacterial performance.
[0038] Embodiment 1:
[0039] A production process for a stainless steel seamless pipe comprises the following steps:
[0040] 1) Clean the stainless steel seamless pipe to remove surface oil and impurities;
[0041] 2) Immerse the cleaned stainless steel seamless pipe in a modified steel pipe treatment solution for surface treatment, and prepare the modified steel pipe treatment solution according to the following formula: 85 parts by weight of water, 7 parts by weight of tetrabutyl titanate, 4 parts by weight of ammonium persulfate, and 0.7 parts by weight of oxalic acid;
[0042] 21) Add ammonium persulfate to a predetermined amount of water under stirring and continue stirring until it is completely dissolved;
[0043] 22) Gradually add oxalic acid to the above solution and continue stirring until the oxalic acid is completely dissolved;
[0044] 23) While stirring, slowly add tetrabutyl titanate to ensure uniform dispersion and prevent local over-concentration;
[0045] 24) Continue stirring the solution for at least 10 minutes to ensure that all components are fully mixed;
[0046] 3) Immerse the cleaned steel pipe in the modified steel pipe treatment solution for 15 minutes;
[0047] 4) Dry the treated steel pipe at 110°C;
[0048] 5) Galvanizing is carried out after drying.
[0049] Embodiment 2:
[0050] A production process for a stainless steel seamless pipe comprises the following steps:
[0051] The specific steps include:
[0052] 1) Clean the stainless steel seamless pipe to remove surface oil and impurities;
[0053] 2) Immerse the cleaned stainless steel seamless pipe in a modified steel pipe treatment solution for surface treatment, and prepare the modified steel pipe treatment solution according to the following formula: 80 parts by weight of water, 10 parts by weight of tetrabutyl titanate, 3 parts by weight of ammonium persulfate, and 0.5 parts by weight of oxalic acid. The preparation steps of the modified steel pipe treatment solution are the same as those in Example 1;
[0054] 3) Immerse the cleaned steel pipe in the modified steel pipe treatment solution for 20 minutes;
[0055] 4) Dry the treated steel pipe at 120°C;
[0056] 5) Galvanizing is carried out after drying.
[0057] Embodiment three:
[0058] A production process for a stainless steel seamless pipe comprises the following steps:
[0059] 1) Clean the stainless steel seamless pipe to remove surface oil and impurities;
[0060] 2) Immerse the cleaned stainless steel seamless steel pipe in a modified steel pipe treatment solution for surface treatment, and prepare the modified steel pipe treatment solution according to the following formula: 90 parts by weight of water, 5 parts by weight of tetrabutyl titanate, 5 parts by weight of ammonium persulfate, and 1 part by weight of oxalic acid. The preparation steps of the modified steel pipe treatment solution are the same as those in Example 1;
[0061] 3) Immerse the cleaned steel pipe in the modified steel pipe treatment solution for 10 minutes;
[0062] 4) Dry the treated steel pipe at 100°C;
[0063] 5) Galvanizing is carried out after drying.
[0064] Embodiment 4:
[0065] A production process for a stainless steel seamless pipe comprises the following steps:
[0066] 1) Clean the stainless steel seamless pipe to remove surface oil and impurities;
[0067] 2) Immerse the cleaned stainless steel seamless steel pipe in a modified steel pipe treatment solution for surface treatment, and prepare the modified steel pipe treatment solution according to the following formula: 88 parts by weight of water, 8 parts by weight of tetrabutyl titanate, 4 parts by weight of ammonium persulfate, and 0.8 parts by weight of oxalic acid. The preparation steps of the modified steel pipe treatment solution are the same as those in Example 1;
[0068] 3) Immerse the cleaned steel pipe in the modified steel pipe treatment solution for 12 minutes;
[0069] 4) Dry the treated steel pipe at 115°C;
[0070] 5) Galvanizing is carried out after drying.
[0071] Embodiment five:
[0072] A production process for a stainless steel seamless pipe comprises the following steps:
[0073] 1) Clean the stainless steel seamless pipe to remove surface oil and impurities;
[0074] 2) Immerse the cleaned stainless steel seamless pipe in a modified steel pipe treatment solution for surface treatment, and prepare the modified steel pipe treatment solution according to the following formula: 87 parts by weight of water, 6 parts by weight of tetrabutyl titanate, 4 parts by weight of ammonium persulfate, and 0.6 parts by weight of oxalic acid. The preparation steps of the modified steel pipe treatment solution are the same as those in Example 1;
[0075] 3) Immerse the cleaned steel pipe in the modified steel pipe treatment solution for 18 minutes;
[0076] 4) Dry the treated steel pipe at 105°C;
[0077] 5) Galvanizing is carried out after drying.
[0078] Comparative Example 1:
[0079] The treatment solution of the modified steel pipe in Example 2 is removed, and the other steps are the same as those in Example 2.
[0080] Comparative Example 2:
[0081] 1) Clean the stainless steel seamless pipe to remove surface oil and impurities;
[0082] 2) Immerse the cleaned stainless steel seamless pipe in a modified steel pipe treatment solution for surface treatment, and prepare the modified steel pipe treatment solution according to the following formula: 85 parts by weight of water, 7 parts by weight of tetrabutyl titanate, and 4 parts by weight of ammonium persulfate;
[0083] 21) Add ammonium persulfate to a predetermined amount of water under stirring and continue stirring until it is completely dissolved;
[0084] 22) While stirring, slowly add tetrabutyl titanate to ensure uniform dispersion and prevent local over-concentration;
[0085] 23) Continue stirring the solution for at least 10 minutes to ensure that all components are fully mixed;
[0086] 3) Immerse the cleaned steel pipe in the modified steel pipe treatment solution for 15 minutes;
[0087] 4) Dry the treated steel pipe at 110°C;
[0088] 5) Galvanizing is carried out after drying.
[0089] The coating adhesion performance and antibacterial performance of multiple samples in Examples 1, 2, 3, 4, 5 and Comparative Examples 1 and 2 were tested respectively using the test method described in GB / T 5210-1985 "Determination of Coating Adhesion by Pull-Off Method" and the test method using the relevant standard GB / T 3621-2018, and the average value was taken. The larger the value of the coating adhesion performance test result, the better the coating adhesion performance, and vice versa. The higher the percentage value of the antibacterial performance test result, the better the antibacterial effect, and vice versa.
[0090] Table 1. Test results of coating adhesion and antibacterial properties of Examples 1-5 and Comparative Examples 1-2
[0091] Test items Embodiment 1 Embodiment 2 Embodiment 3 Embodiment 4 Embodiment 5 Comparative Example 1 Comparative Example 2 Coating adhesion performance (N) 80.3 85.1 75.9 78.6 82.5 51.3 62.1 Antibacterial performance (%) 95.6 96.1 93.8 98.3 93.1 12.6 13.2
[0092] In summary, the test results of the present invention show that the stainless steel seamless steel pipe treated with the modified steel pipe treatment solution has significantly improved coating adhesion after galvanizing and has excellent antibacterial properties. The performance of Comparative Examples 1 and 2 in these two aspects is significantly lower than that of the embodiment, which proves the effectiveness and superiority of the method of the present invention.
[0093] The above are only specific embodiments of the present invention, but the technical features of the present invention are not limited thereto. Any simple changes, equivalent replacements or modifications made based on the present invention to solve basically the same technical problems and achieve basically the same technical effects are all included in the protection scope of the present invention.
Claims
1. A production process for a seamless stainless steel pipe, characterized in that: The specific steps include: a. Clean the stainless steel seamless pipe to remove surface oil and impurities; b. Immerse the cleaned stainless steel seamless pipe in a modified steel pipe treatment solution for surface treatment, wherein the modified steel pipe treatment solution comprises: 80-90 parts by weight of water, 5-10 parts by weight of tetrabutyl titanate, 3-5 parts by weight of ammonium persulfate, and 0.5-1 parts by weight of oxalic acid; c. Drying after surface treatment; d. Galvanize the treated seamless stainless steel pipe.
2. The production process of a stainless steel seamless pipe according to claim 1, characterized in that: The proportion of water in the modified steel pipe treatment solution is 85 parts by weight.
3. The production process of a stainless steel seamless pipe according to claim 1, characterized in that: The proportion of tetrabutyl titanate in the modified steel pipe treatment solution is 7 parts by weight.
4. The production process of a stainless steel seamless pipe according to claim 1, characterized in that: The proportion of ammonium persulfate in the modified steel pipe treatment solution is 4 parts by weight.
5. The production process of a stainless steel seamless pipe according to claim 1, characterized in that: The proportion of oxalic acid in the modified steel pipe treatment solution is 0.7 parts by weight.
6. The production process of a stainless steel seamless pipe according to claim 1, characterized in that: The surface treatment time is 10-20 minutes.
7. The production process of a stainless steel seamless pipe according to claim 1, characterized in that: The drying temperature is 100-120°C.
8. The production process of a stainless steel seamless pipe according to claim 1, characterized in that: The preparation of the modified steel pipe treatment solution comprises the following steps: S1. Raw material preparation: water: 80-90 parts by weight, tetrabutyl titanate: 5-10 parts by weight, ammonium persulfate: 3-5 parts by weight, and oxalic acid: 0.5-1 parts by weight; S2. Add ammonium persulfate to a predetermined amount of water under stirring and continue stirring until it is completely dissolved; S3, gradually adding oxalic acid to the above solution, and continuing to stir until the oxalic acid is completely dissolved; S4. While stirring, slowly add tetrabutyl titanate to ensure uniform dispersion and prevent local over-concentration; S5. Continue stirring the solution for at least 10 minutes to ensure that all components are fully mixed.