Preparation method of high-performance photoelectrocatalysis silicon photo-anode

By using the reaction electron beam evaporation method to prepare CuO intermediate layer and NiCoFe-Bi cocatalysts at the interface of the silicon-based photoanode, the problem of low water oxidation reaction efficiency of the silicon-based photoanode is solved, and efficient photoelectrocatalytic water decomposition performance is achieved. , achieving a half-cell solar hydrogen production efficiency of 4.56%.

CN118979270AActive Publication Date: 2024-11-19UNIV OF ELECTRONICS SCI & TECH OF CHINA
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411044152.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The existing silicon-based photoanode has low efficiency in water oxidation reaction in photoelectric catalytic water decomposition, resulting in large energy loss and making it difficult to achieve commercial application.

Method used

CuO intermediate layer was prepared on the interface of the n-Si photoanode by reacting electron beam evaporation, and combined with NiO and NiCoFe-Bi cocatalysts, the interface energy state was optimized to improve the photoelectrocatalytic performance.

Benefits of technology

The performance of photoelectric catalytic water decomposition has been significantly improved, and the efficiency of half-cell solar hydrogen production has been improved, reaching the current highest 4.56%, meeting the requirements of commercial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979270A_ABST
    Figure CN118979270A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of photoelectrocatalysis water decomposition, and particularly relates to a preparation method of a high-performance photoelectrocatalysis silicon photo-anode. A CuO intermediate layer film, a NiO film and a NiCoFe-Bi cocatalyst layer on the surface of the n-Si photo-anode are prepared by adopting a reaction electron beam evaporation deposition system, a common electron beam evaporation deposition system and a photo-assisted electrochemical deposition method in sequence. In the preparation process, the flow of O2 introduced into a reaction electron beam evaporation deposition system is controlled, and the formation of a CuO phase in an intermediate layer film is controlled, so that the NiO / n-Si heterojunction photo-anode interface is effectively regulated and controlled, the generation of higher photovoltage on an n-Si photo-anode is promoted, and the photoelectrocatalytic water decomposition performance of the n-Si photo-anode is further remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of photoelectrocatalytic water decomposition, and specifically relates to a method for preparing a high-performance photoelectrocatalytic silicon photoanode. Background Art

[0002] Photoelectrocatalytic (PEC) water splitting technology is a method that can directly convert solar energy into hydrogen energy. It is one of the ideal ways to transform the global energy structure into a green, efficient and sustainable one. PEC water splitting technology usually consists of the hydrogen evolution reaction (HER) at the cathode and the oxygen evolution reaction (OER) at the anode. The slow four-electron transfer process in OER causes more energy loss and is the main limiting factor of the overall water splitting reaction. Therefore, the study of water oxidation reaction on the photoanode surface is the basis for the commercialization of PEC water splitting technology.

[0003] As the mainstream semiconductor material on the market, single crystal silicon is widely used in photovoltaics and microelectronics. Due to its abundant reserves on the earth, it can be produced on a large scale, has high theoretical current density, excellent carrier mobility and carrier diffusion length, etc., it can be used as a model for the study of photoelectrode surface / interface in PEC water splitting for strategic development. Since the energy band position of single crystal silicon is not conducive to the water oxidation reaction, its photovoltage is low and the starting position is high. In order to obtain high PEC activity, it is usually necessary to use an appropriate interface layer to adjust the energy state of the buried interface. The interface layer can optimize the band edge (valence band top / conduction band bottom) position between the semiconductor and the protective layer / co-catalyst layer, promote the transfer of holes from the semiconductor to the surface active sites, and thus effectively drive the OER process.

[0004] Currently, the most advanced n-type silicon (n-Si) photoanode devices usually use NiO x 、CoO x SnO x and NiCoO x Lewis et al. pioneered the use of CoO x The intermediate layer is introduced into NiO x A stable saturated photocurrent of up to 1700 hours was achieved in the interface of the n-Si / n-Si heterojunction photoanode, but the half-cell solar hydrogen production efficiency (HC-STH) of the device was only 2.2%. The most efficient silicon-based photoanode in the prior art is achieved by using SnO between the n-Si light absorber and the Ni-based OER catalyst. xThe intermediate layer achieved a 4.1% HC-STH, but this efficiency is still far below the minimum requirement of 10% for commercial applications. These groundbreaking research results highlight the importance of interface engineering for improving the efficiency of silicon-based photoanodes. Nevertheless, how to achieve efficient PEC water oxidation on n-Si photoanodes still requires the exploration of energy-matched and chemically stable interfaces. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a high-performance photoelectrocatalytic silicon photoanode in response to the problems or shortcomings existing in the above-mentioned prior art, in which a CuO intermediate layer film is prepared by reactive electron beam evaporation and introduced into the interface of a NiO / n-Si heterojunction photoanode, thereby improving its performance.

[0006] To achieve the above object, the present invention adopts the following technical solution:

[0007] A method for preparing a high-performance photoelectrocatalytic silicon photoanode comprises the following steps:

[0008] Step 1, the n-Si wafer is ultrasonically cleaned using acetone and isopropanol in sequence, and then blown dry;

[0009] Step 2: Cu 2 O was used as the Cu source, and a CuO intermediate layer was prepared on the n-Si wafer using a reactive electron beam evaporation device;

[0010] Step 3, using NiO as a Ni source, and depositing a NiO film on the structure obtained in step 2 using an electron beam evaporation device;

[0011] Step 4: Use TEM, XPS, UPS and other characterization methods to analyze the morphology, phase and band structure of the structure obtained in step 3. If the analysis results meet the preset standards, proceed to step 5;

[0012] Step 5, after etching the back of the sample obtained in step 3 with a 5%-20% HF solution, rinse it with deionized water, and apply indium-gallium (In-Ga) liquid alloy on the etched surface, and use silver paste to connect the indium-gallium alloy on the back of the n-Si sample obtained in step 3 to the wire, and then use epoxy resin to encapsulate it;

[0013] Step 6: Use a three-electrode system to conduct NiCoFe-B i Light-assisted electrochemical deposition of oxygen evolution promoters, after deposition is complete, rinse thoroughly with deionized water;

[0014] Step 7: Use a three-electrode system to perform PEC water splitting test and evaluation on the structure obtained in step 6.

[0015] Furthermore, in step 2, Cu2 O is used as the Cu source, and the conditions for preparing a CuO intermediate layer on the n-Si wafer using a reactive electron beam evaporation device are:

[0016] The equipment needs to be evacuated to a vacuum degree of 5×10 -6 Torr;

[0017] During the preparation of the CuO intermediate layer, O was introduced at a gas flow rate of 0-17 sccm. 2 The vacuum degree of the chamber corresponding to different gas flow rates is: 2.0×10 -5 -2.1×10 -4 Torr, so that the evaporated Cu 2 O particles are oxidized to CuO particles and deposited on n-Si wafers to prepare a CuO intermediate layer;

[0018] The deposition rate of the CuO film is The deposition thickness is

[0019] Furthermore, in step 3, NiO is used as a Ni source, and an electron beam evaporation device is used to deposit a NiO film on the structure obtained in step 2, and the conditions include:

[0020] No need 2 The air flow is introduced and the deposition rate is The deposition thickness is

[0021] Furthermore, the step 6 uses a three-electrode system to perform NiCoFe-B on the structure obtained in step 5. i The method of light-assisted electrochemical deposition of oxygen evolution promoter comprises:

[0022] (1) Potassium borate with a pH value of 10 is used as a buffer solution;

[0023] (2) Argon was introduced into the buffer solution and stirring was started, followed by addition of 0.5 mM Co(NO 3 ) 2 6H 2 O, 2 mM NiSO 4 6H 2 O and 0.8 mM FeSO 4 7H 2 O makes it an ion source;

[0024] (3) irradiating the product obtained in (2) with simulated sunlight, with the irradiation intensity maintained at 100 mW·cm -2 , with 10-50μA·cm -2 At a constant current density, NiCoFe-B iThe oxygen evolution promoter is deposited onto the surface of the structure obtained in step 5.

[0025] Furthermore, the buffer solution contains H 3 BO 3 It is prepared with KOH at a concentration ratio of 1:0.6.

[0026] The present invention uses a reactive electron beam evaporation deposition system, a common electron beam evaporation deposition system, and a light-assisted electrochemical deposition method to prepare a CuO intermediate layer film, a NiO film, a NiCoFe-B film on the surface of an n-Si photoanode. i During the preparation process, the reaction electron beam evaporation deposition system is controlled to pass O 2 The gas flow rate is controlled to control the formation of CuO phase in the intermediate layer film, so as to achieve effective regulation of the NiO / n-Si heterojunction photoanode interface, promote the generation of a larger photovoltage on the n-Si photoanode, and thus significantly improve the photoelectrocatalytic water splitting performance of the n-Si photoanode (see Figure 6 and Figure 7 ). BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a schematic diagram of the working principle of the reactive electron beam evaporation deposition system;

[0028] Figure 2 NiO / Cu x HR-TEM cross-sectional image of O / n-Si sample;

[0029] Figure 3 NiO / Cu x Elemental analysis of O / n-Si samples using TEM analysis EDS in STEM mode; a is a dark field STEM cross-sectional view, and b is an elemental analysis using TEM analysis EDS in STEM mode (including four elements: Si, Cu, Ni, and O);

[0030] Figure 4 To introduce different gas flow rates O 2 Cu prepared by reactive electron beam evaporation equipment x XPS phase characterization of O thin film; where a is the amount of O 2 Cu prepared with a gas flow rate of 0 sccm x O thin film (Cu 2 O phase), b is the O 2 Cu prepared with a gas flow rate of 17 sccm x O thin film (CuO phase);

[0031] Figure 5 Cu x Characterization of UPS band structure of O film; where a is Cu2 O film, b is the UPS spectrum of CuO film;

[0032] Figure 6 The band structure diagram of n-Si photoanode; a is NiO / Cu 2 Energy band diagram of O / n-Si photoanode in dark state, b is NiCoFe-B i / NiO / Cu 2 The energy band diagram of O / n-Si photoanode under light, c is the energy band diagram of NiO / CuO / n-Si photoanode in the dark state, d is the energy band diagram of NiCoFe-B i Energy band diagram of / NiO / CuO / n-Si photoanode under light irradiation;

[0033] Figure 7 The performance diagram of n-Si photoanode PEC water splitting, where a is the 2 NiCoFe-B with CuO interlayer deposited under gas flow i a is the J-V curve of / NiO / CuO / n-Si photoanode, b is the HC-STH corresponding to the J-V curve in a, and c is the statistics of the highest HC-STH recorded for silicon photoanodes. DETAILED DESCRIPTION

[0034] The technical solution of the present invention is described in detail below in conjunction with the accompanying drawings and embodiments.

[0035] Example 1

[0036] A method for preparing a high-performance photoelectrocatalytic silicon photoanode comprises the following steps:

[0037] Step 1: The n-Si wafer was ultrasonically cleaned using acetone and isopropanol for 10 minutes respectively, and then dried using nitrogen.

[0038] Step 2: Cu 2 O as a Cu source was placed in the crucible tank of the reactive electron beam evaporation equipment, and the n-Si wafer obtained in step 1 was placed in the sample stage of the electron beam evaporation equipment. The system was evacuated to a vacuum degree of 5×10 -6 Torr; O 2 The vacuum degree of the deposition chamber under the working conditions of the chamber is: 2.1×10 -4 Torr. When the Cu source in the crucible is evaporated into the chamber, it will react with the introduced O 2 The reaction takes place, and the Cu 2 O particles are oxidized to CuO particles and deposited on n-Si wafers to prepare a CuO intermediate layer (see Figure 1). A quartz crystal microbalance was used to detect the deposition rate and thickness of the CuO film. The deposition rate of CuO is The deposition thickness is

[0039] Step 3: NiO is then used as a Ni source to deposit a NiO film on the structure obtained in step 2 using an electron beam evaporation device; this process does not require O 2 A quartz crystal microbalance was used to detect the deposition rate and thickness of the NiO film. The deposition rate was The deposition thickness is

[0040] Step 4: Use TEM, XPS, UPS and other characterization methods to analyze the morphology, phase and band structure of the structure obtained in step 3. Figure 2-Figure 6 If the analysis result reaches the preset standard, go to step 5.

[0041] Step 5: Use 10% HF solution to etch the back of the sample obtained in step 3, rinse it with deionized water, and apply indium-gallium (In-Ga) liquid alloy on the etched surface. Use silver paste to connect the indium-gallium alloy on the back of the n-Si sample obtained in step 3 to the wire, and then encapsulate it with epoxy resin.

[0042] Step 6: Use a three-electrode system to conduct NiCoFe-B i Light-assisted electrochemical deposition of oxygen evolution promoter. The deposition process uses potassium borate with a pH value of 10 as a buffer solution. The buffer solution in this embodiment is H 3 BO 3 and KOH in a concentration ratio of 1:0.6. Before deposition, high-purity argon gas was introduced into the buffer solution and stirring was started, followed by the addition of 0.5 mM Co(NO 3 ) 2 6H 2 O, 2 mM NiSO 4 6H 2 O and 0.8 mM FeSO 4 7H 2 O was used as the ion source. The irradiation intensity was kept at 100 mW·cm -2 , at 30μA·cm -2 The constant current density of NiCoFe-B i The oxygen evolution promoter is deposited onto the surface of the n-Si photoanode. After the deposition is completed, the surface of the n-Si photoanode is thoroughly rinsed with deionized water.

[0043] Step 7: Use a three-electrode system to perform PEC water splitting test and evaluation on the structure obtained in step 6.

[0044] Example 2

[0045] Same as Example 1, except that: the O introduced into the reaction electron beam evaporation device during the deposition of the CuO film 2 The gas flow rate is set to 5 sccm, and the PEC water splitting test is shown in Figure 7 .

[0046] Example 3:

[0047] Same as Example 1, except that: the O introduced into the reaction electron beam evaporation device during the deposition of the CuO film 2 The gas flow rate is set to 0 sccm, and the PEC water splitting test is shown in Figure 7 .

[0048] The product obtained in Example 1 was used as a sample to verify the technical effect:

[0049] Figure 2 This is a cross-sectional image of the n-Si sample obtained by HR-TEM. Figure 2 It can be clearly observed that NiO / Cu x The layered structure of the O / n-Si sample indicates the uniformity of the thin film prepared by electron beam evaporation equipment.

[0050] Figure 3 (a)- Figure 3 (b) Elemental analysis of n-Si sample using TEM analysis EDS in STEM mode. Figure 3 (a)- Figure 3 (b) NiO / Cu x The layered element distribution of O / n-Si samples shows that Cu x O interlayer was successfully inserted between NiO film and n-Si wafer.

[0051] Figure 4 (a)- Figure 4 (b) Different gas flow rates O 2 Cu prepared by reactive electron beam evaporation equipment x XPS phase characterization of O thin film. Figure 4 (a)- Figure 4 (b) It can be seen that as O is introduced into the reaction electron beam evaporation device, 2 With the increase of gas flow, the prepared Cu x O thin film composed of Cu 2 The O phase (0 sccm) transforms into the CuO phase (17 sccm).

[0052] Figure 5 (a)- Figure 5 (b) Cu x Characterization of UPS band structure of O film. Figure 5 (a)- Figure 5 (b) It can be seen that the Fermi level of CuO film (17 sccm) is lower than that of Cu 2 O film (0sccm) Fermi level.

[0053] Figure 6 (a)- Figure 6 (d) is the energy band structure diagram of n-Si photoanode in dark state / under illumination. Figure 6 (a)- Figure 6 (d) It can be seen that the Fermi level difference between CuO semiconductor and n-Si semiconductor is greater than that of Cu 2 The Fermi level difference between O semiconductor and n-Si semiconductor increases the barrier (Φ B ), which in turn increases the photovoltage (V ph ) is produced, ultimately reducing the applied bias voltage for water oxidation reaction.

[0054] Figure 7 (a)- Figure 7 (c) is the performance diagram of n-Si photoanode PEC water splitting, Figure 7 (a)- Figure 7 (c) It can be seen that as O is introduced into the reaction electron beam evaporation device, 2 With the increase of gas flow, the PEC performance of n-Si photoanode is significantly improved. i / NiO / CuO / n-Si photoanode (17 sccm) achieved the current highest HC-STH value of 4.56%.

[0055] It is to be understood that the present invention is described by some embodiments, and it is known to those skilled in the art that various changes or equivalent substitutions may be made to these features and embodiments without departing from the spirit and scope of the present invention. In addition, under the teachings of the present invention, these features and embodiments may be modified to adapt to specific circumstances and materials without departing from the spirit and scope of the present invention. Therefore, the present invention is not limited by the specific embodiments disclosed herein, and all embodiments falling within the scope of the claims of this application are within the scope of protection of the present invention.

Claims

1. A method for preparing a high-performance photoelectrocatalytic silicon photoanode. It is characterized in that The following steps are involved: Step 1, the n-Si wafer is ultrasonically cleaned using acetone and isopropanol in sequence, and then blown dry; Step 2: Cu 2 O was used as Cu source, and a CuO intermediate layer was prepared on the n-Si wafer using a reactive electron beam evaporation device; Step 3, using NiO as a Ni source, and depositing a NiO film on the structure obtained in step 2 using an electron beam evaporation device; Step 4: Use TEM, XPS, UPS and other characterization methods to analyze the morphology, phase and band structure of the structure obtained in step 3. If the analysis results meet the preset standards, proceed to step 5; Step 5, after etching the back of the sample obtained in step 3 with a 5%-20% HF solution, rinse it with deionized water, and apply indium-gallium (In-Ga) liquid alloy on the etched surface, and use silver paste to connect the indium-gallium alloy on the back of the n-Si sample obtained in step 3 to the wire, and then use epoxy resin to encapsulate it; Step 6: Use a three-electrode system to conduct NiCoFe-B i Light-assisted electrochemical deposition of oxygen evolution promoters, after deposition is complete, rinse thoroughly with deionized water; Step 7: Use a three-electrode system to perform PEC water splitting test and evaluation on the structure obtained in step 6.

2. A method for preparing a high-performance photoelectrocatalytic silicon photoanode according to claim 1, It is characterized in that In step 2, Cu 2 O is used as the Cu source, and the conditions for preparing a CuO intermediate layer on the n-Si wafer using a reactive electron beam evaporation device are: The equipment needs to be evacuated to a vacuum degree of 5×10 -6 Torr; During the preparation of the CuO intermediate layer, O was introduced at a gas flow rate of 0-17 sccm. 2 The vacuum degree of the chamber corresponding to different gas flow rates is: 2.0×10 -5 -2.1×10 -4 Torr, so that the evaporated Cu 2 O particles are oxidized to CuO particles and deposited on n-Si wafers to prepare a CuO intermediate layer; The deposition rate of the CuO film is The deposition thickness is 3. A method for preparing a high-performance photoelectrocatalytic silicon photoanode according to claim 1, It is characterized in that In step 3, NiO is used as a Ni source, and an electron beam evaporation device is used to deposit a NiO film on the structure obtained in step 2, and the deposition rate is The deposition thickness is 4. A method for preparing a high-performance photoelectrocatalytic silicon photoanode according to claim 1, It is characterized in that The step 6 uses a three-electrode system to conduct NiCoFe-B i The method of light-assisted electrochemical deposition of oxygen evolution promoter comprises: (1) Potassium borate with a pH value of 10 is used as a buffer solution; (2) Argon was introduced into the buffer solution and stirring was started, followed by addition of 0.5 mM Co(NO 3 ) 2 6H 2 O, 2 mM NiSO 4 6H 2 O and 0.8 mM FeSO 4 7H 2 O makes it an ion source; (3) irradiating the product obtained in (2) with simulated sunlight, with the irradiation intensity maintained at 100 mW·cm -2 , with 10-50μA·cm -2 At a constant current density, NiCoFe-B i The oxygen evolution promoter is deposited onto the surface of the structure obtained in step 5.

5. A method for preparing a high-performance photoelectrocatalytic silicon photoanode according to claim 4, It is characterized in that The buffer solution contains H 3 BO 3 It is prepared with KOH in a concentration ratio of 1:0.6.

Citation Information

Patent Citations

  • A / B / Si ternary composite silicon-based photoelectrode with bionic structure and preparation method of A / B / Si ternary composite silicon-based photoelectrode

    CN112680748A