Aluminum alloy antenna surface functional coating and preparation method thereof

By preparing functional coatings containing chromate and aluminum trioxide on the surface of aluminum alloy antenna, combined with electrochemical oxidation and anodization processes, the problem of poor surface oxidation and corrosion resistance of aluminum alloy materials is solved, and high-precision thermal It has a control and anti-salt spray function, suitable for complex structure antennas and sea environments.

CN118979298APending Publication Date: 2024-11-19CHINA ELECTRONIC TECH GRP CORP NO 38 RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411085841.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The surface oxidation of conventional aluminum alloy materials leads to low hemispherical emissivity and poor corrosion resistance. The solar absorption ratio of existing thermal control coatings is less than 0.35, and it is impossible to achieve the thermal control performance requirements of both emissivity and absorption ratio of 0.70, especially in the It is difficult to achieve spatial thermal control and anti-salt spray functions in the sub-array antenna.

Method used

Using aluminum alloy antenna surface functional coating, including conductive coatings containing chromate and its hydrates and thermally controlled coatings containing aluminum oxide, prepared by specific electrochemical oxidation and anodizing processes, combining insulation protection and chemical impregnation By etching treatment, a coating with high-precision thermal control performance and salt spray corrosion resistance was prepared.

Benefits of technology

It realizes high-precision thermal control performance with the surface radiation absorption ratio of aluminum alloy antennas tending to 1, and has both electrical performance requirements and salt spray resistance in the sea environment, solving the problems of ground protection and space thermal control of aluminum alloy array antennas, and The preparation method is simple, the materials are easy to obtain, and it is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979298A_ABST
    Figure CN118979298A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of subarray antennas, in particular to an aluminum alloy antenna surface functional coating and a preparation method thereof.The aluminum alloy antenna surface functional coating comprises a conductive coating and a thermal control coating; wherein the conductive coating contains chromate and a hydrate thereof; and the thermal control coating contains aluminum oxide. The functional coating on the surface of the aluminum alloy antenna has good space environment adaptability and high-precision thermal control performance, the radiation absorption ratio of the thermal control coating tends to be 1, the conductive coating has the electrical performance requirement of the antenna and the sea area environment storage salt mist prevention requirement at the same time, and the technical problems of ground protection, space thermal control and the like of the aluminum alloy subarray antenna are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of subarray antennas, and in particular to a functional coating on the surface of an aluminum alloy antenna and a preparation method thereof. Background Art

[0002] Conventional aluminum alloy materials have a hemispherical emissivity of about 0.20 due to natural oxidation on the surface, and have poor corrosion resistance when stored on the ground, with a neutral salt spray test resistance of less than 24 hours. At present, thermal control coatings prepared by organic white paint, OSR, flexible thermal control coatings, and aluminum alloy anodizing methods used in China have a high hemispherical emissivity (ε H 0.70 or more), the solar absorption rate is only below 0.30; the aluminum alloy antenna design involved in the present invention requires the coating to have a hemispherical emissivity ε H 0.70, while having a thermal control state with a radiation absorption ratio close to 1, maintaining the local conductivity of the antenna, and having salt spray resistance for ground storage in coastal environments.

[0003] Aluminum and its alloys are prepared by in-situ growth of alumina inorganic coating on the surface of aluminum alloy by electrochemical oxidation under the corresponding electrolyte and specific process conditions, using the effect of impressed current. This method has been used on many satellite models in China to develop thermal control coatings for aluminum alloy antennas. The solar absorption ratio of the coating obtained is lower than 0.35, which cannot simultaneously meet the thermal control performance requirements of 0.70 for both emissivity and absorption ratio. There is a big difference with the indicators required by this aluminum alloy antenna.

[0004] Due to the special processing characteristics and structural form of the sub-array antenna, it is difficult to implement methods such as pasting OSR, vacuum coating and wrapping flexible thermal control coating, and it cannot meet the communication function, which limits the use of thermal control coating technology. At the same time, due to the technical blockade of Western countries against my country, the thermal control coating on the antenna surface cannot be imported. Therefore, the development of functional coating for sub-array antenna is an important problem and key task to achieve the multi-functions of this antenna, such as spatial thermal control, electrical performance requirements, and salt spray protection in marine environment storage. Summary of the invention

[0005] The purpose of the present invention is to solve the problems that the surface of conventional aluminum alloy materials will be oxidized, the hemispherical emissivity is low, and the corrosion resistance is poor. At the same time, the solar absorption ratio of the thermal control coating of the aluminum alloy antenna prepared by the prior art is lower than 0.35, and the thermal control performance requirements of both the emissivity and the absorption ratio of 0.70 cannot be achieved at the same time. Thus, a functional coating on the surface of an aluminum alloy antenna and a preparation method thereof are provided. The functional coating on the surface of the aluminum alloy antenna has good adaptability to space environment and high-precision thermal control performance. The thermal control coating has a radiation absorption ratio approaching 1, and the conductive coating has both the electrical performance requirements of the antenna and the salt spray protection requirements for storage in the sea environment, thereby solving the technical problems of ground protection and space thermal control of aluminum alloy subarray antennas.

[0006] In order to achieve the above-mentioned object, in a first aspect, the present invention provides a functional coating on the surface of an aluminum alloy antenna, wherein the functional coating on the surface of the aluminum alloy antenna comprises: a conductive coating and a thermal control coating; wherein:

[0007] The conductive coating contains chromate and its hydrate;

[0008] The thermal control coating contains aluminum oxide.

[0009] Preferably, the aluminum alloy antenna material grade is 5A06.

[0010] Preferably, the neutral salt spray resistance time of the functional coating on the surface of the aluminum alloy antenna is 192 hours, wherein the neutral salt spray resistance time is tested according to the provisions of the neutral salt spray test in the national military standard GJB150.11A.

[0011] In a second aspect, the present invention provides a method for preparing a functional coating on the surface of an aluminum alloy antenna, the preparation method comprising: first activating the aluminum alloy antenna, preparing a conductive coating, first washing, first drying, insulating protection, pretreatment, preparing a thermal control coating, second washing, sealing treatment, second drying, and removing insulating protection.

[0012] Preferably, the method for preparing the conductive coating comprises: placing the aluminum alloy antenna after the first activation into a conductive oxidation solution at a temperature of 15-35° C. for 2-5 minutes.

[0013] Preferably, the conductive oxidizing solution contains chromic anhydride, ammonium bifluoride, potassium ferrocyanide and Al 3+ .

[0014] More preferably, the mass concentration ratio of the chromic anhydride, ammonium bifluoride and potassium ferrocyanide is 10:3:2, wherein the mass concentration of the chromic anhydride is 3-6 g / L.

[0015] Further preferably, the Al 3+ The mass concentration is 3-20g / L, wherein the Al 3+ It is produced by the reaction of aluminum alloy antenna and chromic anhydride.

[0016] Preferably, the method for preparing the thermal control coating comprises: placing the pretreated aluminum alloy antenna into an aluminum alloy anodizing solution for oxidation at a temperature of 16-18° C. for 20-22 minutes at a voltage of 10-14V.

[0017] Preferably, the aluminum alloy anodizing solution contains sulfuric acid, oxalic acid and tartaric acid.

[0018] More preferably, the mass concentration ratio of sulfuric acid, oxalic acid and tartaric acid is 13:1:2, wherein the mass concentration of sulfuric acid is 200-220 g / L.

[0019] Preferably, the first activation conditions include: placing the aluminum alloy antenna in an alkaline etching solution for 10-60 seconds at a temperature of 60-70°C, and washing with a first running water for 20-60 seconds; activating in a first activation solution for 5-15 seconds at a temperature of 10-30°C, and washing with a second running water for 20-60 seconds.

[0020] Preferably, the alkaline etching solution contains sodium hydroxide, sodium carbonate and sodium phosphate.

[0021] More preferably, the mass concentration ratio of the sodium hydroxide, sodium carbonate and sodium phosphate is 2:5:7, wherein the mass concentration of the sodium hydroxide is 10-15 g / L.

[0022] Further preferably, the first activation solution is a mixed solution of nitric acid and sulfuric acid in a volume ratio of 1:1.

[0023] Preferably, the first washing conditions include: washing with running water for 20-60 seconds.

[0024] Preferably, the first drying conditions include: drying the surface of the aluminum alloy antenna after the first washing and then placing it in an oven at a temperature of 50-60° C. for 30-60 minutes.

[0025] More preferably, the insulation protection condition includes: performing local insulation protection treatment with a silicone tape on the Φ1 mm through holes on the surface of the aluminum alloy antenna that need to be conductive after the first drying.

[0026] Preferably, the pretreatment conditions include: chemically etching the insulation-protected aluminum alloy antenna to remove the conductive coating, and then performing a second activation.

[0027] Preferably, the conditions for removing the conductive coating by chemical etching include: placing the aluminum alloy antenna that has been insulated and protected in a chemical etching solution for 30-60 seconds at a temperature of 60-70° C., and then placing it in running water for washing for 20-60 seconds.

[0028] More preferably, the chemical etching solution is an aqueous solution of sodium hydroxide with a mass concentration of 40-50 g / L.

[0029] Further preferably, the second activation conditions include: placing the aluminum alloy antenna after chemical etching to remove the conductive coating into the second activation solution at a temperature of 10-30° C. for 5-10 seconds, taking it out, and washing it in running water for 20-60 seconds.

[0030] More preferably, the second activation solution is an aqueous nitric acid solution with a volume concentration of 20%.

[0031] Preferably, the second washing conditions include: washing the aluminum alloy antenna prepared with the thermal control coating in running water for 20-60 seconds, and then washing in deionized water at a temperature of 50-80° C. for 5-10 seconds.

[0032] Preferably, the sealing treatment conditions include: placing the aluminum alloy antenna after the second washing in deionized water at a temperature of 90-100° C. for 5-8 minutes to perform oxide film sealing treatment.

[0033] Preferably, the second drying condition includes: drying the surface of the aluminum alloy antenna after the sealing treatment, and then putting it into an oven at a temperature of 50-60° C. for 30-60 minutes.

[0034] Preferably, the conditions for removing the insulation protection include: removing the insulating silicone tape at the Φ1mm through hole of the aluminum alloy antenna that has undergone the second drying, and checking the integrity of the conductive coating on the inner wall of the hole.

[0035] In the above technical scheme, the functional coating on the surface of the aluminum alloy antenna of the present invention is based on the application demand of domestic development of dual-band tracking and control communication satellites, and the multifunctional coating on the surface of the 5A06 aluminum alloy sub-array antenna is developed. The developed functional coating on the surface of the aluminum alloy antenna consists of a conductive coating and a thermal control coating, and has good thermal control performance and resistance to salt spray corrosion. The radiation absorption ratio (the ratio of the solar absorption ratio to the hemispherical emissivity) of the thermal control coating tends to 1, which can be used for high-precision thermal control of antennas with complex structures. At the same time, it has both the electrical performance requirements of the antenna and the anti-salt spray characteristics of storage in the sea environment, and has good adaptability to the space environment and high-precision thermal control performance, which solves the technical problems of ground protection and space thermal control of the aluminum alloy sub-array antenna.

[0036] At the same time, the preparation method of the functional coating on the surface of the aluminum alloy antenna of the present invention has simple conditions, the materials are easily available, and it can be mass-produced and promoted for use in batches.

[0037] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:

[0039] Figure 1 It is a partial schematic diagram of the aluminum alloy antenna material grade 5A06 of the present invention;

[0040] Figure 2A physical picture of the silicone tape used for insulation protection in the present invention. DETAILED DESCRIPTION

[0041] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0042] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0043] In a first aspect, the present invention provides a functional coating on the surface of an aluminum alloy antenna, wherein the functional coating on the surface of the aluminum alloy antenna comprises: a conductive coating and a thermal control coating; wherein:

[0044] The conductive coating contains chromate and its hydrate;

[0045] The thermal control coating contains aluminum oxide.

[0046] In a preferred embodiment of the present invention, the aluminum alloy antenna material grade is 5A06.

[0047] In a preferred embodiment of the present invention, the neutral salt spray resistance time of the functional coating on the surface of the aluminum alloy antenna is 192 hours, wherein the neutral salt spray resistance time is tested according to the provisions of the neutral salt spray test in the national military standard GJB150.11A.

[0048] In a second aspect, the present invention provides a method for preparing a functional coating on the surface of an aluminum alloy antenna, the preparation method comprising: first activating the aluminum alloy antenna, preparing a conductive coating, first washing, first drying, insulating protection, pretreatment, preparing a thermal control coating, second washing, sealing treatment, second drying, and removing insulating protection.

[0049] In a preferred embodiment of the present invention, in order to obtain a complete conductive coating in the through hole of the aluminum alloy antenna, the entire antenna is firstly subjected to a conductive coating preparation method, and the method for preparing the conductive coating comprises: placing the first activated aluminum alloy antenna in a conductive oxidizing solution for 2-5 minutes at a temperature of 15-35°C.

[0050] In a preferred embodiment of the present invention, in order to obtain a chromate chemical conversion film with uniform appearance and color, the conductive oxidation solution contains chromic anhydride, ammonium bifluoride, potassium ferrocyanide and Al 3+ .

[0051] In a preferred embodiment of the present invention, in order to obtain a chemical conversion film that meets both electrical conductivity and corrosion resistance, the mass concentration ratio of the chromic anhydride, ammonium bifluoride, and potassium ferrocyanide is 10:3:2, wherein the chromic anhydride concentration is controlled at 3-6 g / L, and the Al 3+ The mass concentration is 3-20g / L, wherein the Al 3+ It is produced by the reaction of aluminum alloy antenna and chromic anhydride.

[0052] In a preferred embodiment of the present invention, the method for preparing the thermal control coating comprises: placing the pretreated aluminum alloy antenna into an aluminum alloy anodizing solution for oxidation at a temperature of 16-18°C for 20-22 minutes at a voltage of 10-14V, preferably 12V.

[0053] In a preferred embodiment of the present invention, in order to obtain an aluminum alloy anodized film layer, the aluminum alloy anodized solution contains sulfuric acid, oxalic acid and tartaric acid.

[0054] In a preferred embodiment of the present invention, in order to obtain an aluminum alloy anodized film thermal control coating with specific thermal radiation performance, the mass concentration ratio of sulfuric acid, oxalic acid and tartaric acid is 13:1:2, wherein the mass concentration of sulfuric acid is 200-220 g / L.

[0055] In a preferred embodiment of the present invention, in order to remove oil stains and naturally loose oxides on the surface of the aluminum alloy antenna, the first activation conditions include: placing the aluminum alloy antenna in an alkaline etching solution for 10-60 seconds at a temperature of 60-70°C, and washing with a first running water for 20-60 seconds; activating in the first activation solution for 5-15 seconds at a temperature of 10-30°C, and washing with a second running water for 20-60 seconds.

[0056] In a preferred embodiment of the present invention, in order to achieve the purpose of degreasing the aluminum alloy, the alkaline etching solution contains sodium hydroxide, sodium carbonate and sodium phosphate.

[0057] In a preferred embodiment of the present invention, in order to remove oil stains on the antenna surface without excessively corroding the aluminum alloy substrate, the mass concentration ratio of the sodium hydroxide, sodium carbonate and sodium phosphate is 2:5:7, wherein the mass concentration of the sodium hydroxide is controlled at 10-15 g / L.

[0058] In a preferred embodiment of the present invention, in order to remove the dust and residual oxides on the surface after alkali etching and expose the fresh aluminum alloy surface, the first activation solution is a mixed solution of nitric acid and sulfuric acid in a volume ratio of 1:1.

[0059] In a preferred embodiment of the present invention, in order to clean the conductive oxidation solution dripping on the surface of the antenna, the first washing condition includes: washing with running water for 20-60 seconds.

[0060] In a preferred embodiment of the present invention, in order to remove water stains on the antenna surface and consolidate the adhesion of the conductive coating, the first drying conditions include: drying the surface of the aluminum alloy antenna after the first washing and placing it in an oven at a temperature of 50-60°C for 30-60 minutes.

[0061] In a preferred embodiment of the present invention, in order to confirm the electrical properties of the prepared conductive coating, the electrical properties of the aluminum alloy antenna after the first drying are tested: the surface lap resistance of the conductive coating is tested to be 0.05 mΩ;

[0062] In a preferred embodiment of the present invention, in order to protect the conductive coating from being corroded and damaged by various acid and alkali solutions such as subsequent etching, the insulation protection conditions include: local insulation protection treatment of the Φ1mm through holes that need to be conductive on the surface of the aluminum alloy antenna after the first drying with silicone tape.

[0063] In a preferred embodiment of the present invention, in order to remove the redundant conductive coating, the pretreatment conditions include: first chemically etching the aluminum alloy antenna after insulation protection to remove the conductive coating, and then performing a second activation.

[0064] In a preferred embodiment of the present invention, in order to remove excess conductive coating, the conditions for chemical etching to remove the conductive coating include: placing the insulated aluminum alloy antenna in a chemical etching solution for 30-60 seconds at a temperature of 60-70°C, and then placing it in running water for washing for 20-60 seconds.

[0065] In a preferred embodiment of the present invention, in order to quickly remove the excess conductive coating without excessively corroding the aluminum alloy substrate, the chemical etching solution is an aqueous solution of sodium hydroxide with a mass concentration of 40-50 g / L.

[0066] In a preferred embodiment of the present invention, in order to expose a fresh aluminum alloy substrate, the second activation conditions include: placing the aluminum alloy antenna from which the conductive coating has been removed by chemical etching into a second activation solution at a temperature of 10-30°C for 5-10 seconds, taking it out, and washing it in running water for 20-60 seconds.

[0067] In a preferred embodiment of the present invention, in order to neutralize possible residual chemical etching alkali solution, the second activation solution is a nitric acid aqueous solution with a volume concentration of 20%.

[0068] In a preferred embodiment of the present invention, in order to fully wash away the anodizing solution, the second washing conditions include: washing the aluminum alloy antenna prepared with the thermal control coating in running water for 20-60 seconds, and then washing in deionized water at a temperature of 50-80°C for 5-10 seconds.

[0069] In a preferred embodiment of the present invention, in order to improve the absorption rate and corrosion resistance of the aluminum alloy anodized film, the sealing treatment conditions include: placing the aluminum alloy antenna after the second washing in deionized water at a temperature of 90-100°C for 5-8 minutes to perform oxide film sealing treatment.

[0070] In a preferred embodiment of the present invention, in order to further solidify the conductive coating and the thermal control coating, the second drying condition includes: drying the surface of the sealed aluminum alloy antenna and placing it in an oven at a temperature of 50-60°C for 30-60 minutes.

[0071] In a preferred embodiment of the present invention, in order to remove the excess material, the conditions for removing the insulation protection include: removing the insulating silicone tape at the Φ1mm through hole of the aluminum alloy antenna after the second drying, and checking the integrity of the conductive coating on the inner wall of the hole.

[0072] The present invention will be described in detail below through examples. In the following examples, the aluminum alloy antenna material used is 5A06, and the drugs and pharmaceuticals are conventional commercial products unless otherwise specified.

[0073] Preparation Example 1

[0074] (1) The mass concentration of sodium hydroxide in the alkaline etching solution is 10 g / L, the mass concentration of sodium carbonate is 25 g / L, and the mass concentration of sodium phosphate is 35 g / L;

[0075] (2) the volume ratio of nitric acid to sulfuric acid in the first activation solution is 1:1;

[0076] (3) The mass concentration of chromic anhydride in the conductive oxidation solution is 4 g / L, the mass concentration of ammonium bifluoride is 1.2 g / L, the mass concentration of potassium ferrocyanide is 0.8 g / L, and the mass concentration of Al 3+ The mass concentration is 3g / L, among which Al 3+ It is produced by the chemical reaction between the aluminum alloy antenna and chromic acid;

[0077] (4) The chemical etching solution is a sodium hydroxide solution with a mass concentration of 40 g / L;

[0078] (5) the second activation solution is a 20% by volume nitric acid aqueous solution;

[0079] (6) The mass concentration of sulfuric acid in the aluminum alloy anodizing solution is 210 g / L, the mass concentration of oxalic acid is 16 g / L, and the mass concentration of tartaric acid is 32 g / L.

[0080] Preparation Example 2

[0081] (1) The mass concentration of sodium hydroxide in the alkaline etching solution is 15 g / L, the mass concentration of sodium carbonate is 38 g / L, and the mass concentration of sodium phosphate is 53 g / L;

[0082] (2) The mass concentration of chromic anhydride in the conductive oxidation solution is 6 g / L, the mass concentration of ammonium bifluoride is 1.8 g / L, the mass concentration of potassium ferrocyanide is 1.2 g / L, and the mass concentration of Al 3+ The mass concentration is 10g / L, among which Al 3+ It is produced by the chemical reaction between the aluminum alloy antenna and chromic acid;

[0083] (3) The chemical etching solution is a sodium hydroxide solution with a mass concentration of 46 g / L;

[0084] (4) The mass concentration of sulfuric acid in the aluminum alloy anodizing solution is 200 g / L, the mass concentration of oxalic acid is 15 g / L, and the mass concentration of tartaric acid is 31 g / L.

[0085] Preparation Example 3

[0086] (1) The mass concentration of sodium hydroxide in the alkaline etching solution is 12 g / L, the mass concentration of sodium carbonate is 30 g / L, and the mass concentration of sodium phosphate is 42 g / L;

[0087] (2) The mass concentration of chromic anhydride in the conductive oxidation solution is 3 g / L, the mass concentration of ammonium bifluoride is 0.9 g / L, the mass concentration of potassium ferrocyanide is 0.6 g / L, and the mass concentration of Al 3+ The mass concentration is 20g / L, of which Al 3+ It is produced by the chemical reaction between the aluminum alloy antenna and chromic acid;

[0088] (3) The chemical etching solution is a sodium hydroxide solution with a mass concentration of 50 g / L;

[0089] (4) The mass concentration of sulfuric acid in the aluminum alloy anodizing solution is 220 g / L, the mass concentration of oxalic acid is 17 g / L, and the mass concentration of tartaric acid is 34 g / L.

[0090] Example 1

[0091] (1) First activation: The aluminum alloy antenna was completely immersed in the alkaline etching solution prepared in Preparation 1 at a temperature of 62° C. for 48 seconds, taken out, and washed with running tap water for 30 seconds; then, the aluminum alloy antenna was immersed in the first activation solution prepared in Preparation Example 1 at a temperature of 15° C. for 10 seconds, taken out, and washed with running tap water for 40 seconds;

[0092] (2) Preparation of conductive coating: The aluminum alloy antenna after the first activation was placed in the conductive oxidation solution prepared in Preparation Example 1 for 5 minutes at a temperature of 19° C. to obtain a conductive coating;

[0093] (3) First washing: the aluminum alloy antenna after conductive oxidation was washed under running tap water for 30 seconds, and then washed in 50°C water for 10 seconds;

[0094] (4) First drying: Place the aluminum alloy antenna after the first washing on a hair dryer to dry the surface, and then place it in an oven at 55° C. for 30 minutes until the inside of the aluminum alloy antenna is completely dry.

[0095] (5) Electrical performance test: The surface lap resistance of the conductive coating is tested to be 0.05 mΩ;

[0096] (6) Insulation protection of conductive parts: Pass the silicone tape from the Φ0.8mm end to the Φ1mm through the Φ1mm through hole until it is tightened to block it, ensuring that the subsequent plating solution cannot enter the hole;

[0097] (7) Pretreatment: Chemical etching to remove the conductive coating: At a temperature of 63° C., place the aluminum alloy antenna with good insulation protection in the chemical etching solution prepared in Preparation Example 1 for 35 seconds to remove the exposed conductive coating, take it out, and wash it under running tap water for 30 seconds. At a temperature of 15° C., place it in the second activation solution prepared in Preparation 1 for activation for 7 seconds, take it out, and wash it under running tap water for 30 seconds.

[0098] (8) Preparation of thermal control coating: The aluminum alloy antenna treated by the above method was placed in an aluminum alloy anodizing solution for anodizing at a temperature of 16.8°C and an oxidation rated total voltage of 12V for 21 minutes;

[0099] (9) Second washing: Take out the aluminum alloy antenna prepared by the thermal control coating, wash it in running tap water for 30 seconds, and then wash it in deionized water at 70° C. for 5 seconds;

[0100] (10) Sealing treatment: The aluminum alloy antenna after the second washing is placed in deionized water with a pH of 5.7 and a temperature of 90° C. for 6 minutes to perform a sealing treatment on the oxide film layer;

[0101] (11) Second drying: After the aluminum alloy antenna after the sealing treatment is dried with a hair dryer, it is placed in an oven and dried at a temperature of 55° C. for 30 minutes until the inside of the antenna is completely dry, thereby obtaining an aluminum alloy antenna with a surface functional coating, which is recorded as B1.

[0102] Example 2

[0103] (1) First activation: The aluminum alloy antenna was completely immersed in the alkaline etching solution prepared in Preparation 2 at a temperature of 65° C. for 40 seconds, taken out, and washed with running tap water for 50 seconds; then, the aluminum alloy antenna was immersed in the first activation solution prepared in Preparation Example 1 at a temperature of 18° C. for 12 seconds, taken out, and washed with running tap water for 40 seconds;

[0104] (2) Preparation of conductive coating: The aluminum alloy antenna after the first activation was placed in the conductive oxidation solution prepared in Preparation Example 2 for 4 minutes at a temperature of 22° C. to obtain a conductive coating;

[0105] (3) First washing: the conductively oxidized aluminum alloy antenna was washed under running tap water for 20 seconds, and then washed in 45°C water for 8 seconds;

[0106] (4) First drying: Place the aluminum alloy antenna after the first washing on a hair dryer to dry the surface, and then place it in an oven at 55° C. for 50 minutes until the inside of the aluminum alloy antenna is completely dry.

[0107] (5) Electrical performance test: The surface lap resistance of the conductive coating was tested to be 0.06 mΩ;

[0108] (6) Insulation protection of conductive parts: Pass the silicone tape from the Φ0.8mm end to the Φ1mm through the Φ1mm through hole until it is tightened to block it, ensuring that the subsequent plating solution cannot enter the hole;

[0109] (7) Pretreatment: Chemical etching to remove the conductive coating: At a temperature of 60° C., place the aluminum alloy antenna with good insulation protection in the chemical etching solution prepared in Preparation Example 2 for 43 seconds to remove the exposed conductive coating, remove it, and wash it under running tap water for 50 seconds. At a temperature of 25° C., place it in the second activation solution prepared in Preparation 1 for activation for 10 seconds, remove it, and wash it under running tap water for 50 seconds.

[0110] (8) Preparation of thermal control coating: The aluminum alloy antenna treated by the above method is placed in an aluminum alloy anodizing solution for anodizing at a temperature of 16.2°C and an oxidation rated total voltage of 12V for 20 minutes;

[0111] (9) Second washing: Take out the aluminum alloy antenna prepared by the thermal control coating, wash it in running tap water for 60 seconds, and then wash it in deionized water at 60° C. for 10 seconds;

[0112] (10) Sealing treatment: The aluminum alloy antenna after the second washing is placed in deionized water with a pH of 5.9 and a temperature of 94° C. for 7 minutes to perform a sealing treatment on the oxide film layer;

[0113] (11) Second drying: After the aluminum alloy antenna after the sealing treatment is dried with a hair dryer, it is placed in an oven and dried at 50° C. for 40 minutes until the inside of the antenna is completely dry, thereby obtaining an aluminum alloy antenna with a surface functional coating, which is denoted as B2.

[0114] Example 3

[0115] (1) First activation: The aluminum alloy antenna was completely immersed in the alkaline etching solution prepared in Preparation 3 at a temperature of 65° C. for 55 seconds, taken out, and washed with running tap water for 60 seconds; then, the aluminum alloy antenna was immersed in the first activation solution prepared in Preparation Example 1 at a temperature of 22° C. for 15 seconds, taken out, and washed with running tap water for 60 seconds;

[0116] (2) Preparation of conductive coating: The aluminum alloy antenna after the first activation was placed in the conductive oxidation solution prepared in Preparation Example 3 for 3 minutes at a temperature of 20° C. to obtain a conductive coating;

[0117] (3) First washing: the conductively oxidized aluminum alloy antenna was washed under running tap water for 10 seconds, and then washed in 45°C water for 5 seconds;

[0118] (4) First drying: Place the aluminum alloy antenna after the first washing on a hair dryer to dry the surface, and then place it in an oven at 60° C. for 40 minutes until the inside of the aluminum alloy antenna is completely dry;

[0119] (5) Electrical performance test: The surface lap resistance of the conductive coating is tested to be 0.05 mΩ;

[0120] (6) Insulation protection of conductive parts: Pass the silicone tape from the Φ0.8mm end to the Φ1mm through the Φ1mm through hole until it is tightened to block it, ensuring that the subsequent plating solution cannot enter the hole;

[0121] (7) Pretreatment: Chemical etching to remove the conductive coating: At a temperature of 65° C., place the aluminum alloy antenna with good insulation protection in the chemical etching solution prepared in Preparation Example 3 for 50 seconds to remove the exposed conductive coating, take it out, and wash it under running tap water for 40 seconds. At a temperature of 16° C., place it in the second activation solution prepared in Preparation 1 for activation for 8 seconds, take it out, and wash it under running tap water for 50 seconds.

[0122] (8) Preparation of thermal control coating: The aluminum alloy antenna treated by the above method is placed in an aluminum alloy anodizing solution for anodizing at a temperature of 17.8°C and an oxidation rated total voltage of 12V for 20 minutes;

[0123] (9) Second washing: Take out the aluminum alloy antenna prepared by the thermal control coating, wash it in running tap water for 60 seconds, and then wash it in deionized water at 80° C. for 10 seconds;

[0124] (10) Sealing treatment: The aluminum alloy antenna after the second washing is placed in deionized water with a pH of 6.2 and a temperature of 95° C. for 5 minutes to perform a sealing treatment on the oxide film layer;

[0125] (11) Second drying: After the aluminum alloy antenna after the sealing treatment is dried with a hair dryer, it is placed in an oven and dried at 60° C. for 50 minutes until the inside of the antenna is completely dry, thereby obtaining an aluminum alloy antenna with a surface functional coating, which is denoted as B3.

[0126] Test Example 1

[0127] The surface hemispherical emissivity and solar absorption ratio of the aluminum alloy antennas B1-B3 with surface functional coatings prepared in Examples 1-3 were tested, and the results are shown in Table 1.

[0128] Example No. <![CDATA[Surface hemispherical emissivity / ε H > <![CDATA[Solar absorptance / α s > Radiation absorption ratio / % Example 1 0.70 0.69 98.57 Example 2 0.71 0.70 98.59 Example 3 0.72 0.70 97.22

[0129] Test Example 2

[0130] Salt spray resistance test: According to the provisions of the neutral salt spray test in the national military standard GJB150.11A, the salt spray corrosion resistance of the aluminum alloy antennas B1-B3 with surface functional coatings prepared in Examples 1-3 was tested. The results are shown in Table 2.

[0131] Example No. Test time / h Corrosion resistance Example 1 192 No obvious corrosion on the antenna surface Example 2 192 No obvious corrosion on the antenna surface Example 3 192 No obvious corrosion on the antenna surface

[0132] It can be seen from the above that the radiation absorption ratio of the aluminum alloy antennas B1-B3 with surface functional coatings of Examples 1-3 prepared by the preparation method of the present invention is close to 1, and has good thermal control performance, which can meet the thermal control accuracy of antennas with complex structures. At the same time, it has good salt spray resistance and corrosion resistance, is suitable for marine environments, and achieves good adaptability to space environments.

[0133] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0134] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0135] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A functional coating on the surface of an aluminum alloy antenna, It is characterized in that The functional coating on the surface of the aluminum alloy antenna includes: a conductive coating and a thermal control coating; wherein, The conductive coating contains chromate and its hydrate; The thermal control coating contains aluminum oxide.

2. The functional coating on the surface of the aluminum alloy antenna according to claim 1, It is characterized in that The material grade of the aluminum alloy antenna is 5A06; Preferably, the neutral salt spray resistance time of the functional coating on the surface of the aluminum alloy antenna is 192 hours, wherein the neutral salt spray resistance time is tested according to the provisions of the neutral salt spray test in the national military standard GJB150.11A.

3. A method for preparing a functional coating on the surface of an aluminum alloy antenna, It is characterized in that The preparation method comprises: first activating the aluminum alloy antenna, preparing a conductive coating, first washing, first drying, insulating protection, pretreatment, preparing a thermal control coating, second washing, sealing treatment, second drying, and removing insulating protection.

4. The preparation method according to claim 3, It is characterized in that The method for preparing the conductive coating comprises: placing the aluminum alloy antenna after the first activation in a conductive oxidation solution for 2-5 minutes at a temperature of 15-35° C.; Preferably, the conductive oxidizing solution contains chromic anhydride, ammonium bifluoride, potassium ferrocyanide and Al 3+ ; More preferably, the mass concentration ratio of the chromic anhydride, ammonium bifluoride and potassium ferrocyanide is 10:3:2, wherein the mass concentration of the chromic anhydride is 3-6 g / L; Further preferably, the Al 3+ The mass concentration is 3-20g / L, wherein the Al 3+ It is produced by the reaction of aluminum alloy antenna and chromic anhydride.

5. The preparation method according to claim 3 or 4, It is characterized in that The method for preparing the thermal control coating comprises: placing the pretreated aluminum alloy antenna in an aluminum alloy anodizing solution for oxidation at a temperature of 16-18° C. for 20-22 minutes at a voltage of 10-14V; Preferably, the aluminum alloy anodizing solution contains sulfuric acid, oxalic acid and tartaric acid; More preferably, the mass concentration ratio of sulfuric acid, oxalic acid and tartaric acid is 13:1:2, wherein the mass concentration of sulfuric acid is 200-220 g / L.

6. The preparation method according to any one of claims 3 to 5, It is characterized in that The first activation conditions include: placing the aluminum alloy antenna in an alkaline etching solution for 10-60 seconds at a temperature of 60-70° C., first washing with running water for 20-60 seconds, activating in a first activation solution for 5-15 seconds at a temperature of 10-30° C., and second washing with running water for 20-60 seconds; Preferably, the alkaline etching solution contains sodium hydroxide, sodium carbonate and sodium phosphate; More preferably, the mass concentration ratio of the sodium hydroxide, sodium carbonate and sodium phosphate is 2:5:7, wherein the mass concentration of the sodium hydroxide is 10-15 g / L; Further preferably, the first activation solution is a mixed solution of nitric acid and sulfuric acid in a volume ratio of 1:

1.

7. The preparation method according to any one of claims 3 to 6, It is characterized in that The first washing conditions include: washing with running water for 20-60 seconds; Preferably, the first drying conditions include: drying the surface of the aluminum alloy antenna after the first washing and then placing it in an oven at a temperature of 50-60° C. for 30-60 minutes; More preferably, the insulation protection condition includes: performing local insulation protection treatment with a silicone tape on the Φ1 mm through holes on the surface of the aluminum alloy antenna that need to be conductive after the first drying.

8. The preparation method according to any one of claims 3 to 7, It is characterized in that The pretreatment conditions include: chemically etching the aluminum alloy antenna after insulation protection to remove the conductive coating, and then performing a second activation; Preferably, the conditions for chemical etching to remove the conductive coating include: placing the aluminum alloy antenna that has been insulated and protected in a chemical etching solution for 30-60 seconds at a temperature of 60-70° C., and then placing it in running water for washing for 20-60 seconds; More preferably, the chemical etching solution is an aqueous solution of sodium hydroxide with a mass concentration of 40-50 g / L; Further preferably, the second activation conditions include: placing the aluminum alloy antenna after chemical etching to remove the conductive coating in the second activation solution at a temperature of 10-30° C. for 5-10 seconds, taking it out, and washing it in running water for 20-60 seconds; More preferably, the second activation solution is an aqueous nitric acid solution with a volume concentration of 20%.

9. The preparation method according to any one of claims 3 to 8, It is characterized in that The second washing conditions include: washing the aluminum alloy antenna prepared by the thermal control coating in running water for 20-60 seconds, and then washing in deionized water at a temperature of 50-80° C. for 5-10 seconds; Preferably, the sealing treatment conditions include: placing the aluminum alloy antenna after the second washing in deionized water at a temperature of 90-100° C. for 5-8 minutes to perform oxide film sealing treatment.

10. The preparation method according to any one of claims 3 to 9, It is characterized in that The second drying condition includes: drying the surface of the aluminum alloy antenna after the sealing treatment, and then putting it into an oven at a temperature of 50-60° C. for 30-60 minutes; Preferably, the conditions for removing the insulation protection include: removing the insulating silicone tape at the Φ1mm through hole of the aluminum alloy antenna that has undergone the second drying, and checking the integrity of the conductive coating on the inner wall of the hole.