Novel breathable high-wear-resistance organic silicon leather and preparation method thereof

By using silicone rubber and microporous structure in the leather, the problems of easy wear and poor breathability of traditional leather are solved, and high breathability and wear resistance are achieved, meeting high durability needs, and meeting environmental standards.

CN118979390APending Publication Date: 2024-11-19GUANGDONG VOCATIONAL & TECHNICAL COLLEGE +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411129292.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Traditional second-layer leather is easy to wear, deform, layer, fade, poor breathability, poor environmental protection and poor efficiency, and cannot meet the needs of high-quality life.

Method used

The new silicone leather is adopted, including a substrate layer, an adhesive layer and a surface layer. The surface layer is formed by the first liquid silicone rubber coating vulcanization, densely spread micropores, and the adhesive layer is vulcanized by the second liquid silicone rubber coating vulcanization, Improve breathability and wear resistance through microporous structure.

Benefits of technology

It achieves the improvement of the breathability and wear resistance of leather, achieves the performance of natural leather, meets high durability requirements, is suitable for multiple fields, provides a long service life and a good user experience, and meets environmental protection requirements.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses novel breathable high-wear-resistance organic silicon leather and a preparation method thereof.The novel breathable high-wear-resistance organic silicon leather comprises a base material layer, a bonding layer arranged on the base material layer and a surface layer arranged on the bonding layer, the surface layer is formed by coating and vulcanizing first liquid organic silicon rubber, and a plurality of through micropores are densely distributed in the surface layer; and the bonding layer is formed by coating and vulcanizing second liquid organic silicon rubber. The novel organic silicon leather disclosed by the invention has various high performances, air permeability and high wear resistance, overcomes the defects that the traditional synthetic leather is poor in air permeability, easy to generate peculiar smell and not suitable for being worn for a long time, can achieve the performance of natural leather in the aspect of wear resistance, meets application scenes with relatively high requirements on durability, and has wide application prospects. Therefore, the requirements of multiple fields are met, and long service life and good use experience are provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of artificial leather, and in particular to a novel breathable and highly wear-resistant organic silicon leather and a preparation method thereof. Background Art

[0002] With the continuous improvement of living standards, the pain points of traditional two-layer leather, such as easy wear, deformation, delamination, fading, poor breathability and poor environmental benefits, are becoming increasingly prominent and can no longer meet people's pursuit of high-quality and better living standards. Summary of the invention

[0003] The invention provides a novel breathable and highly wear-resistant organic silicon leather and a preparation method thereof, which can achieve the breathable and highly wear-resistant leather.

[0004] The present invention provides a novel breathable and highly wear-resistant organic silicone leather, comprising a substrate layer, an adhesive layer arranged on the substrate layer, and a surface layer arranged on the adhesive layer, wherein the surface layer is formed by coating and vulcanizing a first liquid organic silicone rubber, and a plurality of penetrating micropores are densely distributed on the surface layer, and the adhesive layer is formed by coating and vulcanizing a second liquid organic silicone rubber.

[0005] Furthermore, the first liquid silicone rubber is composed of component A and component B in a mass ratio of 100:3, component A of the first liquid silicone rubber includes RTV-2 liquid silicone rubber, component B of the first liquid silicone rubber includes RTV-2 liquid silicone rubber, hydrogen-containing silicone oil with a hydrogen content in the range of 0.36-0.50%, vinyl silicone oil, and silicone color paste pigment, and the mass ratio of RTV-2 liquid silicone rubber, hydrogen-containing silicone oil, vinyl silicone oil, and silicone color paste pigment is 100:6-30:80-100:25-30.

[0006] Furthermore, the second liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1, and component A of the second liquid silicone rubber includes LJ-12510 hyperbranched polyester acrylate special resin. Component B of the second liquid silicone rubber includes vinyl silicone oil with a viscosity of 1000-10000cs, silicone resin tackifier, and reinforcing filler, and the mass ratio of vinyl silicone oil, silicone resin tackifier, and reinforcing filler is 80-100:1-10:25-30.

[0007] Furthermore, the pore size of the micropores is 0.05-0.5 mm, and the density of the micropores is 100,000 / m 2 .

[0008] Further, the substrate layer includes a cool fabric or a warm fabric.

[0009] The present invention also provides a method for preparing the above-mentioned novel silicone leather, comprising the following steps: coating a first liquid silicone rubber on a release paper to obtain a primary coating, and drying the primary coating to obtain a surface layer. Coating a second liquid silicone rubber on the surface layer to obtain a secondary coating, and drying the secondary coating to obtain an adhesive layer. Laminating the substrate layer fabric with the adhesive layer, and subjecting them to a pressure treatment, and finally vulcanizing, and after cooling, peeling off the release paper to obtain leather, and processing micropores on the surface layer of the leather to obtain a novel silicone leather.

[0010] Furthermore, when the first liquid silicone rubber is coated on the release paper, the coating thickness is 0.15-0.25 mm and the coating speed is 6 M / min.

[0011] Furthermore, when the coating is dried once, the drying temperature is 80-150° C. and the drying time is 2-30 min.

[0012] Furthermore, when the second liquid silicone rubber is coated on the surface layer, the coating thickness is 0.35-0.45 mm and the coating speed is 6 M / min.

[0013] Furthermore, when the secondary coating is dried, the drying temperature is 80-150° C. and the drying time is 3-20 min.

[0014] Furthermore, during vulcanization, the vulcanization is performed at a temperature of 80-150° C. for 5-10 minutes.

[0015] Compared with the prior art, the present invention has the following effects:

[0016] The novel silicone leather of the present invention has multiple high performances and is breathable and highly wear-resistant, overcoming the shortcomings of traditional synthetic leather, such as poor breathability, easy generation of odor, and unsuitability for long-term wear. At the same time, it can achieve the performance of natural leather in terms of wear resistance, meeting application scenarios with high durability requirements, thereby meeting the needs of multiple fields, providing a long-lasting service life and a good user experience. DETAILED DESCRIPTION

[0017] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0018] The invention provides a novel breathable and highly wear-resistant organic silicon leather, comprising a substrate layer, an adhesive layer arranged on the substrate layer, and a surface layer arranged on the adhesive layer.

[0019] The surface layer is formed by coating and vulcanizing the first liquid silicone rubber.

[0020] The first liquid silicone rubber is composed of component A and component B in a mass ratio of 100:3, component A includes RTV-2 liquid silicone rubber, component B includes RTV-2 liquid silicone rubber, hydrogen-containing silicone oil with a hydrogen content in the range of 0.36-0.50%, vinyl silicone oil, and silicone color paste pigment, and the mass ratio of RTV-2 liquid silicone rubber, hydrogen-containing silicone oil, vinyl silicone oil, and silicone color paste pigment is 100:6-30:80-100:25-30.

[0021] The surface layer is densely covered with multiple penetrating micropores. The diameter of the micropores is 0.05-0.5mm, and the density of the micropores is 100,000 / m 2 . This micro hole does not affect the appearance.

[0022] The bonding layer is formed by coating and vulcanizing the second liquid silicone rubber.

[0023] The second liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1, wherein component A includes LJ-12510 hyperbranched polyester acrylate special resin, and component B includes vinyl silicone oil with a viscosity of 1000-10000cs, silicone resin tackifier, and reinforcing filler, and the mass ratio of vinyl silicone oil, silicone resin tackifier, and reinforcing filler is 80-100:1-10:25-30.

[0024] The substrate layer can be made of conventional products, such as polyester, spandex, pure cotton, microfiber, etc. The substrate layer can be a cool fabric or a warm fabric. Among them, the cool fabric can be made of yarn with a cool function. The yarn with a cool function (also called cool yarn) can be made by blending modified nylon and seaweed fiber. The cool fabric can also be made by a finishing agent. The warm fabric can be made of yarn with a warm function. The yarn with a warm function (also called warm yarn) can be made by blending aerogel and acrylic. The warm fabric can also be made by a finishing agent. Through the above-mentioned settings, the new silicone leather has different functions on both sides and can be used according to needs. Moreover, the cool effect of the cool fabric and the warm effect of the warm fabric can be dissipated, transmitted or enhanced through the microporous breathable channel.

[0025] In the novel breathable and highly wear-resistant organic silicone leather of the present invention, the surface layer is a layer of silica gel formed by coating, which achieves the effect of dry and wear-resistant surface touch, and at the same time improves the surface density, achieves the characteristics of wear resistance, scratch resistance, scratch resistance, etc., and comprehensively balances the feel of the surface layer glue, wear resistance, oil pollution prevention and mechanical properties. The bonding layer is a layer of silica gel formed by coating, which is used to provide a reliable interlayer bonding effect for the organic silicone resin and the microfiber base cloth, and comprehensively balances the curing speed of the bonding layer and the control of the bonding strength of the surface layer. The novel breathable and highly wear-resistant organic silicone leather of the present invention has the effect of significantly improving the softness, stretchability and wear resistance of the organic silicone leather. The microporous structure on the surface layer gives the organic silicone leather moisture permeability and air permeability, allowing air to pass through the surface of the organic silicone leather. The micropores prevent water droplets in the air from penetrating while still allowing air to pass through, which can make the leather have a certain degree of waterproof and breathable function, ensuring the dryness and comfort of the leather without affecting the surface appearance effect. In the present invention, the organic silicon used in the whole process is an environmentally friendly material itself, so the obtained leather fabric meets the environmental protection requirements, and the fabric solid content reaches 100% of organic silicon molecules, which is more conducive to environmental protection requirements and protects the health of operators.

[0026] The embodiment of the present invention also provides a method for preparing the novel silicone leather, comprising the following steps:

[0027] (1) coating a first liquid silicone rubber on a release paper to obtain a primary coating, and then drying the primary coating in a heated drying oven to obtain a surface layer.

[0028] In the above steps, the first liquid silicone rubber is composed of component A and component B in a mass ratio of 100:3, component A includes RTV-2 liquid silicone rubber, component B includes RTV-2 liquid silicone rubber, hydrogen-containing silicone oil with a hydrogen content range of 0.36-0.50%, vinyl silicone oil, and silicone color paste pigment, and the mass ratio of RTV-2 liquid silicone rubber, hydrogen-containing silicone oil, vinyl silicone oil, and silicone color paste pigment is 100:6-30:80-100:25-30. The operation time of components A and B of the first liquid silicone rubber is 4 to 8 hours, the curing time is 2 to 5 minutes, and the hardness is 45 to 65 Shore A. The viscosity of component A of the first liquid silicone rubber is 100,000 to 500,000 / mPa·S, and the viscosity of component B is 100,000 to 500,000 / mPa·S.

[0029] When the first liquid organic silicone rubber is coated on the release paper, the coating thickness of the first liquid organic silicone rubber is 0.15-0.25 mm, the coating speed is 6 M / min, and the coating temperature is room temperature.

[0030] When the coating is dried once in a heated drying oven, the drying temperature of the drying oven is 80-150°C and the drying time is 2-30 minutes.

[0031] (2) coating the second liquid silicone rubber on the surface layer to obtain a secondary coating, and then drying the secondary coating in a heated drying oven to obtain a bonding layer.

[0032] In the above steps, the second liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1, and component A includes LJ-12510 hyperbranched polyester acrylate special resin. Component B includes vinyl silicone oil with a viscosity of 1000-10000cs, silicone resin tackifier, and reinforcing filler, and the mass ratio of vinyl silicone oil, silicone resin tackifier, and reinforcing filler is 80-100:1-10:25-30. Among them, the silicone resin tackifier includes one or more of γ-aminopropyl triethoxysilane, γ-aminopropyl trimethoxysilane, vinyl triethoxysilane, vinyl trimethoxysilane, and vinyl triisopropoxysilane. The reinforcing filler includes one or more of white carbon black, nano calcium carbonate, fatty acid calcium, and nano silicon dioxide. The operation time of components A and B of the first liquid silicone rubber is 4 to 8 hours, the curing time is 2 to 5 minutes, and the hardness is 45 to 65 Shore A.

[0033] When the second liquid organic silicone rubber is coated on the surface layer, the coating thickness of the second liquid organic silicone rubber is 0.35-0.45 mm, the coating speed is 6 M / min, and the coating temperature is room temperature.

[0034] When the secondary coating is dried in a heated drying oven, the drying temperature of the drying oven is 80-150°C and the drying time is 3-20 minutes.

[0035] (3) The base material layer fabric is laminated to the adhesive layer and subjected to a hot pressing roller pressure treatment, and finally transferred to a tunnel furnace for vulcanization. After exiting the drying tunnel of the tunnel furnace and cooling down, the release paper is peeled off to obtain leather, and holes are punched on the surface layer of the leather using a mechanical perforation process such as needle punching to produce dense micropores, thereby obtaining a new type of silicone leather.

[0036] In the above steps, the base material layer fabric can be conventional products, such as polyester, spandex, pure cotton, microfiber, etc. When the base material layer fabric is attached to the adhesive layer, the adhesive layer and the surface layer are both in a semi-dry state.

[0037] During vulcanization, vulcanize at a temperature of 80-150°C for 5-10 minutes.

[0038] The aperture of the micropores is 0.05-0.5 mm, and the density of the micropores is 100,000 / m 2 . This micro hole does not affect the appearance.

[0039] Different from the two-layer structure of traditional leather, the new silicone leather of the present invention adopts a three-layer structure of a substrate layer, a high-viscosity adhesive layer and a surface layer. The present invention adds a microporous structure to the surface layer to create an oxygen permeable channel for air circulation, thereby improving the breathability of the silicone leather. This characteristic enables the leather to have significant advantages when making products that require high breathability, such as sportswear, outdoor equipment, etc. The high-viscosity adhesive layer of the present invention improves the viscosity of the viscose and highly bonds the surface layer to the substrate layer, so that the leather has excellent wear resistance and can withstand high-intensity friction and wear. The leather can also be used to manufacture some products that require high wear resistance, such as shoes, bags, tents, etc. This characteristic can extend the service life of the product and improve the durability of the product. From the perspective of environmental protection and sustainable development, the present invention reduces the demand for animal leather and reduces environmental pressure by adopting new environmentally friendly materials and green preparation processes, thereby achieving a more sustainable production and consumption model.

[0040] In summary, the new silicone leather of the present invention has multiple high performances and is breathable and highly wear-resistant, overcoming the shortcomings of traditional synthetic leather, such as poor breathability, easy odor generation and unsuitability for long-term wear. At the same time, it can achieve the performance of natural leather in terms of wear resistance, meeting application scenarios with high durability requirements, thereby meeting the needs of multiple fields and providing a long-lasting service life and a good user experience.

[0041] The following is a detailed description with reference to specific embodiments:

[0042] Example 1

[0043] (1) Coating a first liquid silicone rubber on the release paper, wherein the first liquid silicone rubber is composed of component A and component B in a mass ratio of 100:3, component A is RTV-2 liquid silicone rubber, component B includes RTV-2 liquid silicone rubber, hydrogen-containing silicone oil with a hydrogen content of 0.42%, vinyl silicone oil, and silicone color paste pigment, and the mass ratio of RTV-2 liquid silicone rubber, hydrogen-containing silicone oil, vinyl silicone oil, and silicone color paste pigment is 100:6:80:25. The coating thickness of the first liquid silicone rubber is 0.15 mm, the coating speed is 6 M / min, and the coating temperature is room temperature to obtain a primary coating. The primary coating is then dried in a heated drying oven, wherein the drying temperature of the drying oven is 90° C. and the drying time is 10 min to obtain a surface layer.

[0044] (2) Apply a second liquid silicone rubber on the surface layer, wherein the second liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1, and component A is LJ-12510 hyperbranched polyester acrylate special resin. Component B includes vinyl silicone oil with a viscosity of 1000cs, γ-aminopropyl triethoxysilane, and white carbon black, and the mass ratio of vinyl silicone oil, γ-aminopropyl triethoxysilane, and white carbon black is 80:1:25. The coating thickness of the second liquid silicone rubber is 0.35mm, the coating speed is 6M / min, and the coating temperature is room temperature to obtain a secondary coating. The secondary coating is then dried in a heated drying oven, wherein the drying temperature of the drying oven is 90°C and the drying time is 5min to obtain a bonding layer.

[0045] (3) The microfiber base fabric is laminated to the adhesive layer, and subjected to a hot pressing roller pressure treatment, and finally transferred to a tunnel furnace for vulcanization, wherein the vulcanization is performed at a temperature of 90° C. for 5 minutes, and after exiting the drying tunnel of the tunnel furnace and cooling, the release paper is peeled off to obtain leather, and a mechanical perforation process of needle punching is used to punch holes on the surface layer of the leather to form dense micropores, wherein the pore diameter of the micropores is 0.05 mm, and the punching density of the micropores is 100,000 / m 2 , and obtain a new type of silicone leather.

[0046] After testing, the breathable and highly wear-resistant new silicone leather of this embodiment can reach more than 2000 times under the ASTMD3884-09 (2017) (CS-10 grinding wheel / 1000G pressure) standard when the leather is worn. The air permeability is measured using the GBT4689.22-1996 leather air permeability tester, and the air permeability value can reach 500ml / (cm 2 *h) or above.

[0047] Example 2

[0048] (1) Coating a first liquid silicone rubber on the release paper, wherein the first liquid silicone rubber is composed of component A and component B in a mass ratio of 100:3, component A is RTV-2 liquid silicone rubber, component B includes RTV-2 liquid silicone rubber, hydrogen-containing silicone oil with a hydrogen content of 0.42%, vinyl silicone oil, and silicone color paste pigment, and the mass ratio of RTV-2 liquid silicone rubber, hydrogen-containing silicone oil, vinyl silicone oil, and silicone color paste pigment is 100:10:90:28. The coating thickness of the first liquid silicone rubber is 0.2 mm, the coating speed is 6 M / min, and the coating temperature is room temperature to obtain a primary coating. The primary coating is then dried in a heated drying oven, wherein the drying temperature of the drying oven is 120° C. and the drying time is 10 min to obtain a surface layer.

[0049] (2) Apply a second liquid silicone rubber on the surface layer, wherein the second liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1, and component A is LJ-12510 hyperbranched polyester acrylate special resin. Component B includes vinyl silicone oil with a viscosity of 1000cs, γ-aminopropyl triethoxysilane, and nano calcium carbonate, and the mass ratio of vinyl silicone oil, γ-aminopropyl trimethoxysilane, and nano calcium carbonate is 90:5:28. The coating thickness of the second liquid silicone rubber is 0.4mm, the coating speed is 6M / min, and the coating temperature is room temperature to obtain a secondary coating. The secondary coating is then dried in a heated drying oven, wherein the drying temperature of the drying oven is 120°C and the drying time is 10min to obtain a bonding layer.

[0050] (3) The microfiber base fabric is laminated to the adhesive layer, and subjected to a hot pressing roller pressure treatment, and finally transferred to a tunnel furnace for vulcanization, wherein the vulcanization is performed at a temperature of 90° C. for 5 minutes, and after exiting the drying tunnel of the tunnel furnace and cooling, the release paper is peeled off to obtain leather, and a mechanical perforation process of needle punching is used to punch holes on the surface layer of the leather to process dense micropores, wherein the aperture of the micropores is 0.3 mm, and the punching density of the micropores is 100,000 / m 2 , and obtain a new type of silicone leather.

[0051] After testing, the breathable and highly wear-resistant new silicone leather of this embodiment can reach more than 2000 times under the ASTMD3884-09 (2017) (CS-10 grinding wheel / 1000G pressure) standard when the leather is worn. The air permeability is measured using the GBT4689.22-1996 leather air permeability tester, and the air permeability value can reach 500ml / (cm 2 *h) or above.

[0052] Example 3

[0053] (1) Coating a first liquid silicone rubber on the release paper, wherein the first liquid silicone rubber is composed of component A and component B in a mass ratio of 100:3, component A is RTV-2 liquid silicone rubber, component B includes RTV-2 liquid silicone rubber, hydrogen-containing silicone oil with a hydrogen content of 0.48%, vinyl silicone oil, and silicone color paste pigment, and the mass ratio of RTV-2 liquid silicone rubber, hydrogen-containing silicone oil, vinyl silicone oil, and silicone color paste pigment is 100:20:100:30. The coating thickness of the first liquid silicone rubber is 0.22 mm, the coating speed is 6 M / min, and the coating temperature is room temperature to obtain a primary coating. The primary coating is then dried in a heated drying oven, wherein the drying temperature of the drying oven is 145° C. and the drying time is 10 min to obtain a surface layer.

[0054] (2) Apply a second liquid silicone rubber on the surface layer, wherein the second liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1, and component A is LJ-12510 hyperbranched polyester acrylate special resin. Component B includes vinyl silicone oil with a viscosity of 5000cs, vinyl triethoxysilane, and fatty acid calcium, and the mass ratio of vinyl silicone oil, vinyl triethoxysilane, and fatty acid calcium is 100:10:30. The coating thickness of the second liquid silicone rubber is 0.42mm, the coating speed is 6M / min, and the coating temperature is room temperature to obtain a secondary coating. The secondary coating is then dried in a heated drying oven, wherein the drying temperature of the drying oven is 145°C and the drying time is 15min to obtain a bonding layer.

[0055] (3) The microfiber base fabric is laminated to the adhesive layer, and subjected to a hot pressing roller pressure treatment, and finally transferred to a tunnel furnace for vulcanization, wherein the vulcanization is carried out at a temperature of 90° C. for 5 minutes, and after exiting the drying tunnel of the tunnel furnace and cooling, the release paper is peeled off to obtain leather, and a mechanical perforation process of needle punching is used to punch holes on the surface layer of the leather to process dense micropores, wherein the aperture of the micropores is 0.5 mm, and the density of the micropores is 100,000 / m 2 , and obtain a new type of silicone leather.

[0056] After testing, the breathable and highly wear-resistant new silicone leather of this embodiment can reach more than 2000 times under the ASTMD3884-0 (2017) (CS-10 grinding wheel / 1000G pressure) standard when the leather is worn. The air permeability is measured using the GBT4689.22-1996 leather air permeability tester, and the air permeability value can reach 500ml / (cm 2 *h) or above.

[0057] Example 4

[0058] (1) Coating a first liquid silicone rubber on the release paper, wherein the first liquid silicone rubber is composed of component A and component B in a mass ratio of 100:3, component A is RTV-2 liquid silicone rubber, component B includes RTV-2 liquid silicone rubber, hydrogen-containing silicone oil with a hydrogen content of 0.48%, vinyl silicone oil, and silicone color paste pigment, and the mass ratio of RTV-2 liquid silicone rubber, hydrogen-containing silicone oil, vinyl silicone oil, and silicone color paste pigment is 100:20:100:30. The coating thickness of the first liquid silicone rubber is 0.25 mm, the coating speed is 6 M / min, and the coating temperature is room temperature to obtain a primary coating. The primary coating is then dried in a heated drying oven, wherein the drying temperature of the drying oven is 145° C. and the drying time is 10 min to obtain a surface layer.

[0059] (2) Apply a second liquid silicone rubber on the surface layer, wherein the second liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1, and component A is LJ-12510 hyperbranched polyester acrylate special resin. Component B includes vinyl silicone oil with a viscosity of 5000cs, vinyl trimethoxy silane, and nano-silicon dioxide, and the mass ratio of vinyl silicone oil, vinyl trimethoxy silane, and nano-silicon dioxide is 80:10:25. The coating thickness of the second liquid silicone rubber is 0.45mm, the coating speed is 6M / min, and the coating temperature is room temperature to obtain a secondary coating. The secondary coating is then dried in a heated drying oven, wherein the drying temperature of the drying oven is 145°C and the drying time is 15min to obtain a bonding layer.

[0060] (3) The microfiber base fabric is laminated to the adhesive layer, and subjected to a hot pressing roller pressure treatment, and finally transferred to a tunnel furnace for vulcanization, wherein the vulcanization is carried out at a temperature of 90° C. for 5 minutes, and after exiting the drying tunnel of the tunnel furnace and cooling, the release paper is peeled off to obtain leather, and a mechanical perforation process of needle punching is used to punch holes on the surface layer of the leather to process dense micropores, wherein the aperture of the micropores is 0.5 mm, and the density of the micropores is 100,000 / m 2 , and obtain a new type of silicone leather.

[0061] After testing, the breathable and highly wear-resistant new silicone leather of this embodiment can reach more than 2000 times under the ASTMD3884-0 (2017) (CS-10 grinding wheel / 1000G pressure) standard when the leather is worn. The air permeability is measured using the GBT4689.22-1996 leather air permeability tester, and the air permeability value can reach 500ml / (cm 2 *h) or above.

[0062] Example 5

[0063] (1) Coating a first liquid silicone rubber on the release paper, wherein the first liquid silicone rubber is composed of component A and component B in a mass ratio of 100:3, component A is RTV-2 liquid silicone rubber, component B includes RTV-2 liquid silicone rubber, hydrogen-containing silicone oil with a hydrogen content of 0.36%, vinyl silicone oil, and silicone color paste pigment, and the mass ratio of RTV-2 liquid silicone rubber, hydrogen-containing silicone oil, vinyl silicone oil, and silicone color paste pigment is 100:10:100:25. The coating thickness of the first liquid silicone rubber is 0.2 mm, the coating speed is 6 M / min, and the coating temperature is room temperature to obtain a primary coating. The primary coating is then dried in a heated drying oven, wherein the drying temperature of the drying oven is 150° C. and the drying time is 2 min to obtain a surface layer.

[0064] (2) Apply a second liquid silicone rubber on the surface layer, wherein the second liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1, and component A is LJ-12510 hyperbranched polyester acrylate special resin. Component B includes vinyl silicone oil with a viscosity of 10000cs, vinyl trimethoxy silane, and white carbon black, and the mass ratio of vinyl silicone oil, vinyl trimethoxy silane, and white carbon black is 100:1:25. The coating thickness of the second liquid silicone rubber is 0.45mm, the coating speed is 6M / min, and the coating temperature is room temperature to obtain a secondary coating. The secondary coating is then dried in a heated drying oven, wherein the drying temperature of the drying oven is 150°C and the drying time is 3min to obtain a bonding layer.

[0065] (3) The cool fabric is laminated to the adhesive layer, and subjected to a hot pressing roller pressing treatment, and finally transferred to a tunnel furnace for vulcanization, wherein the vulcanization is performed at a temperature of 150° C. for 5 minutes, and after exiting the drying tunnel of the tunnel furnace and cooling, the release paper is peeled off to obtain leather, and a mechanical perforation process of needle punching is used to punch holes on the surface layer of the leather to form dense micropores, wherein the pore diameter of the micropores is 0.1 mm, and the punching density of the micropores is 100,000 / m 2 , and obtain a new type of silicone leather.

[0066] After testing, the breathable and highly wear-resistant new silicone leather of this embodiment can reach more than 2000 times under the ASTMD3884-0 (2017) (CS-10 grinding wheel / 1000G pressure) standard when the leather is worn. The air permeability is measured using the GBT4689.22-1996 leather air permeability tester, and the air permeability value can reach 500ml / (cm 2 *h) or above.

[0067] Example 6

[0068] (1) Coating a first liquid silicone rubber on the release paper, wherein the first liquid silicone rubber is composed of component A and component B in a mass ratio of 100:3, component A is RTV-2 liquid silicone rubber, component B includes RTV-2 liquid silicone rubber, hydrogen-containing silicone oil with a hydrogen content of 0.50%, vinyl silicone oil, and silicone color paste pigment, and the mass ratio of RTV-2 liquid silicone rubber, hydrogen-containing silicone oil, vinyl silicone oil, and silicone color paste pigment is 100:30:100:30. The coating thickness of the first liquid silicone rubber is 0.25 mm, the coating speed is 6 M / min, and the coating temperature is room temperature to obtain a primary coating. The primary coating is then dried in a heated drying oven, wherein the drying temperature of the drying oven is 80°C and the drying time is 30 minutes to obtain a surface layer.

[0069] (2) Apply a second liquid silicone rubber on the surface layer, wherein the second liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1, and component A is LJ-12510 hyperbranched polyester acrylate special resin. Component B includes vinyl silicone oil with a viscosity of 2000cs, vinyl triethoxysilane, and fatty acid calcium, and the mass ratio of vinyl silicone oil, vinyl triethoxysilane, and fatty acid calcium is 90:5:30. The coating thickness of the second liquid silicone rubber is 0.35mm, the coating speed is 6M / min, and the coating temperature is room temperature to obtain a secondary coating. The secondary coating is then dried in a heated drying oven, wherein the drying temperature of the drying oven is 80°C and the drying time is 20min to obtain a bonding layer.

[0070] (3) The warm fabric is laminated to the adhesive layer and subjected to a hot pressing roller pressure treatment. After cooling, the release paper is peeled off to obtain leather. A mechanical perforation process of needle punching is used to punch holes on the surface layer of the leather to produce dense micropores. The micropores have a pore diameter of 0.4 mm and a needle punching density of 100,000 / m 2 , and obtain a new type of silicone leather.

[0071] After testing, the breathable and highly wear-resistant new silicone leather of this embodiment can reach more than 2000 times under the ASTMD3884-0 (2017) (CS-10 grinding wheel / 1000G pressure) standard when the leather is worn. The air permeability is measured using the GBT4689.22-1996 leather air permeability tester, and the air permeability value can reach 500ml / (cm 2 *h) or above.

[0072] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A new type of breathable and highly wear-resistant silicone leather, characterized in that: It comprises a base material layer, an adhesive layer arranged on the base material layer and a surface layer arranged on the adhesive layer, wherein the surface layer is formed by coating and vulcanizing a first liquid organic silicone rubber, the surface layer is densely covered with a plurality of penetrating micropores, and the adhesive layer is formed by coating and vulcanizing a second liquid organic silicone rubber.

2. The novel silicone leather according to claim 1, characterized in that: The first liquid silicone rubber is composed of component A and component B in a mass ratio of 100:3, component A of the first liquid silicone rubber includes RTV-2 liquid silicone rubber, component B of the first liquid silicone rubber includes RTV-2 liquid silicone rubber, hydrogen-containing silicone oil with a hydrogen content in the range of 0.36-0.50%, vinyl silicone oil, and silicone color paste pigment, and the mass ratio of the RTV-2 liquid silicone rubber, the hydrogen-containing silicone oil, the vinyl silicone oil, and the silicone color paste pigment is 100:6-30:80-100:25-30.

3. The novel silicone leather according to claim 1, characterized in that: The second liquid silicone rubber consists of component A and component B in a mass ratio of 1:1, wherein component A of the second liquid silicone rubber includes LJ-12510 hyperbranched polyester acrylate special resin; component B of the second liquid silicone rubber includes vinyl silicone oil with a viscosity of 1000-10000cs, a silicone resin tackifier, and a reinforcing filler, and the mass ratio of the vinyl silicone oil, the silicone resin tackifier, and the reinforcing filler is 80-100:1-10:25-30.

4. The novel silicone leather according to claim 1, characterized in that: The aperture of the micropores is 0.05-0.5 mm, and the punching density of the micropores is 100,000 / m 2 ; The substrate layer comprises a cool fabric or a warm fabric.

5. A method for preparing the novel silicone leather according to any one of claims 1 to 4, characterized in that: The following steps are involved: Applying a first liquid silicone rubber on the release paper to obtain a primary coating, and drying the primary coating to obtain a surface layer; Applying a second liquid silicone rubber on the surface layer to obtain a secondary coating, and then drying the secondary coating to obtain a bonding layer; The base material layer fabric is laminated to the adhesive layer, and subjected to a pressing treatment, and finally vulcanized. After cooling, the release paper is peeled off to obtain leather, and micropores are processed on the surface layer of the leather to obtain a novel silicone leather.

6. The preparation method according to claim 5, characterized in that: When the first liquid silicone rubber is coated on the release paper, the coating thickness is 0.15-0.25 mm and the coating speed is 6 M / min.

7. The preparation method according to claim 5, characterized in that: When drying the primary coating, the drying temperature is 80-150° C. and the drying time is 2-30 min.

8. The preparation method according to claim 5, characterized in that: When the second liquid silicone rubber is coated on the surface layer, the coating thickness is 0.35-0.45 mm and the coating speed is 6 M / min.

9. The preparation method according to claim 5, characterized in that: When the secondary coating is dried, the drying temperature is 80-150° C. and the drying time is 3-20 min.

10. The preparation method according to claim 5, characterized in that: During vulcanization, vulcanize at a temperature of 80-150°C for 5-10 minutes.