Mass spectrum method for rapidly detecting antioxidant in environment and food
By using the magnetic nanocomposite Fe3O4@BN as the matrix and enrichment medium, the problems of numerous interference peaks and low sensitivity in the detection of complex samples in traditional MALDI mass spectrometry analysis are solved, enabling rapid and effective detection of antioxidants in the environment and food, with high sensitivity and good signal reproducibility.
Patent Information
- Application Number
- CN202411052108.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
Traditional MALDI mass spectrometry analysis suffers from numerous interference peaks, high background noise, and low sensitivity when detecting complex samples, making it difficult to quickly and effectively detect antioxidants in the environment and food.
Using the magnetic nanocomposite Fe3O4@BN as the matrix and enrichment medium, rapid adsorption and separation are achieved by utilizing its magnetic properties. Five antioxidants are identified by mass spectrometry signals at the low molecular weight end, exhibiting high sensitivity and salt tolerance.
It enables rapid detection of antioxidants in the environment and food, with high sensitivity and reliable MALDI mass spectrometry signal reproducibility. It can identify a variety of antioxidants and exhibits good signal response and salt tolerance in complex samples.
Smart Images

Figure CN118980736A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of analysis and detection, and more particularly to a mass spectrometry method for rapid detection of antioxidants in the environment and food. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Antioxidants are industrial chemicals produced in large quantities and have been widely used as additives in plastics, rubber, wires, cables and other polymer materials to prevent oxidative degradation of the products. Due to their large-scale use worldwide, the accumulation of antioxidants in the environment and excessive intake by humans may pose health risks. Therefore, it is of great significance to establish a rapid analysis method for antioxidants using MALDI mass spectrometry.
[0004] Traditional MALDI mass spectrometry relies on organic matrices as a medium for energy absorption and transmission. However, these organic matrices often have problems such as many interference peaks, large background noise, and low sensitivity when detecting complex samples. Therefore, how to quickly and effectively detect antioxidants in the environment and food is an urgent problem that technicians in this field need to solve. Summary of the invention
[0005] In order to overcome the shortcomings of the prior art, the present invention provides a MALDI mass spectrometry method for rapid detection of antioxidants in the environment and food. For the first time, the magnetic nanocomposite material Fe3O4@BN is used as a matrix and enrichment medium to detect antioxidants in the environment and food. The magnetic properties of the Fe3O4@BN itself achieve rapid adsorption of the detection target and rapid separation under the action of an external magnetic field. At the same time, there is a clean mass spectrometry signal background at the low molecular weight end, and 5 antioxidants can be identified. It also has high sensitivity, strong salt resistance and reliable MALDI mass spectrometry signal reproducibility.
[0006] The technical solution adopted by the present invention is as follows:
[0007] In a first aspect, the present invention provides a mass spectrometry method for rapid detection of antioxidants in the environment and food.
[0008] The method comprises the following steps:
[0009] a) Preparation of a composite material of boron nitride nanosheets and magnetic Fe3O4 nanoparticles (Fe3O4@BN);
[0010] b) Fe3O4@BN composite material was used as MALDI matrix and enrichment medium;
[0011] c) Mixing the sample to be tested with the Fe3O4@BN composite material and performing MALDI mass spectrometry analysis.
[0012] Specifically, the preparation method of the Fe3O4@BN composite material comprises the following steps:
[0013] a) preparing boron nitride nanosheets by high temperature calcination method;
[0014] Weigh urea and boric acid, mix them with methanol aqueous solution, shake them evenly, and then heat and evaporate until a white crystalline powder of the precursor is formed, then calcine the powder to obtain white boron nitride nanosheets, and then wash, dry and grind to obtain two-dimensional porous boron nitride nanosheets;
[0015] b) mixing the boron nitride nanosheets with an iron salt solution;
[0016] Boron nitride nanosheets were dispersed in deionized water and sonicated, then FeCl3·6H2O and FeCl2·4H2O were added and sonicated continuously to ensure complete mixing;
[0017] c) adding an alkaline solution to the mixed solution for reaction;
[0018] NH4OH solution was added dropwise until the mixture became alkaline, and then magnetic stirring was performed;
[0019] d) heating, washing and drying the reaction product to obtain a Fe3O4@BN composite material.
[0020] Specifically, a) urea and boric acid are mixed with 18-22 ml of methanol aqueous solution, shaken for 1-1.2 hours, and then heated and evaporated at 50-55° C. until a white crystalline powder of the precursor is formed, and then the powder is transferred to a quartz boat and placed in a tube furnace for calcination, the temperature of the tube furnace is heated from room temperature to 1000-1100° C. at a rate of 4-5° C. / min, and then maintained at 1000-1100° C. for 2-2.5 hours under N2 protection, after the reaction is completed, the tube furnace is cooled from 1000-1100° C. to 200-300° C. at a rate of 5-10° C. / min, and finally the furnace temperature is naturally cooled to room temperature, the obtained white boron nitride nanosheet product is washed with methanol for multiple times, and dried in an oven at 50-60° C., and the obtained two-dimensional porous boron nitride nanosheet is dried and stored at room temperature after grinding;
[0021] The molar ratio of urea to boric acid is 0.1-0.2 mol: 0.04 mol-0.06 mol; the volume ratio of methanol to deionized water in the methanol aqueous solution is 1:1.2;
[0022] Preferably, 0.15 mol urea and 0.05 mol boric acid are mixed with 20 ml of a methanol aqueous solution with a volume ratio of 1:1, shaken for 1 hour, and then heated and evaporated at 50°C until a white crystalline powder of the precursor is formed. Then, the powder is transferred to a quartz boat and placed in a tube furnace for calcination. The temperature of the tube furnace is heated from room temperature to 1000°C at a rate of 5°C / min, and then maintained at 1000°C for 2 hours under N2 protection. After the reaction is completed, the tube furnace is cooled from 1000°C to 200°C at a rate of 5°C / min, and finally the furnace temperature is naturally cooled to room temperature. The obtained white boron nitride nanosheet product is washed three times with methanol and dried in an oven at 50°C. After grinding, the obtained two-dimensional porous boron nitride nanosheet is dried and stored at room temperature;
[0023] b) Boron nitride nanosheets were dispersed in deionized water, ultrasonically treated for 30-40 min, and then FeCl3·6H2O and FeCl2·4H2O were added, and the ultrasonic treatment was continued for 30-50 min;
[0024] Preferably, the mass ratio of the boron nitride nanosheets to the volume of deionized water is (50-250) mg:100 mL; the mass ratio of the boron nitride nanosheets to FeCl3·6H2O and FeCl2·4H2O is 1:(8-10):(2.3-3.3);
[0025] Preferably, 150 mg of boron nitride nanosheets are dispersed in 100 mL of deionized water, ultrasonically treated for 30 min, and then 1.35 g of FeCl3·6H2O and 0.5 g of FeCl2…4H2O are added, and the ultrasonic treatment is continued for 30 min;
[0026] c) adding 3-10 mL of 13-15 M NH4OH solution dropwise until the mixture becomes alkaline, and then stirring magnetically for 3.5-5 h;
[0027] Preferably, 3 mL of 14 M NH4OH solution is added dropwise until the mixture is alkaline to pH 8.0, and then magnetic stirring is performed for 3.5 h;
[0028] d) placing the reaction product obtained in step c) into a hydrothermal reactor, reacting for 9-12 hours under the protection of N2 atmosphere and at a temperature of 160-180°C, then gradually cooling to room temperature, washing with deionized water and anhydrous ethanol, placing in an oven, and drying at 70-100°C to obtain a Fe3O4@BN composite material;
[0029] Preferably, the reaction product obtained in step c) is placed in a hydrothermal reactor, reacted for 10 hours under the protection of N2 atmosphere and at a temperature of 175°C, then gradually cooled to room temperature, washed with deionized water and anhydrous ethanol, placed in an oven, and dried at 70°C to obtain a Fe3O4@BN composite material.
[0030] Specifically, the sample is an environmental water sample, a biological sample or a food sample;
[0031] Preferably, the environmental water sample includes industrial wastewater or aquaculture wastewater, the biological sample includes serum or plant tissue, and the food sample is a vegetable oil sample.
[0032] Specifically, the rapifleX with a laser emission wavelength of 355nm TM The MALDI-TOF / TOF mass spectrometer is used to analyze samples in positive (negative) ion mode, with a voltage between -20-20 kV, and a laser frequency of 500 Hz. Mass spectral data is acquired by capturing 500 lasers, with a scanning range of m / z 150 Da to 1000 Da and a spatial resolution of 100 μm.
[0033] In a second aspect, the present invention provides a Fe3O4@BN composite material, comprising boron nitride nanosheets (h-BNNs) and magnetic Fe3O4 nanoparticles, wherein the Fe3O4 nanoparticles are uniformly distributed on the surface of the boron nitride nanosheets.
[0034] In a third aspect of the present invention, a method for preparing a Fe3O4@BN composite material is provided, comprising the following steps:
[0035] a) preparing boron nitride nanosheets by high temperature calcination method;
[0036] Weigh urea and boric acid, mix them with methanol aqueous solution, shake them evenly, and then heat and evaporate until a white crystalline powder of the precursor is formed, then calcine the powder to obtain white boron nitride nanosheets, and then wash, dry and grind to obtain two-dimensional porous boron nitride nanosheets;
[0037] b) mixing the boron nitride nanosheets with an iron salt solution;
[0038] Boron nitride nanosheets were dispersed in deionized water and sonicated, then FeCl3·6H2O and FeCl2·4H2O were added and sonicated continuously to ensure complete mixing;
[0039] c) adding an alkaline solution to the mixed solution for reaction;
[0040] NH4OH solution was added dropwise until the mixture became alkaline, and then magnetic stirring was performed;
[0041] d) heating, washing and drying the reaction product to obtain a Fe3O4@BN composite material.
[0042] Specifically, a) urea and boric acid are mixed with 18-22 ml of methanol aqueous solution, shaken for 1-1.2 hours, and then heated and evaporated at 50-55° C. until a white crystalline powder of the precursor is formed, and then the powder is transferred to a quartz boat and placed in a tube furnace for calcination, the temperature of the tube furnace is heated from room temperature to 1000-1100° C. at a rate of 4-5° C. / min, and then maintained at 1000-1100° C. for 2-2.5 hours under N2 protection, after the reaction is completed, the tube furnace is cooled from 1000-1100° C. to 200-300° C. at a rate of 5-10° C. / min, and finally the furnace temperature is naturally cooled to room temperature, the obtained white boron nitride nanosheet product is washed with methanol for multiple times, and dried in an oven at 50-60° C., and the obtained two-dimensional porous boron nitride nanosheet is dried and stored at room temperature after grinding;
[0043] The molar ratio of urea to boric acid is 0.1-0.2 mol: 0.04 mol-0.06 mol; the volume ratio of methanol to deionized water in the methanol aqueous solution is 1:1.2;
[0044] Preferably, 0.15 mol urea and 0.05 mol boric acid are mixed with 20 ml of a methanol aqueous solution with a volume ratio of 1:1, shaken for 1 hour, and then heated and evaporated at 50°C until a white crystalline powder of the precursor is formed. Then, the powder is transferred to a quartz boat and placed in a tube furnace for calcination. The temperature of the tube furnace is heated from room temperature to 1000°C at a rate of 5°C / min, and then maintained at 1000°C for 2 hours under N2 protection. After the reaction is completed, the tube furnace is cooled from 1000°C to 200°C at a rate of 5°C / min, and finally the furnace temperature is naturally cooled to room temperature. The obtained white boron nitride nanosheet product is washed three times with methanol and dried in an oven at 50°C. After grinding, the obtained two-dimensional porous boron nitride nanosheet is dried and stored at room temperature;
[0045] b) Boron nitride nanosheets were dispersed in deionized water, ultrasonically treated for 30-40 min, and then FeCl3·6H2O and FeCl2·4H2O were added, and the ultrasonic treatment was continued for 30-50 min;
[0046] Preferably, the mass ratio of the boron nitride nanosheets to the volume of deionized water is (50-250) mg:100 mL; the mass ratio of the boron nitride nanosheets to FeCl3·6H2O and FeCl2·4H2O is 1:(8-10):(2.3-3.3);
[0047] Preferably, 150 mg of boron nitride nanosheets are dispersed in 100 mL of deionized water, ultrasonically treated for 30 min, and then 1.35 g of FeCl3·6H2O and 0.5 g of FeCl2·4H2O are added, and ultrasonic treatment is continued for 30 min;
[0048] c) adding 3-10 mL of 13-15 M NH4OH solution dropwise until the mixture becomes alkaline, and then stirring magnetically for 3.5-5 h;
[0049] Preferably, 3 mL of 14 M NH4OH solution is added dropwise until the mixture is alkaline to pH 8.0, and then magnetic stirring is performed for 3.5 h;
[0050] d) placing the reaction product obtained in step c) into a hydrothermal reactor, reacting for 9-12 hours under the protection of N2 atmosphere and at a temperature of 160-180°C, then gradually cooling to room temperature, washing with deionized water and anhydrous ethanol, placing in an oven, and drying at 70-100°C to obtain a Fe3O4@BN composite material;
[0051] Preferably, the reaction product obtained in step c) is placed in a hydrothermal reactor, reacted for 10 hours under the protection of N2 atmosphere and at a temperature of 175°C, then gradually cooled to room temperature, washed with deionized water and anhydrous ethanol, placed in an oven, and dried at 70°C to obtain a Fe3O4@BN composite material.
[0052] The third aspect of the present invention provides applications of Fe3O4@BN composite materials in the following fields:
[0053] a) Detection of antioxidants in environmental samples;
[0054] b) Detection of antioxidants in biological samples;
[0055] c) Detection of antioxidants in food samples;
[0056] d) mass spectrometry imaging analysis;
[0057] e) Quantitative analysis of antioxidants.
[0058] Preferably, the environmental water sample includes industrial wastewater or aquaculture wastewater, the biological sample includes but is not limited to serum, plant tissue and other biological fluids; and the food sample is a vegetable oil sample.
[0059] Specifically, the Fe3O4@BN composite material is used for mass spectrometry imaging quantitative analysis, and is suitable for analyzing the spatial distribution and content level of antioxidants in plant samples.
[0060] One or more embodiments of the present invention have at least the following beneficial effects:
[0061] (1) The present invention is the first to use Fe3O4@BN composite materials as both MALDI matrix and enrichment medium to detect synthetic antioxidants. Fe3O4@BN, which has rapid adsorption and rapid separation effects as well as matrix function, improves the mass spectrometry detection capability. The magnetic properties of Fe3O4@BN itself achieve rapid adsorption of the detection target and rapid separation under the action of an external magnetic field. Compared with commercial traditional matrices, it has a clean mass spectrometry signal background at the low molecular weight end, recognizes 5 antioxidants, and has higher sensitivity. Compared with inorganic monomer matrices, it presents a higher mass spectrometry signal response. In addition, the Fe3O4@BN composite inorganic nanomatrix has good salt resistance, high point-to-point and sample-to-sample reproducibility, and brings gains for enhancing signal response.
[0062] (2) Fe3O4@BN adsorbent and composite inorganic nanomatrix showed good MALDI mass spectrometry signal response and were able to trace antioxidant analysis. For seafood aquaculture wastewater, the detection limit of the BHT method was 0.25 μg / L, the linear range was 1-1000 μg / L, the precision RSD was 3.65%-8.73%, and the sample recovery rate was 87.2%-102.7%. For human serum samples, the detection limit of the Irganox565 method was 1 μg / L, the linear range was 5-750 μg / L, the precision RSD was 3.75%-6.49%, and the recovery rate was 81.34%-109.4%. For vegetable oil samples, the detection limit of the BHT method was 1 ng / g, the linear range was 5-500 ng / g, the precision RSD was 5.19%-8.23%, and the recovery rate was 85.6%-111.2%. In addition, Fe3O4@BN was successfully used as a matrix for the quantitative analysis of AO168 concentration levels in the range of 10 to 1000 μg / L in cactus by mass spectrometry imaging, with a detection limit of 2.5 μg / L. These results indicate that Fe3O4@BN composite inorganic nanomatrix exhibits satisfactory performance in MALDI mass spectrometry analysis of antioxidants.
[0063] (3) The synergistic effect of Fe3O4 and h-BNNs enhances the MALDI mass spectrometry performance of the composite matrix. The strong absorption capacity of Fe3O4@BN in the ultraviolet region enables more efficient energy transfer from the material to the analyte. The synergistic effect of h-BNNs and Fe3O4 in the composite structure improves the photothermal conversion efficiency and promotes the ionization of the target. There are two types of hydrogen bonding forces (-NH…OH- and -OH…OH-) between Fe3O4@BN and analytes such as synthetic antioxidants, which enhance the affinity and selectivity of the matrix for the target and help achieve desorption ionization. BRIEF DESCRIPTION OF THE DRAWINGS
[0064] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0065] Figure 1 (a) SEM image of h-BNNs, (b) TEM image of h-BNNs, (c) SEM image of Fe3O4@BN, (d) TEM image of Fe3O4@BN;
[0066] Figure 2 (a) hysteresis curve of Fe3O4@BN, (b) XRD spectra of h-BNNs and Fe3O4@BN, (c) XPS spectra of h-BNNs and Fe3O4@BN, (d) type IV isotherms of h-BNNs and Fe3O4@BN;
[0067] Figure 3 (a) IR spectrum of h-BNNs, (b) IR spectrum of Fe3O4@BN, (c) UV-visible spectrum of h-BNNsandFe3O4@BN;
[0068] Figure 4 Mass spectra of (a) CHCA, (b) DHB, (c) Dithranol, (d) Fe3O4, (e) h-BNNs, and (f) Fe3O4@BN matrices used for MALDI mass spectrometry detection of synthetic antioxidants, with the concentration of each compound being 10 μg / L;
[0069] Figure 5 The salt tolerance of synthetic antioxidants (1-PZ, 2-BHT, 3-Irganox2246, 4-Irganox565, AO168) was investigated for Fe3O4@BN composite matrix, with each target concentration of 10 μg / L;
[0070] Figure 6 Mass spectral intensity values of Fe3O4@BN composite matrix for MALDI mass spectrometry detection of synthetic antioxidants: (a) point-to-point mass spectrometry signal intensity, (b) sample-to-sample mass spectrometry signal intensity, concentration of each target: 10 μg / L;
[0071] Figure 7 (a) BHT working curve in environmental water sample, (b) blank sample mass spectrum, (c) blank sample spiked mass spectrum, (d) Fe3O4@BN matrix enriched spiked sample mass spectrum;
[0072] Figure 8(a) Irganox565 working curve in human serum sample, (b) mass spectrum of blank human serum sample, (c) mass spectrum of sample spiked, (d) mass spectrum of Fe3O4@BN enriched sample spiked;
[0073] Fig. 9 Fe3O4@BN was used as a matrix for MALDI mass spectrometry imaging to analyze AO168: (a) imaging distribution diagram of different concentration points, (b) working curve of AO168 in cactus samples;
[0074] Fig.10 (a) The organizational structure of cactus, (bd) Fe3O4@BN was used as a matrix for MALDI mass spectrometry imaging to quantitatively distribute AO168 in different cactus samples;
[0075] Fig.11 Working curve of BHT in edible oil samples;
[0076] Fig.12 The diagram shows the interaction and ionization mechanism between Fe3O4@BN composite nanomatrix and target;
[0077] Fig.13 MALDI mass spectrum of BP analyzed in positive ion mode using Fe3O4@BN composite matrix.
[0078] Fig.14 Schematic diagram of the preparation of Fe3O4@BN and its enhanced MALDI mass spectrometry and imaging analysis of antioxidant compounds. DETAILED DESCRIPTION
[0079] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0080] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0081] As the background technology introduces, it is of great significance to establish a MALDI mass spectrometry rapid analysis method for synthetic antioxidants. Traditional MALDI mass spectrometry analysis relies on organic matrices as a medium for energy absorption and transmission. However, these organic matrices often have problems such as many interference peaks, large background noise, and low sensitivity when detecting complex samples. Therefore, how to quickly and effectively detect antioxidants in the environment and food is a problem that those skilled in the art need to solve urgently.
[0082] The experimental drugs and materials required for a MALDI mass spectrometry method for rapid detection of antioxidants in the environment and food are shown in Table 1 below:
[0083] Table 1 List of experimental drugs
[0084]
[0085] The experimental equipment required for a MALDI mass spectrometry method for rapid detection of antioxidants in the environment and food is shown in Table 2 below:
[0086] Table 2 List of experimental equipment
[0087]
[0088]
[0089] Example 1 Preparation of magnetic nanocomposite Fe3O4@BN
[0090] (1) Preparation of Boron Nitride Nanosheets by High-temperature Calcination
[0091] 0.15 mol urea and 0.05 mol boric acid are mixed with 20 ml methanol aqueous solution with a volume ratio of 1:1, shaken for 1 hour, and then heated at 50°C for evaporation until a white crystalline powder of the precursor is formed. Then, the powder is transferred to a quartz boat and placed in a tube furnace for calcination. The temperature of the tube furnace is heated from room temperature to 1000°C at a rate of 5°C / min, and then maintained at 1000°C for 2 hours under N2 protection. After the reaction is completed, the tube furnace is cooled from 1000°C to 200°C at a rate of 5°C / min, and finally the furnace temperature is naturally cooled to room temperature. The obtained white boron nitride nanosheet product is washed three times with methanol and dried in an oven at 50°C. After grinding, the obtained two-dimensional porous boron nitride nanosheet is dried and stored at room temperature;
[0092] (2) 150 mg of BN nanosheets were dispersed in 100 mL of deionized water and ultrasonicated for 30 min. Then, 1.35 g of FeCl3·6H2O and 0.5 g of FeCl2·4H2O were added and ultrasonicated for another 30 min to ensure complete mixing.
[0093] (3) 3 mL of 14 M NH4OH solution was added dropwise until the mixture was alkaline to pH 8.0, and then magnetically stirred for 3.5 h. The mixture was placed in a hydrothermal reactor and reacted for 10 h at 175 °C under the protection of N2 atmosphere. The mixture was then gradually cooled to room temperature, washed with deionized water and anhydrous ethanol, placed in an oven, and dried at 70 °C to obtain a Fe3O4@BN composite material.
[0094] Example 2
[0095] (1) Preparation of Boron Nitride Nanosheets by High-temperature Calcination
[0096] 0.15 mol urea and 0.05 mol boric acid are mixed with 20 ml methanol aqueous solution with a volume ratio of 1:1, shaken for 1 hour, and then heated at 50°C for evaporation until a white crystalline powder of the precursor is formed. Then, the powder is transferred to a quartz boat and placed in a tube furnace for calcination. The temperature of the tube furnace is heated from room temperature to 1000°C at a rate of 5°C / min, and then maintained at 1000°C for 2 hours under N2 protection. After the reaction is completed, the tube furnace is cooled from 1000°C to 200°C at a rate of 5°C / min, and finally the furnace temperature is naturally cooled to room temperature. The obtained white boron nitride nanosheet product is washed three times with methanol and dried in an oven at 50°C. After grinding, the obtained two-dimensional porous boron nitride nanosheet is dried and stored at room temperature;
[0097] (2) 100 mg of BN nanosheets were dispersed in 100 mL of deionized water and ultrasonicated for 30 min. Then, 0.9 g of FeCl3·6H2O and 0.33 g of FeCl2·4H2O were added and ultrasonicated for another 30 min to ensure complete mixing.
[0098] (3) 3 mL of 14 M NH4OH solution was added dropwise until the mixture was alkaline to pH 8.0, and then magnetically stirred for 3.5 h. The mixture was placed in a hydrothermal reactor and reacted for 10 h at 175 °C under the protection of N2 atmosphere. The mixture was then gradually cooled to room temperature, washed with deionized water and anhydrous ethanol, placed in an oven, and dried at 70 °C to obtain a Fe3O4@BN composite material.
[0099] Example 3
[0100] 0.15 mol urea and 0.05 mol boric acid are mixed with 20 ml methanol aqueous solution with a volume ratio of 1:1, shaken for 1 hour, and then heated at 50°C for evaporation until a white crystalline powder of the precursor is formed. Then, the powder is transferred to a quartz boat and placed in a tube furnace for calcination. The temperature of the tube furnace is heated from room temperature to 1000°C at a rate of 5°C / min, and then maintained at 1000°C for 2 hours under N2 protection. After the reaction is completed, the tube furnace is cooled from 1000°C to 200°C at a rate of 5°C / min, and finally the furnace temperature is naturally cooled to room temperature. The obtained white boron nitride nanosheet product is washed three times with methanol and dried in an oven at 50°C. After grinding, the obtained two-dimensional porous boron nitride nanosheet is dried and stored at room temperature;
[0101] (2) 200 mg of BN nanosheets were dispersed in 100 mL of deionized water and ultrasonicated for 30 min. Then, 1.8 g of FeCl3·6H2O and 0.66 g of FeCl2·4H2O were added and ultrasonicated for another 30 min to ensure complete mixing.
[0102] (3) 3 mL of 14 M NH4OH solution was added dropwise until the mixture was alkaline to pH 8.0, and then magnetically stirred for 3.5 h. The mixture was placed in a hydrothermal reactor and reacted for 10 h at 175 °C under the protection of N2 atmosphere. The mixture was then gradually cooled to room temperature, washed with deionized water and anhydrous ethanol, placed in an oven, and dried at 70 °C to obtain a Fe3O4@BN composite material.
[0103] Experimental example
[0104] Solution preparation
[0105] Preparation of standard solution: Prepare a 10 μg / mL stock standard solution of antioxidants in acetonitrile as solvent, and prepare a series of working dilutions for use. Before preparing the standard solution of AO168, add 1% silver trifluoroacetate to the acetonitrile solvent. The standard solution of antioxidants is used to compare Fe3O4@BN as a matrix material with other materials and to investigate the salt resistance and reproducibility of Fe3O4@BN as a matrix. Prepare a 100 mg / L 1-(phenylmethyl)pyridinium chloride solution in methanol as solvent. The 1-(phenylmethyl)pyridinium chloride solution is used for mechanism studies. All prepared reagents were stored in a refrigerator at 4°C before the experiment.
[0106] Matrix preparation:
[0107] Using α-cyano-4-hydroxycinnamic acid (CHCA) as solute and acetonitrile: water (containing 0.1% trifluoroacetic acid) = 3:7 as solvent, 0.5-10 mg / mL α-cyano-4-hydroxycinnamic acid (CHCA) matrix was prepared;
[0108] Using 2,5-dihydroxybenzoic acid (DHB) as a solute and acetonitrile: water (containing 0.1% trifluoroacetic acid) = 3:7 as a solvent, a 0.5-10 mg / mL 2,5-dihydroxybenzoic acid (DHB) matrix was prepared;
[0109] Using dithranol as solute and acetonitrile:tetrahydrofuran (containing 0.1% trifluoroacetic acid) = 3:7 as solvent, a 0.5-10 mg / mL dithranol matrix was prepared;
[0110] Inorganic nanomatrix h-BNNs solution, h-BNNs is the boron nitride nanosheets prepared in step (1) of Example 1, 0.5-2.5 mg of inorganic nanomatrix (h-BNNs) is weighed and dispersed in 1 mL of water, and ultrasonically treated for 1 min to prepare inorganic nanomatrix (h-BNNs) solutions with different concentrations of 0.5-2.5 mg / mL;
[0111] Inorganic nanomatrix Fe3O4 solution, Fe3O4 is Fe3O4 prepared in Example 1, and the difference from Example 1 is that h-BNNs are not added, 0.5-2.5 mg of inorganic nanomatrix (Fe3O4) is respectively weighed and dispersed in 1 mL of water, and ultrasonic treatment is performed for 1 min to prepare inorganic nanomatrix (Fe3O4) solutions with different concentrations of 0.5-2.5 mg / mL;
[0112] 0.5-2.5 mg of inorganic nanomatrix (Fe3O4@BN) was weighed and dispersed in 1 mL of water, and ultrasonicated for 1 min to prepare 0.5-2.5 mg / mL inorganic nanomatrix (Fe3O4@BN) solution;
[0113] 0.5-2.5 mg of inorganic nanomatrix (Fe3O4@BN) was weighed and dispersed in 1 mL of ethanol, and ultrasonic treatment was performed for 1 min to prepare 0.5-2.5 mg / mL inorganic nanomatrix (Fe3O4@BN) solution ethanol dispersion.
[0114] Experimental conditions
[0115] A rapifleXTM MALDI-TOF / TOF mass spectrometer equipped with a laser emission wavelength of 355 nm was used to analyze samples in positive (negative) ion mode with a voltage between -20 and 20 kV. Mass spectrometry data was acquired by capturing 500 lasers at a laser frequency of 500 Hz. The scanning range was m / z 150 Da to 1000 Da, and the spatial resolution was 100 μm.
[0116] Further, ion source voltage 1 and ion source voltage 2 are operated at 20 and 19.55 kV, respectively. LasAtten value is 15%. Lens and PIE are set to 11.383 and 2.632, respectively. Reflector voltage 1, reflector voltage 2 and reflector voltage 3 are operated at 22.5, 1.55 and 9.25 kV, respectively. Delay extraction time is 100 ns. Beam scanning range: 30×30 μm 2 , result field: 10 4 ×10 4 μm 2 For the cactus sample, the mode was M5 and the resulting area size was 200 × 200 μm 2 . Laser intensity: 60%.
[0117] The acquired MALDI mass spectrometry data were processed and analyzed using Flex analysis software (4.0). The mass spectrometry imaging data were analyzed using SCiLS2018b software, and the mass spectrometry imaging results were processed by normalizing the total ion counts.
[0118] Sample processing
[0119] Environmental water samples: Collect seafood aquaculture wastewater, seal it in a brown ground-mouth bottle, and store it in a refrigerator at 4°C. First, filter the water sample through a 0.45μm filter membrane to remove suspended matter, add an antioxidant (BHT) to 1mL of the water sample, and then mix it with 100μL of a 1mg / mL Fe3O4@BN solution to complete the enrichment of the target analyte by the Fe3O4@BN inorganic composite nanomatrix. The mixture is oscillated at room temperature for 1h, the matrix is separated by a magnet, the supernatant is discarded, the residue is dispersed in 100μL ultrapure water, and 1μL of the mixed solution is deposited on a MALDI target plate for analysis. The same procedure as above was used to prepare seafood aquaculture wastewater samples treated with different concentrations of antioxidant (BHT).
[0120] Human serum sample: Antioxidant (Irganox565) was added to 1 mL of human serum sample, then an equal amount of PBS and saturated ammonium sulfate solution were added, mixed and allowed to stand for 30 min, centrifuged at 3000 rpm for 10 min to precipitate high-abundance proteins, and the supernatant was collected and mixed with 100 μL of 1 mg / mL Fe3O4@BN solution to complete the enrichment of target analytes by Fe3O4@BN inorganic composite nanomatrix. The mixture was oscillated at room temperature for 1 h, the matrix was separated by magnet, the supernatant was discarded, the residue was dispersed in 100 μL ultrapure water, and 1 μL of the mixture was deposited on the MALDI target plate for analysis. Human serum samples treated with different concentrations of antioxidant (Irganox565) were prepared using the same procedure as above.
[0121] Cactus samples: Growing cacti were exposed to 7 mg AO168 every day for one week. The cacti were cut into blocks and frozen in a -80° freezer. Before slicing, the temperature in the cryostat was set to -30°C. The cactus samples taken out of the -80°C freezer were immediately transferred to the sample holder in the cryostat. Tissue-TekO.CT composite solution (a water-soluble mixture of polyethylene glycol and polyvinyl alcohol) was poured on the cactus for fixation. 15 μm thick cactus slices were prepared at -30°C using a ThermoCryostarNX50 cryostat and mounted on an ITO conductive glass slide. 5 mL of 1 mg / mL Fe3O4@BN ethanol dispersion was repeatedly sprayed on the tissue surface. During spraying, the nozzle was kept 20 cm away from the tissue surface. All samples on the ITO conductive glass slides needed to be dried in a vacuum dryer for 15 min before mass spectrometry imaging.
[0122] Vegetable oil sample: Weigh 2g of edible vegetable oil in a 15mL centrifuge tube, add antioxidant (BHT) to the vegetable oil sample, add 10mL acetonitrile, vortex and oscillate at 3000r / min for 3min, ultrasonically extract for 15 minutes, centrifuge at 10000r / min for 5 minutes, take the supernatant, blow dry with nitrogen, add 10mL ultrapure water, add 5mL of 1mg / mL Fe3O4@BN solution, ultrasonically oscillate for 15 minutes, separate with a magnet, and redisperse the solid residue in 100μL ultrapure water. Take 1μL of the above solution and deposit it on the MALDI target for analysis. Use the same procedure as above to prepare vegetable oil samples treated with different concentrations of antioxidant (BHT).
[0123] 1. Characterization of Fe3O4@BN composites
[0124] In this work, field emission scanning electron microscope (SEM), transmission electron microscope (TEM), X-ray diffractometer (XRD), X-ray photoelectron spectrometer (XPS), specific surface area analyzer and other equipment were used to systematically characterize the microscopic morphology, phase composition, element valence state, specific surface area and other microstructural properties of the prepared h-BNNs and Fe3O4@BN.
[0125] SEM and TEM are used together to observe the microscopic morphology and surface element distribution of the samples. For the SEM test of powdered samples, 10 mg of powder was dispersed in 10 mL of anhydrous ethanol and ultrasonicated for 20 min, and then a small amount of supernatant was dripped on the surface of the silicon wafer and dried naturally. The Si wafer carrying the sample was fixed on the sample stage by conductive double-sided tape, and a platinum coating was sputtered on the surface of the silicon wafer using a parameter combination of 10 mA power, 200 s and 50-60 mTorr to improve conductivity. Finally, SEM images were obtained at an accelerating voltage of 15 kV. For the SEM test of sheet samples (epoxy resin film and other samples), the Al sheet carrying the sample was directly fixed on the sample stage by conductive double-sided tape, and then the platinum coating was sputtered and tested. TEM tests were all carried out on powdered samples. 10 mg of the sample was dispersed in 30 mL of ultrapure water and ultrasonicated for 1 h, and a copper grid was used as the detection sample stage. In addition, the surface element distribution of the sample was characterized using the X-ray energy dispersive spectrum (EDX-Mapping) carried by TEM.
[0126] XPS was used to characterize the chemical composition and valence bond composition of the samples. The prepared samples were connected to the sample stage via double-sided copper tape, and an AlKα target was used to generate X-rays (hν = 1486.6 eV). The test vacuum, operating voltage, and filament current were set to 5×10 -9 mbar, 15 kV and 15 mA; the pass energy was 40 eV, and the energy step was 0.05 eV. C1s = 284.8 eV was used as the energy standard to calibrate the binding energy of each element, and XPSpeak software was used for peak fitting.
[0127] XRD was used to obtain the phase composition information of the samples. The target of the X-ray tube was a Cu target (λ = 0.15418 nm), the scanning angle range was 2theta = 5-90°, and the scanning step was 0.05°. A fully automatic specific surface area and porosity analyzer was used to determine the specific surface area and pore structure information of the samples. 100 mg of the sample was degassed at 150°C for 8 h, and the N2 adsorption / desorption isotherm was measured at 77K. Brunauer-Emmett-Teller (BET) and Barrett Joyner Halenda (BJH) were used to derive the specific surface area and pore size distribution of the samples, respectively.
[0128] In addition, UV-visible spectral data were recorded by a Hitachi U-2910 UV / Visible spectrophotometer. The chemical functional group composition of the obtained materials was measured using a Vertex70 Fourier transform infrared (FT-IR) spectrometer.
[0129] The boron nitride nanosheets and Fe3O4@BN composite materials prepared in Example 1 were selected for characterization:
[0130] The microstructure of Fe3O4@BN samples was investigated by SEM. Figure 1 a and Figure 1 c shows the surface morphology of h-BNNs and Fe3O4@BN. h-BNNs present a two-dimensional graphene-like morphology with wrinkles and curled structures at the edges of the sheets. Magnetic Fe3O4 exists in the form of nanoparticles and is randomly distributed on the surface of h-BNNs. After h-BNNs are composited with Fe3O4, the curled edges in the wrinkled structure are reduced. Metal oxide nanoparticles may also be adsorbed on the curled edges and stretch the edges of h-BNNs during oxidation. SEM results show that Fe3O4 is successfully composited to h-BNNs.
[0131] The microstructure of h-BNNs and Fe3O4@BN samples was investigated by TEM. Figure 1 As shown in b, the TEM image of h-BNNs also shows a typical lamellar morphology, which is consistent with the SEM results. Figure 1 As shown in (d), the TEM image of the Fe3O4@BN sample shows the uniform distribution of Fe3O4 nanoparticles on h-BNNs, with a particle size of approximately 150 nm. The SEM and TEM results indicate that the favorable loading of Fe3O4 on the Fe3O4@BN surface helps to improve the reproducibility of the matrix for detecting the target mass spectrometry signal.
[0132] The paramagnetism of Fe3O4@BN is characterized by the hysteresis regression line, such as Figure 2 As shown in a, there is no hysteresis, coercivity or remanence in the hysteresis curve of Fe3O4@BN, indicating that Fe3O4@BN has good superparamagnetism. The saturation value of the magnetization intensity of Fe3O4@BN is 34.8emu / g, which has a high magnetic sensitivity. Through the external magnetic field, rapid magnetic separation can be achieved, which provides a guarantee for the establishment of a rapid analysis method in the experiment.
[0133] XRD was used to characterize the phase composition of Fe3O4@BN samples. Figure 2 As shown in Figure 2b, the h-BNNs sample exhibits two characteristic diffraction peaks at 26.8° and 41.6°, corresponding to the (002) and (100) crystal planes of h-BNNs, respectively. For the Fe3O4@BN sample, in addition to the characteristic diffraction peaks of h-BNNs, new characteristic diffraction peaks can be observed at 2theta of 30.2°, 35.6°, 43.3°, 53.7°, 57.3° and 62.8°, corresponding to the (200), (311), (400), (422), (511) and (400) crystal planes of Fe3O4, respectively. The appearance of the characteristic diffraction peaks of metal oxides indicates the successful loading of Fe3O4 on h-BNNs.
[0134] The elemental composition and chemical state of Fe3O4@BN samples were characterized by XPS. Figure 2 c, it can be observed that the XPS spectrum has two characteristic bands at 191eV and 398eV, corresponding to B1s and N1s, respectively. h-BNNs are mainly composed of B and N elements. The weak O1s peak may come from the hydroxyl groups on the edge surface. After Fe3O4 composite, three characteristic bands at 724, 710 and 55eV can be observed, corresponding to Fe2p 1 / 2 、Fe2p 2 / 3 and Fe3p. Fe2p 2 / 3 and Fe2p 1 / 2 The peak position is located between the peak positions of 2FeOSiO2 (Fe(II)) and Fe2O3 (Fe(III)). The disappearance of charge transfer around 715 eV also indicates the formation of mixed oxides of Fe(II) and Fe(III). The peak intensity of oxygen atoms also increases due to the attachment of iron oxides. XPS results show that h-BNNs and Fe3O4 are successfully composited. The synergistic structure of the two is conducive to promoting the charge transfer of target molecules and improving the MALDI mass spectrometry activity of the Fe3O4@BN composite matrix.
[0135] The nitrogen adsorption-desorption isotherm was used to characterize the specific surface area of the Fe3O4@BN sample. Figure 2 As shown in Figure d, the curve is a typical type IV isotherm, indicating that Fe3O4@BN is a porous material with typical mesoporous characteristics. The specific surface areas of h-BNNs and Fe3O4@BN calculated based on the BET equation are 1747.8 m 2 / g and 188.5m 2 / g, the decrease in the specific surface area of Fe3O4@BN proves the successful hybridization of Fe3O4. Nitrogen adsorption-desorption isotherms and BET results show that Fe3O4@BN is successfully prepared, which is beneficial to the adsorption of the target and the energy transfer in the MALDI process.
[0136] The surface functional group structure of Fe3O4@BN was investigated by Fourier transform infrared spectroscopy. Figure 3 a, 804 and 1379 cm -1 The absorption peaks at and correspond to the BN out-of-plane bending vibration and BN in-plane tensile vibration on h-BNNs, respectively. Figure 3 As shown in b, 558~636cm -1 The bands in the range describe the symmetric stretching of the Fe-O bond vibration. In addition, the stretching vibration of Fe-O-Fe and the structural vibration of Fe-OH are at 857 and 1030 cm-1, respectively. -1 Appear at 1400cm -1 Another peak at sp 2 In-plane vibration of the BN bond; 1627cm-1 The peaks at 2852 and 2925 cm are the bending vibrations of H2O adsorbed on the surface of the nanocomposite. -1 corresponds to the -BNH2 group. Finally, at 3415 cm -1 The wide band at is attributed to the B-OH group. These results indicate that the Fe3O4 nanoparticles were successfully loaded on the surface of h-BNNs. Therefore, the combination of h-BNNs and Fe3O4 is not only beneficial for the recovery of the adsorbent from the sample solution, but also helps the surface stretching deformation and enhances the physical adsorption of the target with h-BNNs. This modification will also improve the energy transfer efficiency to the target, leading to rapid desorption and ionization.
[0137] The optical properties of Fe3O4@BN samples were investigated using UV-visible absorption spectroscopy. Figure 3 c depicts the UV-visible spectrum of h-BNNs with strong and broad (300-600 nm) light absorption. Fe3O4@BN shows stronger absorption capacity than h-BNNs at 355 nm, indicating that Fe3O4@BN as a composite nanomatrix can promote the desorption and ionization efficiency of the detection target.
[0138] 2. Comparison of Fe3O4@BN as a matrix material with other materials
[0139] The performance comparison was performed to verify the enhancement effect of the designed Fe3O4@BN composite nanomatrix on the five synthetic antioxidants, with the traditional organic matrices (CHCA, DHB and Dithranol) and some inorganic nanomaterials (Fe3O4, h-BNNs) as controls. The concentration of the above matrices was 1 mg / mL.
[0140] like Figure 4 As shown in a, CHCA can only find three targets, namely BHT: m / z 221.24 [M+H] + , Irganox565: m / z589.95[M+H] + and AO168: m / z 754.95 [M+Ag] + .like Figure 4 As shown in b, DHB can only find three targets, namely PZ: m / z200.27[M+H] + ,BHT:m / z267.38[M+H] + and Irganox565: m / z589.95[M+H] + .like Figure 4 As shown in c, Dithranol can only find three targets, namely BHT: m / z 267.38 [M+H] +, Irganox565: m / z589.95[M+H] + and AO168: m / z 754.95 [M+Ag+H] + It can be seen that these commercial organic matrices produce a large number of interfering peaks in the low molecular weight range of m / z 200-600. Figure 4 d and Figure 4 As shown in e, Fe3O4 and h-BNNs can identify four targets, namely PZ: m / z200.27[M+H] + ,BHT:m / z267.38[M+H] + ,Irganox565:m / z589.95[M+H] + (m / z 627.95[M+K] + ), and AO168: m / z 754.95 [M+Ag+H] + .like Figure 4 As shown in f, Fe3O4@BN can identify five targets, namely PZ: m / z200.27[M+H] + ,BHT:m / z267.38[M+H] + , Irganox2246: m / z379.49[M+K] + , Irganox565: m / z589.95[M+H] + (m / z 627.95[M+K] + ), and AO168m / z754.95[M+Ag] + Compared with organic matrices, Fe3O4@BN has a clean background at the low molecular weight end and a higher response; in addition, the composite matrix has a higher response to the target than the monomer Fe3O4 and h-BNNs, which is attributed to the strong absorption of the composite matrix in the ultraviolet region and the synergistic effect of the two. In summary, Fe3O4@BN can effectively improve the desorption / ionization efficiency of the target.
[0141] 3. Investigation of salt resistance and reproducibility of Fe3O4@BN as matrix
[0142] The salt content of actual samples is usually relatively high, and the matrix salt resistance plays a vital role in the detection of samples in complex environments. In order to investigate whether the Fe3O4@BN composite material is interfered by salt, the matrix salt resistance was investigated by adding sodium chloride to the synthetic antioxidant target solution, in which 1 mg / mL Fe3O4@BN solution was used. Figure 5As shown in the figure, when the NaCl concentration increases from 0mM to 500mM, the mass spectrometry signal value of PZ decreases to 88.9% of the original value, the mass spectrometry signal value of BHT decreases to 87.0% of the original value, the mass spectrometry signal value of Irganox2246 decreases to 89.8% of the original value, the mass spectrometry signal value of Irganox565 decreases to 86.5% of the original value, and the mass spectrometry signal value of AO168 decreases to 85.7% of the original value. This result indicates that the Fe3O4@BN composite nanomatrix has strong salt tolerance in the detection of synthetic antioxidants by MALDI mass spectrometry.
[0143] The reproducibility of Fe3O4@BN composite nanomatrix was evaluated by calculating the relative standard deviations (RSDs) of the mass spectrometry signals using 1 mg / mL Fe3O4@BN solution. Figure 6 As shown in a, the relative standard deviations (RSDs) of mass spectrometry signals at different points in the same sample are PZ: 2.76%, BHT: 3.98%, Irganox2246: 5.69%, Irganox565: 3.20%, and AO168: 5.27%. Figure 6 As shown in b, the RSDs among samples (n=30) are PZ: 3.74%, BHT: 4.08%, Irganox2246: 5.50%, Irganox565: 3.49%, and AO168: 4.26%. These results indicate that Fe3O4@BN can be used as a matrix to obtain reliable MALDI mass spectrometry signal reproducibility.
[0144] 4. Determination of BHT in environmental water samples and Irganox565 in human serum samples
[0145] In order to verify the feasibility of Fe3O4@BN as an adsorbent and MALDI inorganic nanomatrix, it was used to analyze BHT in seafood aquaculture wastewater. Figure 7 As shown in a, the linear fitting curve of BHT concentration change and its mass spectrum intensity value shows that BHT has good linearity in the range of 1 to 1000 μg / L, the limit of detection (LOD) is 0.25 μg / L, the limit of quantification (LOQ) is 0.75 μg / L, and the linear correlation coefficient (R 2 )=0.9986. The reproducibility of the method was investigated, and its precision RSD was 3.65%~8.73%. In order to further study the application of Fe3O4@BN in the analysis of actual wastewater samples, the established method was used to determine BHT in seafood aquaculture wastewater. Figure 7 b is the mass spectrum of blank aquaculture wastewater. The spike recovery experiment (5 μg / L) was performed on blank aquaculture wastewater to compare the recovery rate before enrichment ( Figure 7 c) and after enrichment ( Figure 7d) Mass spectra collected by BHT, after enrichment, the mass spectrometric peak with significantly enhanced BHT signal can be clearly observed. As can be seen from Table 2, the recovery rate of BHT in seafood aquaculture wastewater is 87.2% to 102.7%. The results show that the Fe3O4@BN composite inorganic nanomatrix can be successfully used for the application of MALDI mass spectrometry to determine BHT in seafood aquaculture wastewater.
[0146] To further evaluate the potential of Fe3O4@BN as an adsorbent and MALDI matrix, we applied it to the analysis of Irganox565 in human serum samples. Figure 8 As shown in a, the linear fitting curve of Irganox565 concentration change and its mass spectrum intensity value shows that Irganox565 has good linearity in the range of 5-750 μg / L, the limit of detection (LOD) is 1 μg / L, the limit of quantification (LOQ) is 3.5 μg / L, and the linear correlation coefficient (R 2 )=0.9961. The reproducibility of the method was investigated, and the precision RSD of the method was 3.75%~6.49%. In order to further study the application of Fe3O4@BN in the actual serum sample analysis, Figure 8 As shown in b, Irganox565 in human serum samples was determined using the established method. Figure 6-8 b is the mass spectrum of blank human serum. The spike recovery experiment (5 μg / L) was performed on blank human serum samples to compare the recovery rate before enrichment ( Figure 8 c) and after enrichment ( Figure 8 d) Mass spectra collected by Irganox565. After enrichment, the mass spectrometric peak with significantly enhanced Irganox565 signal can be clearly observed. As listed in Table 3, the recovery of Irganox565 in serum ranged from 81.34% to 109.4%. The results showed that the Fe3O4@BN composite inorganic nanomatrix can be successfully used for the determination of Irganox565 in human serum samples by MALDI mass spectrometry.
[0147] Table 3 Fe3O4@BN as adsorbent and matrix for MADI mass spectrometry detection of BHT in aquaculture wastewater and Irganox565 in human serum
[0148]
[0149]
[0150] Note: ND was not detected.
[0151] 5. Determination of AO168 in cactus samples
[0152] The distribution of AO168 in cactus was quantitatively analyzed by Fe3O4@BN composite nanomatrix-assisted mass spectrometry imaging. On the surface of blank cactus tissue, 1 μL of 10, 50, 100, 500, and 1000 μg / L AO168 standard solutions were dripped, respectively, and the mass spectrometry images presented were as follows: Fig. 9 a. The linear fitting curve of AO168 concentration change and its mass spectrometry imaging signal absolute intensity is shown in Fig. 9 As shown in b, AO168 in blank cactus showed good linearity in the range of 10-1000 μg / L, and the linear correlation coefficient (R 2 )=0.9832, and the method detection limit (LOD, S / N=3) is 2.5μg / L. Fig.10 As shown in a, the cactus cross section from outside to inside is epidermis, vascular bundle, xylem and pith. The distribution of AO168 in cactus is as follows Fig.10 b-10d. After exposure to a specific dose, different areas of the cactus showed different degrees of AO168 migration. The AO168 content in the epidermal tissue was determined to be in the range of 125 to 200 μg / L ( Fig.10 b, 10c). In addition, the concentration of AO168 in the vascular bundle ranged from 150 to 300 μg / L ( Fig.10 c, 10d), the concentration in the central column was about 450 μg / L ( Fig.10 e). Therefore, the Fe3O4@BN composite inorganic nanomatrix-assisted mass spectrometry imaging method can not only effectively visualize the distribution of AO168 in cactus, but also accurately and quantitatively determine the concentration level of AO168.
[0153] 6. Determination of BHT in edible oil samples
[0154] It is used for the analysis of BHT in edible oil samples, such as Fig.11 As shown in Table 4, BHT has good linearity in the range of 5-500 ng / g, the detection limit is 1 ng / g, the quantification limit is 3.5 ng / g, and the linear coefficient r = 0.9922. The reproducibility of the method was studied, and the relative standard deviation of the precision of the method was 5.19% to 8.23%. In order to further study the performance of Fe3O4@BN in quantitative analysis, BHT in edible oil samples was determined by the established method. As can be seen from Table 4, the recovery rate of BHT in peanut oil is 85.6% to 111.2%. The results show that the Fe3O4@BN composite inorganic nanomatrix can be successfully used for the application of MALDI mass spectrometry to determine BHT in edible oil samples.
[0155] Table 4 Fe3O4@BN as adsorbent and matrix for MADI mass spectrometry detection of BHT in peanut oil.
[0156]
[0157] 7. Mechanism study
[0158] like Fig.12 As shown in the figure, the good MALDI mass spectrometry performance of the Fe3O4@BN composite matrix can be attributed to the following three aspects:
[0159] (1) High electron transfer desorption ability: Compared with h-BNNs, the Fe3O4@BN nanocomposite material formed after loading Fe3O4 nanoparticles exhibits higher absorbance under 355 nm laser irradiation. This property allows the Fe3O4@BN matrix to be used as a matrix for MALDI-TOF-MS, absorbing the energy of UV laser irradiation and increasing the surface temperature to desorb and ionize the target analytes.
[0160] Using 1-(Benzyl)pyridinium chloride (BP) as a chemical thermometer, the simplified survival yield method (SY) was used to analyze the ion internal energy transfer efficiency of Fe3O4@BN matrix for MALDI mass spectrometry. Fig.13 As shown in the figure, the SY value of Fe3O4@BN is 62.86% and the SY value of h-BNNs is 75.87%. It can be seen that the Fe3O4@BN matrix has a stronger desorption ability than h-BNNs, thus promoting the ionization of the target.
[0161] (2) Favorable enrichment affinity: There are three types of hydrogen bonds (B-NH…OH-, B-OH…NH-, and -OH…OH-) between Fe3O4@BN and analytes such as Irganox565. These hydrogen bonds contribute to the adsorption of the target by Fe3O4@BN. The binding energy values of -OH and -NH between Fe3O4@BN and the analyte were studied and analyzed using DFT, and the values were -29.62, -48.14, and -70.92 kJ / mol, respectively. The hydrogen bonding interaction between the matrix and the analyte molecules improves the target recognition ability and achieves effective energy transfer to the target.
[0162] (3) Effective charge transport capability: The curled edges in the Fe3O4@BN wrinkle structure are reduced, and the metal oxide nanoparticles are adsorbed on the curled edges, which stretches the edges of the composite matrix, and the large specific surface area and mesoporous structure enable it to effectively transport electrons. Compared with organic matrices and inorganic monomer nanomatrices, Fe3O4@BN exhibits a higher signal response to the synthetic antioxidant, further indicating that the composite matrix efficiently transports electrons to promote the desorption and ionization of the target.
[0163] Therefore, the present invention uses the magnetic nanocomposite Fe3O4@BN as a matrix and enrichment medium for the first time to detect antioxidants in the environment and food. Fig.14As shown, schematic diagram of the preparation of Fe3O4@BN and its enhanced MALDI mass spectrometry and imaging analysis of antioxidant compounds.
[0164] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A mass spectrometry method for rapid detection of antioxidants in the environment and food, characterized in that: The method comprises the following steps: a) preparing a composite material of boron nitride nanosheets and magnetic Fe3O4 nanoparticles; b) Fe3O4@BN composite material was used as MALDI matrix and enrichment medium; c) Mixing the sample to be tested with the Fe3O4@BN composite material and performing MALDI mass spectrometry analysis.
2. The mass spectrometry method for rapid detection of antioxidants in environment and food according to claim 1, characterized in that: The preparation method of the Fe3O4@BN composite material comprises the following steps: a) preparing boron nitride nanosheets by high temperature calcination method; Weigh urea and boric acid, mix them with methanol aqueous solution, shake them evenly, and then heat and evaporate until a white crystalline powder of the precursor is formed, then calcine the powder to obtain white boron nitride nanosheets, and then wash, dry and grind to obtain two-dimensional porous boron nitride nanosheets; b) mixing the boron nitride nanosheets with an iron salt solution; Boron nitride nanosheets were dispersed in deionized water and sonicated, then FeCl3·6H2O and FeCl2·4H2O were added and sonicated continuously to ensure complete mixing; c) adding an alkaline solution to the mixed solution for reaction; NH4OH solution was added dropwise until the mixture became alkaline, and then magnetic stirring was performed; d) heating, washing and drying the reaction product to obtain a Fe3O4@BN composite material.
3. The mass spectrometry method for rapid detection of antioxidants in environment and food according to claim 2, characterized in that: a) urea and boric acid are mixed with 18-22 ml of methanol aqueous solution, shaken for 1-1.2 hours, and then heated and evaporated at 50-55°C until a white crystalline powder of the precursor is formed. Then, the powder is transferred to a quartz boat and placed in a tube furnace for calcination. The temperature of the tube furnace is heated from room temperature to 1000-1100°C at a rate of 4-5°C / min, and then maintained at 1000-1100°C for 2-2.5 hours under N2 protection. After the reaction is completed, the tube furnace is cooled from 1000-1100°C to 200-300°C at a rate of 5-10°C / min. Finally, the furnace temperature is naturally cooled to room temperature. The obtained white boron nitride nanosheet product is washed with methanol for multiple times and dried in an oven at 50-60°C. After grinding, the obtained two-dimensional porous boron nitride nanosheet is dried and stored at room temperature; The molar ratio of urea to boric acid is 0.1-0.2 mol: 0.04 mol-0.06 mol; the volume ratio of methanol to deionized water in the methanol aqueous solution is 1:1.2; Preferably, 0.15 mol urea and 0.05 mol boric acid are mixed with 20 ml of a methanol aqueous solution with a volume ratio of 1:1, shaken for 1 hour, and then heated and evaporated at 50°C until a white crystalline powder of the precursor is formed. Then, the powder is transferred to a quartz boat and placed in a tube furnace for calcination. The temperature of the tube furnace is heated from room temperature to 1000°C at a rate of 5°C / min, and then maintained at 1000°C for 2 hours under N2 protection. After the reaction is completed, the tube furnace is cooled from 1000°C to 200°C at a rate of 5°C / min, and finally the furnace temperature is naturally cooled to room temperature. The obtained white boron nitride nanosheet product is washed three times with methanol and dried in an oven at 50°C. After grinding, the obtained two-dimensional porous boron nitride nanosheet is dried and stored at room temperature; b) Boron nitride nanosheets were dispersed in deionized water, ultrasonically treated for 30-40 min, and then FeCl3·6H2O and FeCl2·4H2O were added, and the ultrasonic treatment was continued for 30-50 min; Preferably, the mass ratio of the boron nitride nanosheets to the volume of deionized water is (50-250) mg:100 mL; the mass ratio of the boron nitride nanosheets to FeCl3·6H2O and FeCl2·4H2O is 1:(8-10):(2.3-3.3); Preferably, 150 mg of boron nitride nanosheets are dispersed in 100 mL of deionized water, ultrasonically treated for 30 min, and then 1.35 g of FeCl3·6H2O and 0.5 g of FeCl2·4H2O are added, and ultrasonic treatment is continued for 30 min; c) adding 3-10 mL of 13-15 M NH4OH solution dropwise until the mixture becomes alkaline, and then stirring magnetically for 3.5-5 h; Preferably, 3 mL of 14 M NH4OH solution is added dropwise until the mixture is alkaline to pH 8.0, and then magnetic stirring is performed for 3.5 h; d) placing the reaction product obtained in step c) into a hydrothermal reactor, reacting for 9-12 hours under the protection of N2 atmosphere and at a temperature of 160-180°C, then gradually cooling to room temperature, washing with deionized water and anhydrous ethanol, placing in an oven, and drying at 70-100°C to obtain a Fe3O4@BN composite material; Preferably, the reaction product obtained in step c) is placed in a hydrothermal reactor, reacted for 10 hours under the protection of N2 atmosphere and at a temperature of 175°C, then gradually cooled to room temperature, washed with deionized water and anhydrous ethanol, placed in an oven, and dried at 70°C to obtain a Fe3O4@BN composite material.
4. The mass spectrometry method for rapid detection of antioxidants in environment and food according to claim 1, characterized in that: The sample is an environmental water sample, a biological sample or a food sample; Preferably, the environmental water sample includes industrial wastewater or aquaculture wastewater, the biological sample includes serum or plant tissue, and the food sample is a vegetable oil sample.
5. The mass spectrometry method for rapid detection of antioxidants in environment and food according to claim 1, characterized in that: Equipped with rapifleX with a laser emission wavelength of 355nm TM The MALDI-TOF / TOF mass spectrometer is used to analyze samples in positive (negative) ion mode, with a voltage between -20-20 kV, and a laser frequency of 500 Hz. Mass spectral data is acquired by capturing 500 lasers, with a scanning range of m / z 150 Da to 1000 Da and a spatial resolution of 100 μm.
6. A Fe3O4@BN composite material, characterized in that: The invention comprises boron nitride nanosheets (h-BNNs) and magnetic Fe3O4 nanoparticles, wherein the Fe3O4 nanoparticles are uniformly distributed on the surface of the boron nitride nanosheets.
7. A method for preparing the Fe3O4@BN composite material according to claim 6, characterized in that: The following steps are involved: a) preparing boron nitride nanosheets by high temperature calcination method; Weigh urea and boric acid, mix them with methanol aqueous solution, shake them evenly, and then heat and evaporate until a white crystalline powder of the precursor is formed, then calcine the powder to obtain white boron nitride nanosheets, and then wash, dry and grind to obtain two-dimensional porous boron nitride nanosheets; b) mixing the boron nitride nanosheets with an iron salt solution; Boron nitride nanosheets were dispersed in deionized water and sonicated, then FeCl3·6H2O and FeCl2·4H2O were added and sonicated continuously to ensure complete mixing; c) adding an alkaline solution to the mixed solution for reaction; NH4OH solution was added dropwise until the mixture became alkaline, and then magnetic stirring was performed; d) heating, washing and drying the reaction product to obtain a Fe3O4@BN composite material.
8. The preparation method according to claim 7, characterized in that: The following steps are involved: a) urea and boric acid are mixed with 18-22 ml of methanol aqueous solution, shaken for 1-1.2 hours, and then heated and evaporated at 50-55°C until a white crystalline powder of the precursor is formed. Then, the powder is transferred to a quartz boat and placed in a tube furnace for calcination. The temperature of the tube furnace is heated from room temperature to 1000-1100°C at a rate of 4-5°C / min, and then maintained at 1000-1100°C for 2-2.5 hours under N2 protection. After the reaction is completed, the tube furnace is cooled from 1000-1100°C to 200-300°C at a rate of 5-10°C / min. Finally, the furnace temperature is naturally cooled to room temperature. The obtained white boron nitride nanosheet product is washed with methanol for multiple times and dried in an oven at 50-60°C. After grinding, the obtained two-dimensional porous boron nitride nanosheet is dried and stored at room temperature; The molar ratio of urea to boric acid is 0.1-0.2 mol: 0.04 mol-0.06 mol; the volume ratio of methanol to deionized water in the methanol aqueous solution is 1:1.2; Preferably, 0.15 mol urea and 0.05 mol boric acid are mixed with 20 ml of a methanol aqueous solution with a volume ratio of 1:1, shaken for 1 hour, and then heated and evaporated at 50°C until a white crystalline powder of the precursor is formed. Then, the powder is transferred to a quartz boat and placed in a tube furnace for calcination. The temperature of the tube furnace is heated from room temperature to 1000°C at a rate of 5°C / min, and then maintained at 1000°C for 2 hours under N2 protection. After the reaction is completed, the tube furnace is cooled from 1000°C to 200°C at a rate of 5°C / min, and finally the furnace temperature is naturally cooled to room temperature. The obtained white boron nitride nanosheet product is washed three times with methanol and dried in an oven at 50°C. After grinding, the obtained two-dimensional porous boron nitride nanosheet is dried and stored at room temperature; b) Boron nitride nanosheets were dispersed in deionized water, ultrasonically treated for 30-40 min, and then FeCl3·6H2O and FeCl2·4H2O were added, and the ultrasonic treatment was continued for 30-50 min; Preferably, the mass ratio of the boron nitride nanosheets to the volume of deionized water is (50-250) mg:100 mL; the mass ratio of the boron nitride nanosheets to FeCl3·6H2O and FeCl2·4H2O is 1:(8-10):(2.3-3.3); Preferably, 150 mg of boron nitride nanosheets are dispersed in 100 mL of deionized water, ultrasonically treated for 30 min, and then 1.35 g of FeCl3·6H2O and 0.5 g of FeCl2·4H2O are added, and ultrasonic treatment is continued for 30 min; c) adding 3-10 mL of 13-15 M NH4OH solution dropwise until the mixture becomes alkaline, and then stirring magnetically for 3.5-5 h; Preferably, 3 mL of 14 M NH4OH solution is added dropwise until the mixture is alkaline to pH 8.0, and then magnetic stirring is performed for 3.5 h; d) placing the reaction product obtained in step c) into a hydrothermal reactor, reacting for 9-12 hours under the protection of N2 atmosphere and at a temperature of 160-180°C, then gradually cooling to room temperature, washing with deionized water and anhydrous ethanol, placing in an oven, and drying at 70-100°C to obtain a Fe3O4@BN composite material; Preferably, the reaction product obtained in step c) is placed in a hydrothermal reactor, reacted for 10 hours under the protection of N2 atmosphere and at a temperature of 175°C, then gradually cooled to room temperature, washed with deionized water and anhydrous ethanol, placed in an oven, and dried at 70°C to obtain a Fe3O4@BN composite material.
9. Application of the Fe3O4@BN composite material according to claim 6 in the following fields: a) Detection of antioxidants in environmental samples; b) Detection of antioxidants in biological samples; c) Detection of antioxidants in food samples; d) mass spectrometry imaging analysis; e) Quantitative analysis of antioxidants; Preferably, the environmental water sample includes industrial wastewater or aquaculture wastewater, the biological sample includes but is not limited to serum, plant tissue and other biological fluids; and the food sample is a vegetable oil sample.
10. The use according to claim 9, characterized in that: The Fe3O4@BN composite material is used for mass spectrometry imaging quantitative analysis and is suitable for analyzing the spatial distribution and content level of antioxidants in plant samples.
Citation Information
Cited By
Method for detecting liquid phase content of BHT and EMQ in solid antioxidant
CN119198973A
Detection method of BHT and EMQ liquid content in solid antioxidants
CN119198973B
Direct mass spectrometric detection method for degrading antioxidant in plastic and kit thereof