Metal foil, metal-clad laminate, wiring board, semiconductor, negative electrode, and battery

By optimizing the relationship between the square resistance value and elastic modulus value of the metal layer and the carrier layer, the problem of wrinkling and curling of the carrier metal foil in production is solved, the tensile resistance and yield of the metal foil are improved, and the production cost is reduced.

CN118983129APending Publication Date: 2024-11-19GUANGZHOU FANGBANG ELECTRONICS +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411157724.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing metal foil with carrier is prone to wrinkles or automatic curling during the production process, resulting in low yield rate for preparing fine circuit boards, affecting product quality and production costs.

Method used

By optimizing the relationship between the square resistance value and elastic modulus value of the metal layer and the carrier layer, we ensure that the mechanical properties of the metal layer and the carrier layer are close, reduce stratification phenomenon, and control the longitudinal elastic modulus and square resistance within a specific strain range. The product difference value reduces the risk of breakage of metal foil during winding.

Benefits of technology

It effectively improves the tensile resistance and yield of metal foil, reduces wrinkles and fine stripes, improves the quality of metal foil and the preparation efficiency of applied products, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983129A_ABST
    Figure CN118983129A_ABST
Patent Text Reader

Abstract

The invention discloses a metal foil, a metal-clad laminated plate, a circuit board, a semiconductor, a negative electrode and a battery, the metal foil comprises a carrier layer and a metal layer, the metal layer is arranged on one surface of the carrier layer, the strain of the metal layer and the strain of the carrier layer are respectively in the range of 0.2%-0.5%, and the strain of the metal layer and the strain of the carrier layer are respectively in the range of 0.2%-0.5%. The elastic modulus value E (gold) of the metal layer and the elastic modulus value E (load) of the carrier layer meet the following relational expression: R1E (gold)-R2E (load) is greater than or equal to 1100 and less than or equal to 50000; wherein R1 is the sheet resistance value of the metal layer, and R2 is the sheet resistance value of the carrier layer. By adopting the method, the probability of wrinkles on the surface of the metal foil can be reduced, the layering phenomenon is reduced, and the tensile property and the yield of the metal foil are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal foil, and in particular to a metal foil, a metal-clad laminate, a circuit board, a semiconductor, a negative electrode and a battery. Background Art

[0002] With the rapid development of the electronics industry, metal foil is widely used in printed circuit boards, battery negative electrode materials, chip packaging and other fields. The quality of metal foil will directly affect the quality of manufactured circuit boards, batteries and other products.

[0003] The metal foil with carrier is a composite structure of at least two layers, including a metal layer and a carrier layer stacked in layers. However, the inventors have found that the prior art has at least the following problems: the surface of the existing metal foil with carrier is prone to wrinkles or automatic curling during the production process, which results in the metal foil with carrier being unable to be used to prepare fine circuit boards, or the yield rate of the circuit boards prepared using the metal foil with carrier is low, which seriously affects the production of fine circuit boards. In addition, the metal foil with carrier that is prone to wrinkles is not convenient for curling packaging and transportation of samples, which will increase production costs. Summary of the invention

[0004] The purpose of the embodiments of the present invention is to provide a metal foil, a metal-clad laminate, a circuit board, a semiconductor, a negative electrode and a battery, which can reduce the probability of wrinkles on the surface of the metal foil, reduce the delamination phenomenon, and effectively improve the tensile performance and yield rate of the metal foil.

[0005] To achieve the above object, an embodiment of the present invention provides a metal foil, including a carrier layer and a metal layer, wherein the metal layer is arranged on one surface of the carrier layer, and the strains of the metal layer and the carrier layer are respectively in the range of 0.2% to 0.5%, and the elastic modulus value E of the metal layer is 金 and the elastic modulus value E of the carrier layer 载 The relationship between them is: 1100≤|R1E 金 -R2E 载 |≤50000; wherein R1 is the square resistance of the metal layer, and R2 is the square resistance of the carrier layer.

[0006] As an improvement of the above solution, when the strains of the metal layer and the carrier layer are respectively in the range of 0.2% to 0.5%, the longitudinal elastic modulus value E of the metal layer is 11 and the longitudinal elastic modulus value E of the carrier layer 12 The relationship between them is: 1600≤|R1E 11 -R2E 12 |≤48400.

[0007] As an improvement of the above solution, when the strains of the metal layer and the carrier layer are respectively in the range of 0.5% to 0.8%, the longitudinal elastic modulus value E of the metal layer is 13 and the longitudinal elastic modulus value E of the carrier layer 14 The relationship between them is: 1000≤|R1E 13 -R2E 14 |≤38940.

[0008] As an improvement of the above solution, when the strains of the metal layer and the carrier layer are respectively in the range of 0.2% to 0.5%, the transverse elastic modulus value E of the metal layer is 21 and the transverse elastic modulus value E of the carrier layer 22 The relationship between them is: 1500≤|R1E 21 -R2E 22 |≤40200.

[0009] As an improvement of the above solution, when the strains of the metal layer and the carrier layer are respectively in the range of 0.5% to 0.8%, the transverse elastic modulus value E of the metal layer is 23 and the transverse elastic modulus value E of the carrier layer 24 The relationship between them is: 2560≤|R1E 23 -R2E 24 |≤36000.

[0010] As an improvement of the above solution, when the strain of the metal layer is in the range of 0.2% to 0.5%, the longitudinal elastic modulus value E of the metal layer is 11 and the transverse elastic modulus E 21 The relationship between them is:

[0011] As an improvement of the above solution, when the strain of the carrier layer is in the range of 0.2% to 0.5%, the longitudinal elastic modulus value E of the carrier layer is 12 and the transverse elastic modulus E 22 The relationship between them is:

[0012] As an improvement of the above solution, when the strain of the metal layer is in the range of 0.5% to 0.8%, the longitudinal elastic modulus value E of the metal layer is 13 and the transverse elastic modulus E 23 The relationship between them is:

[0013] As an improvement of the above solution, when the strain of the carrier layer is in the range of 0.5% to 0.8%, the longitudinal elastic modulus value E of the carrier layer is 14 and the transverse elastic modulus E 24 The relationship between them is:

[0014] As an improvement of the above solution, the roughness Ra of the surface of the carrier layer close to the metal layer is 0.1-1.5 μm.

[0015] As an improvement of the above solution, the metal layer and / or the carrier layer includes at least a two-layer structure.

[0016] As an improvement of the above solution, the metal foil further includes a dielectric layer, and the dielectric layer is arranged on at least one surface of the metal layer.

[0017] As an improvement of the above solution, the metal foil further includes an adhesive layer, and the adhesive layer is provided on at least one surface of the metal layer.

[0018] An embodiment of the present invention further provides a metal-clad laminate, comprising the metal foil as described in any one of the above items.

[0019] An embodiment of the present invention further provides a circuit board, characterized in that the circuit board comprises the metal foil as described in any one of the above items or the metal-clad laminate as described in the above items.

[0020] An embodiment of the present invention further provides a semiconductor material, characterized in that the semiconductor material comprises the metal foil as described in any one of the above items.

[0021] An embodiment of the present invention further provides a negative electrode material for a battery, characterized in that the negative electrode material comprises the metal foil as described in any one of the above items.

[0022] An embodiment of the present invention further provides a battery, characterized in that the negative electrode material of the battery includes any of the metal foils described above.

[0023] Compared with the prior art, the present invention discloses a metal foil, a metal-clad laminate, a circuit board, a semiconductor, a negative electrode and a battery, wherein the metal foil comprises a carrier layer and a metal layer, and the relationship between the square resistance value and the elastic modulus value of the metal layer and the carrier layer is optimized, and under a specific strain range of the metal foil, the difference between the product of the longitudinal elastic modulus and the square resistance of the metal layer and the product of the longitudinal elastic modulus and the square resistance of the carrier layer is limited, so that the difference between the two is not much or is similar, indicating that the mechanical properties of the two are relatively close, ensuring that the structure and performance presented by the carrier layer and the conductive layer in the metal foil are more uniform, reducing the delamination phenomenon, and being able to effectively avoid the situation where the metal foil is easy to break during the winding process, and at the same time being able to reduce or improve the problem that the thinner metal foil is easy to wrinkle, fine stripes, etc. during the preparation process, effectively improving the tensile resistance and yield of the metal foil, thereby effectively improving the quality of the metal foil, and improving the quality and preparation efficiency of the application products containing the metal foil. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is a schematic structural diagram of a first metal foil provided by an embodiment of the present invention;

[0025] Figure 2 is a schematic structural diagram of a second metal foil provided by an embodiment of the present invention;

[0026] Figure 3 is a schematic structural diagram of a third metal foil provided by an embodiment of the present invention;

[0027] Figure 4 is a schematic structural diagram of a fourth metal foil provided by an embodiment of the present invention;

[0028] Figure 5 is a schematic structural diagram of a fifth metal foil provided by an embodiment of the present invention;

[0029] Among them, 1. carrier layer; 2. metal layer; 3. dielectric layer; 4. adhesive layer. DETAILED DESCRIPTION

[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] In the description of the present application, it should be understood that the terms "center", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0032] The terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, "plurality" means two or more.

[0033] In the description of this application, it should be noted that, unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those commonly understood by those skilled in the art. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. For those of ordinary skill in the art, the specific meanings of the above terms in this application can be understood by specific circumstances.

[0034] See also Figure 1 , is a schematic structural diagram of the first metal foil provided in an embodiment of the present invention. An embodiment of the present invention provides a metal foil, including a carrier layer 1 and a metal layer 2, wherein the metal layer 2 is arranged on a surface of the carrier layer 1, that is, the carrier layer 1 and the metal layer 2 are stacked.

[0035] It should be noted that the carrier layer 1 is used to carry and protect the metal layer 2 so that the metal layer is not damaged by external contact or collision. After the metal foil and the circuit board are pressed together at high temperature, the carrier layer 1 needs to be peeled off.

[0036] When the strains of the metal layer and the carrier layer are respectively in the range of 0.2% to 0.5%, the elastic modulus value E of the metal layer 金 and the elastic modulus value E of the carrier layer 载 The relationship between them is: 1100≤|R1E 金 -R2E 载 |≤50000; wherein R1 is the square resistance of the metal layer, and R2 is the square resistance of the carrier layer.

[0037] In the embodiment of the present invention, in order to avoid the problem that a large stress appears inside the thinner metal foil, which may cause the metal foil to be easily wrinkled, curled or broken during the production process, thereby affecting the production efficiency and yield rate, the embodiment of the present invention comprehensively considers the strain of the metal layer and the carrier layer, the elastic modulus and square resistance of the metal layer, the elastic model and square resistance of the carrier layer, and other parameters. When the strain of the metal foil is within the range of 0.2% to 0.5%, the elastic modulus E of the metal layer 2 is controlled. 金 The product of the square resistance R1 and the elastic modulus E of the carrier layer 1 载 The absolute value of the difference between the product of |R1E and the square resistance R2 金 -R2E 载 | is between 1100 and 50000, and specifically can be 1100, 2000, 3500, 4000, 4528, 4600, 4745, 4840, 6149, 8000, 10386, 12028, 15498, 18542, 20457, 23548, 28548, 30124, 31737, 33451, 35862, 37452, 38718, 40521, 41076, 43200, 45100, 46200, 47100 or 50000. Of course, it can also be any other value between 1100 and 50000, which is not specifically limited here.

[0038] When the strains of the metal layer and the carrier layer are respectively in the range of 0.2% to 0.5%, the longitudinal elastic modulus value E of the metal layer 11 and the longitudinal elastic modulus value E of the carrier layer 12 The relationship between them is: 1600≤|R1E 11 -R2E 12 |≤48400; wherein R1 is the square resistance of the metal layer 1, and R2 is the square resistance of the carrier layer 2.

[0039] It should be noted that the above relationship is dimensionless. The unit of elastic modulus E is kgf / mm 2 , the unit of square resistance R is milliohm.

[0040] In the embodiment of the present invention, in order to avoid the problem that a large stress appears inside the thinner metal foil, which may cause the metal foil to be easily wrinkled, curled or broken during the production process, thereby affecting the production efficiency and yield rate, the embodiment of the present invention comprehensively considers the strain of the metal layer and the carrier layer, the elastic modulus and square resistance of the metal layer, the elastic model and square resistance of the carrier layer, and other parameters. When the strain of the metal foil is in the range of 0.2% to 0.5%, the longitudinal elastic modulus E of the metal layer 2 is controlled. 11 The product of the square resistance R1 and the longitudinal elastic modulus E of the carrier layer 1 12The absolute value of the difference between the product of |R1E and the square resistance R2 11 -R2E 12 |It is between 1600 and 48400, and specifically can be 1600, 2045, 3150, 3500, 4000, 4528, 4600, 4745, 4840, 5567, 6149, 8000, 10386, 12028, 15498, 18542, 20457, 23548, 25759, 28548, 30124, 31737, 32654, 33451, 35862, 37452, 38718, 40521, 41076, 43200, 45100, 46200, 47100 or 48400. Of course, it can also be any other value between 1600 and 48400, which is not specifically limited here.

[0041] More preferably, the strains of the metal layer and the carrier layer are respectively in the range of 0.2% to 0.5%, and the longitudinal elastic modulus value E of the metal layer is 11 and the longitudinal elastic modulus value E of the carrier layer 12 The relationship between them is: 4528≤|R1E 11 -R2E 12 |≤31737.

[0042] By adopting the technical means of the embodiment of the present invention, since the ranges of the square resistance and elastic modulus of the metal layer and the carrier layer are different under different strain values ​​of the metal foil, and the square resistance and elastic modulus of the metal layer and the carrier layer are related to multiple factors such as the thickness, constituent elements, type and content of the metal layer and the carrier layer themselves, by optimizing the relationship between the square resistance and elastic modulus of the metal layer and the carrier layer, under a specific strain range of the metal foil, the difference between the product of the longitudinal elastic modulus and the square resistance of the metal layer and the product of the longitudinal elastic modulus and the square resistance of the carrier layer is limited, so that the difference between the two is not much or is similar, indicating that the mechanical properties of the two are relatively close, ensuring that the structure and performance presented by the carrier layer and the conductive layer in the metal foil are more uniform, reducing the delamination phenomenon, and effectively avoiding the situation that the metal foil is easy to break during the winding process. At the same time, it can reduce or improve the problem that the thinner metal foil is prone to wrinkles, fine stripes, etc. during the preparation process, effectively improving the tensile resistance and yield of the metal foil, thereby effectively improving the quality of the metal foil, and improving the quality and preparation efficiency of the application products containing the metal foil.

[0043] As a preferred embodiment, based on the above embodiment, when the strains of the metal layer and the carrier layer are respectively in the range of 0.2% to 0.5%, the longitudinal elastic modulus E of the metal layer 2 is 11 The value range is 3100~6500kgf / mm2 . For example, it can be 3100kgf / mm 2 、3197.09kgf / mm 2 、3722.99kgf / mm 2 、4330.31kgf / mm 2 、5138.64kgf / mm 2 、4461.06kgf / mm 2 、5622.96kgf / mm 2 、5000kgf / mm 2 or 6200kgf / mm 2 Of course, the longitudinal elastic modulus E 11 It can also be between 3100 and 6500 kgf / mm 2 Any other values ​​between and are not described here.

[0044] The longitudinal elastic modulus E of the carrier layer 1 12 The value range is 1200~4000kgf / mm 2 . For example, it can be 1200kgf / mm 2 、1500kgf / mm 2 、1983.53kgf / mm 2 、2825.39kgf / mm 2 、3197kgf / mm 2 or 3722.99kgf / mm 2 Of course, the longitudinal elastic modulus E 12 It can also be between 1200 and 4000 kgf / mm 2 Any other values ​​between and are not described here.

[0045] By adopting the technical means of the embodiment of the present invention, the strains of the metal layer and the carrier layer are respectively within the range of 0.2% to 0.5%, and the range of the longitudinal elastic modulus values ​​of the metal layer and the carrier layer is limited respectively, which can effectively control the longitudinal elastic modulus of each structural layer of the metal foil to be within a reasonable range, and can ensure that the elastic deformation of each metal foil product is within a reasonable range, thereby ensuring the stability and qualified rate of the metal foil product. And on the basis of satisfying the longitudinal elastic modulus range, the difference between the product of the longitudinal elastic modulus and square resistance of the metal layer and the product of the longitudinal elastic modulus and square resistance of the carrier layer is controlled to be within a reasonable range of 1600 to 48400, which more effectively ensures that the structure and performance presented by the carrier layer and the conductive layer in the metal foil are more uniform, reduces the delamination phenomenon, and avoids the situation that the metal foil is easy to break during the winding process. At the same time, it can reduce or improve the problem that the thinner metal foil is prone to wrinkles, fine stripes, etc. during the preparation process, effectively improve the tensile performance and yield of the metal foil, and thus effectively improve the quality of the metal foil.

[0046] As a preferred embodiment, when the strains of the metal layer and the carrier layer are respectively in the range of 0.5% to 0.8%, the longitudinal elastic modulus value E of the metal layer 13 and the longitudinal elastic modulus value E of the carrier layer 14 The relationship between them is: 1000≤|R1E 13 -R2E 14 |≤38940. The relation is dimensionless.

[0047] In the embodiment of the present invention, when the strain of the metal foil is in the range of 0.5% to 0.8%, the longitudinal elastic modulus E of the metal layer 2 is controlled. 13 The product of the square resistance R1 and the longitudinal elastic modulus E of the carrier layer 1 14 The absolute value of the difference between the product of |R1E and the square resistance R2 13 -R2E 14 | is between 1000 and 38940, and can specifically be 1000, 1171, 1256, 1387, 1424, 1600, 2345, 3345, 4234, 4528, 4600, 4745, 4840, 5267, 6160, 8630, 10366, 12058, 15408, 18642, 19759, 20417, 21313, 23248, 26759, 30124, 32654, 35562, 36472, 37112 or 38940. Of course, it can also be any other value between 1000 and 38940, which is not specifically limited here.

[0048] More preferably, the strains of the metal layer and the carrier layer are respectively in the range of 0.5% to 0.8%, and the longitudinal elastic modulus value E of the metal layer is 11 and the longitudinal elastic modulus value E of the carrier layer 12 The relationship between them is: 1171≤|R1E 11 -R2E 12 |≤21313.

[0049] As a preferred embodiment, based on the above embodiment, when the strains of the metal layer and the carrier layer are respectively in the range of 0.5% to 0.8%, the longitudinal elastic modulus E of the metal layer 2 is 13 The value range is 1000~4000kgf / mm 2 . For example, it can be 1166.94kgf / mm 2 、1537.05kgf / mm 2 、2730.98kgf / mm 2 、3283.79kgf / mm 2 、3100kgf / mm 2 or 3739.98kgf / mm 2 Of course, the longitudinal elastic modulus E 13 It can also be between 1000 and 4000 kgf / mm 2 Any other values ​​between and are not described here.

[0050] The longitudinal elastic modulus E of the carrier layer 1 14 The value range is 900~3800kgf / mm 2 . For example, it can be 900kgf / mm 2 、1100kgf / mm 2 、1121.92kgf / mm 2 、1512.33kgf / mm 2 、2683.96kgf / mm 2 or 3688.92kgf / mm 2 Of course, the longitudinal elastic modulus E 14 It can also be between 900 and 3800 kgf / mm 2 Any other values ​​between and are not described here.

[0051] By adopting the technical means of the embodiment of the present invention, the strains of the metal layer and the carrier layer are respectively within the range of 0.5% to 0.8%, and the range of the longitudinal elastic modulus values ​​of the metal layer and the carrier layer is limited respectively, which can effectively control the longitudinal elastic modulus of each structural layer of the metal foil to be within a reasonable range, and can ensure that the elastic deformation of each metal foil product is within a reasonable range, thereby ensuring the stability and qualified rate of the metal foil product. And on the basis of satisfying the longitudinal elastic modulus range, the product of the longitudinal elastic modulus and square resistance of the metal layer is controlled, and the difference between the product of the longitudinal elastic modulus and square resistance of the carrier layer is within a reasonable range of 1000 to 38940, which more effectively ensures that the structure and performance presented by the carrier layer and the conductive layer in the metal foil are more uniform, reduces the delamination phenomenon, and avoids the situation that the metal foil is easy to break during the winding process. At the same time, it can reduce or improve the problem that the thinner metal foil is easy to wrinkle, fine stripes, etc. during the preparation process, effectively improve the tensile performance and yield of the metal foil, and thus effectively improve the quality of the metal foil.

[0052] As a preferred embodiment, when the strain of the metal layer and the carrier layer is in the range of 0.2% to 0.5%, the transverse elastic modulus value E of the metal layer 21 and the transverse elastic modulus value E of the carrier layer 22 The relationship between them is: 1500≤|R1E 21 -R2E 22 |≤40200. The relationship is dimensionless.

[0053] In the embodiment of the present invention, when the strain of the metal foil is in the range of 0.2% to 0.5%, the transverse elastic modulus E of the metal layer 2 is controlled. 21 The product of the square resistance R1 and the transverse elastic modulus E of the carrier layer 1 22 The absolute value of the difference between the product of |R1E and the square resistance R2 21 -R2E 22 |It is between 1500 and 40200, and specifically can be 1500, 1621, 1900, 2045, 3150, 3486, 3665, 4130, 4528, 4600, 4745, 4840, 5567, 6149, 8000, 10386, 12028, 15498, 18542, 20457, 23548, 25759, 28548, 30124, 31737, 32654, 33451, 35862, 37452, 38718, 39413 or 40200. Of course, it can also be any other value between 1000 and 38940, which is not specifically limited here.

[0054] More preferably, the strains of the metal layer and the carrier layer are respectively in the range of 0.2% to 0.5%, and the transverse elastic modulus value E of the metal layer is 21 and the transverse elastic modulus value E of the carrier layer 22 The relationship between them is: 3665≤|R1E 21 -R2E 22 |≤39413.

[0055] As a preferred embodiment, based on the above embodiment, when the strains of the metal layer and the carrier layer are respectively in the range of 0.2% to 0.5%, the transverse elastic modulus E of the metal layer 2 is 21 The value range is 2500~5200kgf / mm 2 . For example, it can be 2680.26kgf / mm 2 、3237.66kgf / mm 2 、4445.67kgf / mm 2 、4740.39kgf / mm 2 、4800kgf / mm 2 or 5200kgf / mm 2 Of course, the transverse elastic modulus E 21 It can also be between 2500 and 5200 kgf / mm 2 Any other values ​​between and are not described here.

[0056] The transverse elastic modulus E of the carrier layer 1 22 The value range is 1400~3500kgf / mm 2 . For example, it can be 1400kgf / mm 2 、2000kgf / mm 2 、2186.15kgf / mm 2 、2497.81kgf / mm 2 、2680.26kgf / mm 2 or 3237.66kgf / mm 2 Of course, the transverse elastic modulus E 22 It can also be between 1400 and 3500 kgf / mm 2 Any other values ​​between and are not described here.

[0057] By adopting the technical means of the embodiment of the present invention, the strains of the metal layer and the carrier layer are respectively within the range of 0.2% to 0.5%, and the range of the transverse elastic modulus values ​​of the metal layer and the carrier layer is limited respectively, which can effectively control the transverse elastic modulus of each structural layer of the metal foil to be within a reasonable range, and can ensure that the elastic deformation of each metal foil product is within a reasonable range, thereby ensuring the stability and qualified rate of the metal foil product. And on the basis of satisfying the transverse elastic modulus range, the product of the transverse elastic modulus and square resistance of the metal layer is controlled, and the difference between the product of the transverse elastic modulus and square resistance of the carrier layer is within a reasonable range of 1500 to 40200, which more effectively ensures that the structure and performance presented by the carrier layer and the conductive layer in the metal foil are more uniform, reduces the delamination phenomenon, and avoids the situation that the metal foil is easy to break during the winding process. At the same time, it can reduce or improve the problem that the thinner metal foil is easy to wrinkle, fine stripes, etc. during the preparation process, effectively improve the tensile performance and yield of the metal foil, and thus effectively improve the quality of the metal foil.

[0058] As a preferred embodiment, when the strains of the metal layer and the carrier layer are respectively in the range of 0.5% to 0.8%, the transverse elastic modulus value E of the metal layer 23 and the transverse elastic modulus value E of the carrier layer 24 The relationship between them is: 2560≤|R1E 23 -R2E 24 |≤36000. The relation is dimensionless.

[0059] In the embodiment of the present invention, when the strain of the metal foil is in the range of 0.5% to 0.8%, the transverse elastic modulus E of the metal layer 2 is controlled. 23 The product of the square resistance R1 and the transverse elastic modulus E of the carrier layer 1 24 The absolute value of the difference between the product of |R1E and the square resistance R2 23 -R2E 24 |It is between 2560 and 36000, and specifically can be 2560, 2717, 2800, 3024, 3257, 3486, 3600, 4130, 4498, 4613, 4861, 5567, 6149, 7890, 10386, 13528, 16198, 17900, 21289, 23548, 26159, 28548, 30124, 31737, 32654, 33451, 35862 or 36000. Of course, it can also be any other value between 2560 and 36000, which is not specifically limited here.

[0060] More preferably, the strains of the metal layer and the carrier layer are respectively in the range of 0.5% to 0.8%, and the transverse elastic modulus value E of the metal layer is23 and the transverse elastic modulus value E of the carrier layer 24 The relationship between them is: 2560≤|R1E 23 -R2E 24 |≤28252.

[0061] As a preferred embodiment, based on the above embodiment, when the strains of the metal layer and the carrier layer are respectively in the range of 0.5% to 0.8%, the transverse elastic modulus E of the metal layer 2 is 23 The value range is 1000~5000kgf / mm 2 . For example, it can be 1068kgf / mm 2 、2434.64kgf / mm 2 、2828.4kgf / mm 2 、3031.81kgf / mm 2 、4593.6kgf / mm 2 、4915.87kgf / mm 2 or 5000kgf / mm 2 Of course, the transverse elastic modulus E 23 It can also be between 1000 and 5000 kgf / mm 2 Any other values ​​between and are not described here.

[0062] The transverse elastic modulus E of the carrier layer 1 24 The value range is 600~2500kgf / mm 2 . For example, it can be 600kgf / mm 2 、1238.22kgf / mm 2 、1405.85kgf / mm 2 、1068kgf / mm 2 or 2434.64kgf / mm 2 Of course, the transverse elastic modulus E 24 It can also be between 600 and 2500 kgf / mm 2 Any other values ​​between and are not described here.

[0063] By adopting the technical means of the embodiment of the present invention, the strains of the metal layer and the carrier layer are respectively within the range of 0.5% to 0.8%, and the range of the transverse elastic modulus values ​​of the metal layer and the carrier layer is limited respectively, which can effectively control the transverse elastic modulus of each structural layer of the metal foil to be within a reasonable range, and can ensure that the elastic deformation of each metal foil product is within a reasonable range, thereby ensuring the stability and qualified rate of the metal foil product. And on the basis of satisfying the transverse elastic modulus range, the product of the transverse elastic modulus and square resistance of the metal layer is controlled, and the difference between the product of the transverse elastic modulus and square resistance of the carrier layer is within a reasonable range of 2560 to 36000, which more effectively ensures that the structure and performance presented by the carrier layer and the conductive layer in the metal foil are more uniform, reduces the delamination phenomenon, and avoids the situation that the metal foil is easy to break during the winding process. At the same time, it can reduce or improve the problem that the thinner metal foil is prone to wrinkles, fine stripes, etc. during the preparation process, effectively improve the tensile performance and yield of the metal foil, and thus effectively improve the quality of the metal foil.

[0064] As a preferred embodiment, when the strain of the metal layer is in the range of 0.2% to 0.5%, the longitudinal elastic modulus value E of the metal foil is 11 and the transverse elastic modulus E 21 The relationship between them is:

[0065]

[0066] In the embodiment of the present invention, when the strain of the metal layer is in the range of 0.2% to 0.5%, the longitudinal elastic modulus E of the metal layer 2 11 and the transverse elastic modulus E 21 The ratio is in the range of 0.58 to 1.39, for example, it can be 0.58, 0.86, 1.17, 0.91, 0.98, 1.16 or 1.39. Of course, the ratio can also be any other value between 0.58 and 1.39, which will not be repeated here.

[0067] As a preferred embodiment, when the strain of the metal layer is in the range of 0.5% to 0.8%, the longitudinal elastic modulus value E of the metal layer is 13 and the transverse elastic modulus E 23 The relationship between them is:

[0068]

[0069] In the embodiment of the present invention, when the strain of the metal layer is in the range of 0.5% to 0.8%, the longitudinal elastic modulus E of the metal layer 2 13 and the transverse elastic modulus E 23The ratio is in the range of 0.48 to 1.40, for example, it can be 0.48, 0.63, 0.81, 0.9, 1.16 or 1.40. Of course, the ratio can also be any other value between 0.48 and 1.40, which will not be repeated here.

[0070] By adopting the technical means of the embodiments of the present invention, the ratio of the longitudinal elastic modulus and the transverse elastic modulus of the metal layer itself is limited within the specific strain range of the metal layer, thereby ensuring that the difference between the longitudinal elastic modulus and the transverse elastic modulus of the metal layer is not too large, thereby improving the uniformity of the metal layer surface in the transverse and longitudinal latitudes, thereby making the metal layer have excellent bending resistance, tensile strength, warping resistance, tensile strength and reasonable deformation capacity in the transverse and longitudinal latitudes, thereby effectively improving the quality of the metal foil.

[0071] As a preferred embodiment, when the strain of the carrier layer is in the range of 0.2% to 0.5%, the longitudinal elastic modulus value E of the carrier layer is 12 and the transverse elastic modulus E 22 The relationship between them is:

[0072]

[0073] In the embodiment of the present invention, when the strain of the carrier layer is in the range of 0.2% to 0.5%, the longitudinal elastic modulus value E of the carrier layer 1 is 12 and the transverse elastic modulus E 22 The ratio is in the range of 0.79 to 1.39, for example, it can be 0.79, 0.86, 1.29, 0.98, 1.38 or 1.39. Of course, the ratio can also be any other value between 0.79 and 1.39, which will not be repeated here.

[0074] As a preferred embodiment, when the strain of the carrier layer is in the range of 0.5% to 0.8%, the longitudinal elastic modulus value E of the carrier layer is 14 and the transverse elastic modulus E 24 The relationship between them is:

[0075]

[0076] In the embodiment of the present invention, when the strain of the carrier layer is in the range of 0.2% to 0.5%, the longitudinal elastic modulus value E of the carrier layer 1 is 14 and the transverse elastic modulus E 24 The ratio is in the range of 0.46 to 1.50, for example, it can be 0.46, 0.65, 0.79, 1.5, 1.22 or 1.50. Of course, the ratio can also be any other value between 0.46 and 1.50, which will not be repeated here.

[0077] By adopting the technical means of the embodiments of the present invention, the ratio of the longitudinal elastic modulus and the transverse elastic modulus of the carrier layer itself is limited within the specific strain range of the metal foil, thereby ensuring that the difference between the longitudinal elastic modulus and the transverse elastic modulus of the carrier layer is not too large, thereby improving the uniformity of the surface of the carrier layer in the transverse and longitudinal dimensions, and thereby making the carrier layer have excellent bending resistance, tensile strength, warping resistance, tensile strength and reasonable deformation capacity in both the transverse and longitudinal dimensions, thereby effectively improving the quality of the metal foil.

[0078] As a preferred embodiment, the roughness Ra of the surface of the carrier layer 1 close to the metal layer 2 is 0.1-1.5 μm, and the thickness of the metal layer is 1-9 μm.

[0079] It should be noted that the arithmetic mean roughness Ra is specifically the arithmetic mean of the absolute values ​​of the contour ordinate value Z(x) within a sampling length, and the ordinate value Z(x) refers to the distance from each point on the contour to the contour centerline. The arithmetic mean roughness Ra is used to evaluate the arithmetic mean deviation of the surface profile, which can fully reflect the height characteristics of the surface micro-geometry.

[0080] In an embodiment of the present invention, on the basis that the elastic modulus and square resistance of the carrier layer 1 and the metal layer 2 satisfy the above-mentioned relationship, the roughness Ra of the surface of the carrier layer 1 close to the metal layer 2 is further optimized to be between 0.1 and 1.5 μm, for example, it can be 0.10 μm, 0.20 μm, 0.30 μm, 0.50 μm, 0.60 μm, 0.80 μm, 1.10 μm, 1.20 μm, 1.30 μm, 1.40 μm or 1.50 μm. Of course, the specific value of the arithmetic mean roughness Ra of the roughened surface can be set according to actual use requirements, and no further details are given here.

[0081] By adopting the technical means of the embodiments of the present invention, the roughness of the side of the carrier layer close to the metal layer is within a most reasonable range, thereby improving the bonding performance between the carrier layer and the metal layer, greatly improving the adhesion effect, and avoiding problems such as delamination, wrinkles or curling during manufacturing or transportation. At the same time, it also meets the requirements for appropriate peel strength between the carrier layer and the metal layer before and after lamination with application carriers such as circuit board substrates, effectively improving the quality of the metal foil.

[0082] As a preferred embodiment, the metal layer and / or the carrier layer includes at least a two-layer structure.

[0083] In an embodiment of the present invention, the metal layer 2 is a composite structure including at least two layers, that is, the metal layer is composed of two or more layers stacked together, and each layer of the structure can be made of the same material or different materials, and can be adjusted according to actual usage requirements.

[0084] See also Figure 2 , is a schematic diagram of the structure of the second metal foil provided in an embodiment of the present invention, taking the metal layer as a two-layer structure as an example, which are a first metal layer 21 and a second metal layer 22, respectively. The first metal layer 21 and the second metal layer 22 are stacked in sequence and stacked on the carrier layer 1.

[0085] Preferably, the metal layer 2 includes a single metal conductive layer and / or an alloy conductive layer; wherein the single metal conductive layer is made of any one of copper, aluminum, iron, zinc, titanium, cobalt, gold, silver, nickel, chromium, indium, gallium, tin, thallium, lead, bismuth, germanium, antimony, polonium, beryllium, magnesium, calcium, strontium, barium, radium, lanthanide metals, actinide metals and transition metals; the alloy conductive layer is made of any two or more of copper, aluminum, iron, zinc, titanium, cobalt, gold, silver, nickel, chromium, indium, gallium, tin, thallium, lead, bismuth, germanium, antimony, polonium, beryllium, magnesium, calcium, strontium, barium, radium, lanthanide metals, actinide metals and transition metals; and may be a mixture of any two or more of the above metals and other materials.

[0086] The carrier layer 1 is a composite structure including at least two layers, that is, the carrier layer is formed by stacking two or more layers, and each layer of the structure can be made of the same material or different materials, which can be adjusted according to actual use requirements.

[0087] See also Figure 3 , is a schematic diagram of the structure of the third metal foil provided in an embodiment of the present invention, taking the carrier layer as a two-layer structure as an example, which are a first carrier layer 11 and a second carrier layer 12, respectively, and the first carrier layer 11 and the second carrier layer 12 are stacked in sequence.

[0088] Preferably, the carrier layer 1 is made of a metal material or a non-metal material. The metal material includes at least one of metal elements such as copper, aluminum, nickel and zinc; the non-metal material includes organic films and the like. Since the carrier layer 1 mainly plays a bearing role, a certain thickness is required. The specific thickness of the carrier layer 1 can be set according to the actual use requirements, and no further details are given here. The carrier layer 1 is separated from the metal layer 2 in a strippable removal manner or in a non-stripping removal manner. When the carrier layer 1 is removed in a non-stripping removal manner, the non-stripping manner may be, for example, laser etching, chemical etching, grinding, plasma removal, etc. When the carrier layer 1 is removed by stripping, the stripping manner may be, for example, manual stripping and direct removal, or stripping and removal with the aid of mechanical equipment.

[0089] By adopting the technical means of the embodiments of the present invention, the metal layer and / or the carrier layer is set as a composite structure of at least two layers, and structural layers of different materials are set according to the performance requirements of the metal foil, which is conducive to improving the performance of the metal foil.

[0090] As a preferred embodiment, see Figure 4 , is a schematic structural diagram of a fourth metal foil provided in an embodiment of the present invention, wherein the metal foil further comprises a dielectric layer 3, and the dielectric layer 3 is disposed on at least one surface of the metal layer 2. As an example, the metal foil is a four-layer structure in which a carrier layer 1, a dielectric layer 3, a metal layer 2 and a dielectric layer 3 are sequentially stacked, and the dielectric layer 3 is disposed on both surfaces of the metal layer 2.

[0091] Preferably, the material of the dielectric layer 3 is selected from at least one of polyimide, epoxy resin, modified epoxy resin, modified acrylic resin, cyanate resin, polyethylene terephthalate, polybutylene terephthalate, polyethylene, polyethylene naphthalate, polystyrene, polyvinyl chloride, polysulfone, polyphenylene sulfide, polyetheretherketone, polyphenylene ether, polytetrafluoroethylene, liquid crystal polymer, polyoxadiazole, epoxy glass cloth, BT resin, metal, and ceramic.

[0092] By adopting the technical means of the embodiment of the present invention, the dielectric layer 3 mainly plays an insulating role. When the metal foil is used in the fields of printed circuit boards or battery materials, the dielectric layer can isolate the metal layer to avoid short circuits between electrodes. At the same time, the dielectric layer has excellent dielectric properties and can prepare capacitors with low dielectric losses.

[0093] As a preferred embodiment, see Figure 5, is a schematic diagram of the structure of the fifth metal foil provided in an embodiment of the present invention, wherein the metal foil further comprises an adhesive layer 4, and the adhesive layer 4 is disposed on at least one surface of the metal layer 2. As an example, the metal foil is a four-layer structure in which a carrier layer 1, an adhesive layer 4, a metal layer 2 and an adhesive layer 4 are sequentially stacked, and adhesive layers 4 are disposed on both surfaces of the metal layer 2.

[0094] Preferably, the material of the adhesive layer is selected from at least one of polystyrene, vinyl acetate, polyester, polyethylene, polyamide, rubber or acrylic thermoplastic resins, phenolic, epoxy, thermoplastic polyimide, urethane, melamine or alkyd thermosetting resins, BT resin, and ABF resin.

[0095] By adopting the technical means of the embodiment of the present invention, the adhesive layer 4 mainly plays a bonding role, thereby improving the adhesion between two adjacent material layers. When the adhesive layer is arranged between the carrier layer and the metal layer, it can effectively improve the adhesion between the carrier layer and the metal layer, avoid separation, wrinkles and other problems, ensure the peeling strength between the metal layer and the carrier layer, and ensure that the carrier layer can be stably peeled off from the metal layer, so that the entire surface of the carrier layer 1 is more uniform and dense, which is conducive to peeling off the carrier layer 1 to obtain an extremely thin metal foil with fewer pinholes, and further facilitates the subsequent production of circuits. When the adhesive layer is arranged on the side of the metal layer away from the carrier layer, when the metal foil is used in the fields of printed circuit boards or battery materials, it can improve the adhesion between the metal layer and the pressed application material, thereby improving the quality of the application product containing the metal foil. For example, when used in the field of new energy batteries, it can ensure the maximum adhesion and bonding between the conductive layer surface of the metal foil and the negative active material of the battery, avoiding the peeling and falling of the negative active material on the surface of the conductive layer. At the same time, an adhesive layer with an appropriate amount of attachment can avoid too much bonding aid in the bonding layer, which will increase the weight and volume of the metal foil itself, affecting the weight control of the battery and the improvement of the energy density.

[0096] The properties of the common metal foil and the metal foil in the structure of the embodiment of the present invention were tested respectively by using specific examples, as follows:

[0097] Example 1

[0098] A metal foil, comprising a carrier layer and a metal layer, wherein the metal layer is arranged on one surface of the carrier layer, and the strains of the metal layer and the carrier layer are respectively in the range of 0.2% to 0.5%, and the longitudinal elastic modulus value E of the metal layer 11 and the longitudinal elastic modulus of the carrier layer E 12 The relationship between them is: |R1E 11 -R2E 12 |=1600.

[0099] Example 2

[0100] The metal foil of this embodiment is the same as that of embodiment 1, except that: the strains of the metal layer and the carrier layer are respectively in the range of 0.2% to 0.5%, and the longitudinal elastic modulus value E of the metal layer is 11 and the longitudinal elastic modulus of the carrier layer E 12 The relationship between them is: |R1E 111 -R2E 12 |=48400.

[0101] Example 3

[0102] The metal foil of this embodiment is the same as that of embodiment 1, except that: the strains of the metal layer and the carrier layer are respectively in the range of 0.2% to 0.5%, and the longitudinal elastic modulus value E of the metal layer is 11 and the longitudinal elastic modulus of the carrier layer E 12 The relationship between them is: |R1E 11 -R2E 12 |=20000.

[0103] Example 4

[0104] The metal foil of this embodiment is the same as that of embodiment 3, except that: the strains of the metal layer and the carrier layer are respectively in the range of 0.5% to 0.8%, and the longitudinal elastic modulus value E of the metal layer is 13 and the longitudinal elastic modulus value E of the carrier layer 14 The relationship between them is: |R1E 13 -R2E 14 |=1000.

[0105] Example 5

[0106] The metal foil of this embodiment is the same as that of embodiment 3, except that: the strains of the metal layer and the carrier layer are respectively in the range of 0.5% to 0.8%, and the longitudinal elastic modulus value E of the metal layer is 13 and the longitudinal elastic modulus value E of the carrier layer 14 The relationship between them is: |R1E 13 -R2E 14 |=38000.

[0107] Example 6

[0108] The metal foil of this embodiment is the same as that of embodiment 3, except that: the strains of the metal layer and the carrier layer are respectively in the range of 0.2% to 0.5%, and the transverse elastic modulus value E of the metal layer is 21 and the transverse elastic modulus of the carrier layer E 22The relationship between them is: |R1E 21 -R2E 22 |=1600.

[0109] Example 7

[0110] The metal foil of this embodiment is the same as that of embodiment 3, except that: the strains of the metal layer and the carrier layer are respectively in the range of 0.2% to 0.5%, and the transverse elastic modulus value E of the metal layer is 21 and the transverse elastic modulus of the carrier layer E 22 The relationship between them is: |R1E 21 -R2E 22 |=40000.

[0111] Example 8

[0112] The metal foil of this embodiment is the same as that of embodiment 5, except that: the strains of the metal layer and the carrier layer are respectively in the range of 0.5% to 0.8%, and the transverse elastic modulus value E of the metal layer is 23 and the transverse elastic modulus of the carrier layer E 24 The relationship between them is: |R1E 23 -R2E 24 |=2600.

[0113] Example 9

[0114] The metal foil of this embodiment is the same as that of embodiment 5, except that: the strains of the metal layer and the carrier layer are respectively in the range of 0.5% to 0.8%, and the transverse elastic modulus value E of the metal layer is 23 and the transverse elastic modulus of the carrier layer E 24 The relationship between them is: |R1E 23 -R2E 24 |=35000.

[0115] Example 10

[0116] The metal foil of this embodiment is the same as that of embodiment 6, except that: when the strain of the metal layer is in the range of 0.2% to 0.5%, the longitudinal elastic modulus value E of the metal layer is 11 and the transverse elastic modulus E 21 The relationship between them is: 11 / E 21 =0.89.

[0117] Embodiment 11

[0118] The metal foil of this embodiment is the same as that of embodiment 6, except that: when the strain of the metal layer is in the range of 0.2% to 0.5%, the longitudinal elastic modulus value E of the metal layer is 11and the transverse elastic modulus E 21 The relationship between them is: 11 / E 21 =1.30

[0119] Example 12

[0120] The metal foil of this embodiment is the same as that of embodiment 6, except that: when the strain of the carrier layer is in the range of 0.2% to 0.5%, the longitudinal elastic modulus value E of the carrier layer is 12 and the transverse elastic modulus E d2 The relationship between them is: 12 / E 22 =0.8.

[0121] Example 13

[0122] The metal foil of this embodiment is the same as that of embodiment 6, except that: when the strain of the carrier layer is in the range of 0.2% to 0.5%, the longitudinal elastic modulus value E of the carrier layer is 12 and the transverse elastic modulus E 22 The relationship between them is: 12 / E 22 =1.28.

[0123] Embodiment 14

[0124] The metal foil of this embodiment is the same as that of embodiment 9, except that when the strain of the metal layer is in the range of 0.5% to 0.8%, the longitudinal elastic modulus value E of the metal layer is 13 and the transverse elastic modulus E 23 The relationship between them is: 13 / E 23 =0.5.

[0125] Embodiment 15

[0126] The metal foil of this embodiment is the same as that of embodiment 9, except that when the strain of the metal layer is in the range of 0.5% to 0.8%, the longitudinal elastic modulus value E of the metal layer is 13 and the transverse elastic modulus E 23 The relationship between them is: 13 / E 23 =1.2.

[0127] Example 16

[0128] The metal foil of this embodiment is the same as that of embodiment 9, except that when the strain of the carrier layer is in the range of 0.5% to 0.8%, the longitudinal elastic modulus value E of the carrier layer is 14 and the transverse elastic modulus E 24 The relationship between them is: 14 / E24 =0.5.

[0129] Embodiment 17

[0130] The metal foil of this embodiment is the same as that of embodiment 9, except that when the strain of the carrier layer is in the range of 0.5% to 0.8%, the longitudinal elastic modulus value E of the carrier layer is 14 and the transverse elastic modulus E 24 The relationship between them is: 14 / E 24 =1.4.

[0131] Comparative Example 1

[0132] The metal foil of this embodiment is the same as that of embodiment 3, except that: the strains of the metal layer and the carrier layer are respectively in the range of 0.2% to 0.5%, and the longitudinal elastic modulus value E of the metal layer is 11 and the longitudinal elastic modulus of the carrier layer E 12 The relationship between them is: |R1E 11 -R2E 12 |=55000.

[0133] The above embodiments and comparative examples were tested and classified as excellent, good, fair, poor, etc. according to the relative test results therebetween.

[0134] The test results are as follows:

[0135]

[0136]

[0137] It should be noted that the longitudinal elastic modulus and transverse elastic modulus of the metal foil can be tested by an electronic universal testing machine, and can be obtained by inputting the thickness, length and width of the metal foil in the test software. In order to improve the accuracy of the test results, each set of data is tested more than 30 times, and the average value of all results is taken as the final test result. Among them, the gauge length of the metal foil test sample is 100mm and the width is 10mm. Surface wrinkles and stratification can be obtained by observing, counting and analyzing the surface of the metal foil.

[0138] It can be seen from the above comparison table that the metal foil samples provided by the embodiments of the present invention have excellent wrinkle resistance and delamination resistance compared with the control samples.

[0139] An embodiment of the present invention further provides a metal-clad laminate, which comprises the metal foil as described in any one of the above embodiments.

[0140] It should be noted that the metal foil comprises a carrier layer 1 and a metal layer 2, and its specific structure can refer to the structure of the metal foil described in any of the above embodiments, which will not be described in detail here.

[0141] It should be noted that the metal-clad laminate can be a flexible copper-clad laminate (FCCL), also known as a flexible copper-clad laminate. The structure of the flexible copper-clad laminate includes: a metal foil layer, an adhesive layer, a metal foil layer, or includes: a metal foil layer, an adhesive layer. The adhesive layer material can be polyimide (PI), thermoplastic polyimide (TPI), resin, etc.

[0142] The metal-clad laminate may also be resin-coated copper (RCC), which is mainly used for high-density circuits. In this case, the roughened surface of the metal foil is away from the side of the copper foil coated with resin.

[0143] Compared with the prior art, the application of improved metal foil as the above flexible copper-clad laminate material has the following advantages: by controlling the difference between the product of the longitudinal elastic modulus and the square resistance of the metal layer and the product of the longitudinal elastic modulus and the square resistance of the carrier layer within a reasonable range, the probability of wrinkles on the surface of the metal foil can be reduced, the delamination phenomenon can be reduced, and the tensile performance and yield of the metal foil can be effectively improved, so that the yield of the manufactured metal-clad laminate products is improved, and the performance of the product is more stable and reliable in the subsequent specific use process, the high-frequency signal transmission loss is smaller, and the production cost is reduced.

[0144] An embodiment of the present invention further provides a circuit board, which includes a circuit substrate and the metal foil as described in any one of the above embodiments or the metal-clad laminate as described in the above embodiments.

[0145] It should be noted that the structure of the metal foil or metal-clad laminate may refer to the structure of the metal foil or metal-clad laminate described in any of the above embodiments, and will not be described in detail here.

[0146] By adopting the technical means of the embodiments of the present invention and improving the structure of the metal foil, it is suitable for the production of high-frequency and high-density circuit boards, can effectively improve the quality of metal foil products, improve the adhesion of the metal foil when combined with the circuit board substrate, further reduce blistering, wrinkles and cracks, improve the quality and processing efficiency of the circuit boards, and reduce the defective rate of the circuit boards.

[0147] An embodiment of the present invention further provides a semiconductor material, wherein the semiconductor material includes the metal foil as described in any one of the above embodiments.

[0148] It should be noted that the metal foil comprises a carrier layer 1 and a metal layer 2, and its specific structure can refer to the structure of the metal foil described in any of the above embodiments, which will not be described in detail here.

[0149] By adopting the technical means of the embodiments of the present invention and using the metal foil as a semiconductor material, the metal foil structure is improved, thereby improving the quality of the metal foil product, and the metal foil is suitable for making semiconductor devices and integrated circuits. The adhesion of the metal foil can be effectively improved, and blistering, wrinkling and cracking can be further reduced, thereby improving the quality and processing efficiency of semiconductor devices and integrated circuits and reducing the defective rate of semiconductor devices and integrated circuits.

[0150] An embodiment of the present invention further provides a negative electrode material for a battery, wherein the negative electrode material includes the metal foil as described in any one of the above embodiments.

[0151] It should be noted that the metal foil comprises a carrier layer 1 and a metal layer 2, and its specific structure can refer to the structure of the metal foil described in any of the above embodiments, which will not be described in detail here.

[0152] An embodiment of the present invention further provides a battery, wherein the negative electrode material of the battery includes the metal foil as described in any one of the above embodiments.

[0153] Compared with the prior art, the use of the metal foil as the negative electrode carrier or current collector of the above battery has the following advantages: the structure of the metal foil is improved, the quality of the metal foil product is improved, and the bonding strength requirements of the metal foil are effectively met. It can be applied to new energy batteries, such as lithium batteries and sodium ion batteries. In the negative electrode material, as a negative electrode current collector and carrier material, the negative electrode active material of the battery can be tightly combined with the metal foil. During the use of the battery, the negative electrode active material is not easy to fall off. When subjected to strong impact or the battery charging and discharging process, the metal foil material is not easy to break or deform, which is beneficial to improving the service life and safety of the new energy battery.

[0154] The above is a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.

Claims

1. A metal foil, characterized in that: The invention comprises a carrier layer and a metal layer, wherein the metal layer is arranged on one surface of the carrier layer, and the strains of the metal layer and the carrier layer are respectively in the range of 0.2% to 0.5%, and the elastic modulus value E of the metal layer 金 and the elastic modulus value E of the carrier layer 载 The relationship between them is: 1100≤|R1E 金 -R2E 载 |≤50000; wherein R1 is the square resistance of the metal layer, and R2 is the square resistance of the carrier layer.

2. The metal foil according to claim 1, characterized in that When the strains of the metal layer and the carrier layer are respectively in the range of 0.2% to 0.5%, the longitudinal elastic modulus value E of the metal layer 11 and the longitudinal elastic modulus value E of the carrier layer 12 The relationship between them is: 1600≤|R1E 11 -R2E 12 |≤48400.

3. The metal foil according to claim 1, characterized in that When the strains of the metal layer and the carrier layer are respectively in the range of 0.5% to 0.8%, the longitudinal elastic modulus value E of the metal layer 13 and the longitudinal elastic modulus value E of the carrier layer 14 The relationship between them is: 1000≤|R1E 13 -R2E 14 |≤38940.

4. The metal foil according to claim 1, characterized in that When the strains of the metal layer and the carrier layer are respectively in the range of 0.2% to 0.5%, the transverse elastic modulus value E of the metal layer 21 and the transverse elastic modulus value E of the carrier layer 22 The relationship between them is: 1500≤|R1E 21 -R2E 22 |≤40200.

5. The metal foil according to claim 1, wherein When the strains of the metal layer and the carrier layer are respectively in the range of 0.5% to 0.8%, the transverse elastic modulus value E of the metal layer 23 and the transverse elastic modulus value E of the carrier layer 24 The relationship between them is: 2560≤|R1E 23 -R2E 24 |≤36000.

6. The metal foil according to claim 4, characterized in that When the strain of the metal layer is in the range of 0.2% to 0.5%, the longitudinal elastic modulus value E of the metal layer 11 and the transverse elastic modulus E 21 The relationship between them is:

7. The metal foil according to claim 4, characterized in that When the strain of the carrier layer is in the range of 0.2% to 0.5%, the longitudinal elastic modulus value E of the carrier layer 12 and the transverse elastic modulus E 22 The relationship between them is:

8. The metal foil according to claim 5, characterized in that When the strain of the metal layer is in the range of 0.5% to 0.8%, the longitudinal elastic modulus value E of the metal layer 13 and the transverse elastic modulus E 23 The relationship between them is:

9. The metal foil according to claim 5, characterized in that When the strain of the carrier layer is in the range of 0.5% to 0.8%, the longitudinal elastic modulus value E of the carrier layer 14 and the transverse elastic modulus E 24 The relationship between them is:

10. The metal foil according to claim 1, wherein The roughness Ra of the surface of the carrier layer close to the metal layer is 0.1-1.5 μm.

11. The metal foil according to any one of claims 1 to 10, characterized in that The metal layer and / or the carrier layer includes at least a two-layer structure.

12. The metal foil according to any one of claims 1 to 10, characterized in that The metal foil further includes a dielectric layer, and the dielectric layer is disposed on at least one surface of the metal layer.

13. The metal foil according to any one of claims 1 to 10, characterized in that The metal foil further includes an adhesive layer disposed on at least one surface of the metal layer.

14. A metal-clad laminate, characterized in that: Comprising the metal foil according to any one of claims 1 to 13.

15. A circuit board, characterized in that: The circuit board includes the metal foil according to any one of claims 1 to 13 or the metal-clad laminate according to claim 14.

16. A semiconductor material, characterized in that: The semiconductor material comprises the metal foil according to any one of claims 1 to 13.

17. A negative electrode material for a battery, characterized in that: The negative electrode material comprises the metal foil according to any one of claims 1 to 13.

18. A battery, characterized in that: The negative electrode material of the battery comprises the metal foil according to any one of claims 1 to 13.

Citation Information

Cited By