Conductive copper bar and preparation method and application thereof
By forming a dense oxide layer and a metal material layer on the conductive copper strip, combined with process parameter optimization and surface treatment, the problems of insufficient conductivity and poor corrosion resistance of traditional conductive copper strips are solved, and high conductivity and corrosion resistance are achieved. promote.
Patent Information
- Application Number
- CN202411122269.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-19
AI Technical Summary
Traditional conductive copper strips have insufficient conductivity and poor corrosion resistance, making it difficult to meet the needs of modern electronic equipment for high performance and high reliability.
Using a composite coating structure, including a dense oxide layer and a covered metal material layer, the surfaces such as smelting temperature, rolling down pressure rate, cooling speed, etc. are carried out by controlling the process parameters such as smelting, electrolysis, grinding, polishing, anodizing, etc. The treatment is combined with the precise control of nickel, silver and tin coatings to form a multi-layer protective structure.
It significantly improves the conductivity and corrosion resistance of the conductive copper strip, extends the service life, enhances the mechanical strength and welding performance, and ensures the stability and quality of the product.
Smart Images

Figure BDA0004995423280000111
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of conductive materials, and in particular to a conductive copper busbar and a preparation method and application thereof. Background Art
[0002] With the continuous development and popularization of electronic equipment, the demand for efficient conductive materials is also increasing. Conductive copper busbars, as an important conductive material, are widely used in power transmission, electronic appliances, communication equipment and other fields.
[0003] However, traditional conductive copper busbars have problems such as insufficient conductivity and poor corrosion resistance, which makes it difficult to meet the requirements of modern electronic equipment for high performance and high reliability of conductive materials.
[0004] Therefore, the present invention provides a conductive copper busbar and a preparation method and application thereof to solve the problems raised in the above background technology. Summary of the invention
[0005] The object of the present invention is to provide a conductive copper busbar having high mechanical strength and good conductive performance.
[0006] The invention also provides a method for preparing the conductive copper busbar.
[0007] The present invention also provides the application of the above conductive copper busbar
[0008] Specifically, in a first aspect of the present invention, there is provided a conductive copper busbar, wherein the raw material for preparing the conductive copper busbar comprises a copper plate having a copper content of 99% to 100%, and the surface of the copper plate has a conductive layer;
[0009] The structure of the conductive layer includes a dense oxide layer formed on the surface of the copper plate and a metal material layer covering the dense oxide layer.
[0010] According to one technical solution of the conductive copper busbar technical solution of the present invention, at least the following beneficial effects are achieved:
[0011] The dense oxide layer can effectively prevent oxidation and corrosion on the surface of the conductive copper busbar, prolong its service life and improve its corrosion resistance. The metal material layer covering the dense oxide layer improves the conductivity of the conductive copper busbar, making it perform better in electrical conduction.
[0012] As a further technical solution of the present invention, the metal material layer includes a nickel coating, a silver coating and a tin coating in sequence from the inside to the outside.
[0013] The present invention adopts a composite coating structure, each layer of coating has a specific function. The nickel coating of the bottom layer provides corrosion resistance and mechanical strength, the silver coating of the middle layer provides good conductivity, and the tin coating of the top layer provides weldability. The synergistic effect forms a multi-layer protection, which comprehensively improves the performance and stability of the conductive copper busbar.
[0014] In a second aspect of the present invention, a method for preparing a conductive copper busbar is provided, comprising the following steps: sequentially smelting, casting, cooling, rolling, surface treatment, molding and surface coating a copper material;
[0015] The smelting temperature is 1100°C-1200°C;
[0016] The rolling reduction rate is 11%-30%;
[0017] The final temperature of the rolling is 254°C-330°C;
[0018] The cooling rate is 170°C / min-210°C / min;
[0019] The final temperature of the cooling is 10°C-15°C.
[0020] According to one technical solution of the conductive copper busbar technical solution of the present invention, at least the following beneficial effects are achieved:
[0021] Too high a melting temperature will cause the copper material to oxidize, burn or volatilize excessively, affecting the purity and composition of the raw materials and causing the conductive properties of the copper busbar to decrease. Too low a melting temperature will cause the copper material to fail to melt completely, affecting the smooth progress of subsequent processes and causing unstable product quality or defects.
[0022] If the rolling reduction rate is too high, the crystal structure of the conductive copper busbar will be too dense, affecting the conductivity. If the rolling reduction rate is too low, the deformation capacity of the material will be insufficient, and the expected hardness and strength of the material will not be achieved, affecting the mechanical properties of the conductive copper busbar.
[0023] Too fast cooling speed will cause the grains of the conductive copper busbar to be too fine or the solidification speed to be too fast, which will affect the mechanical properties and organizational structure of the material, resulting in a decrease in the strength and toughness of the product. Too slow cooling speed will cause excessive tempering of the copper material or excessive residual stress, affecting the dimensional stability and processing performance of the conductive copper busbar, and causing deformation or deformation of the product.
[0024] As a further technical solution of the present invention, the surface treatment includes pickling, electrolysis, grinding, polishing, and anodizing;
[0025] The pickling temperature is 40°C-60°C;
[0026] The pickling time is 5min-15min;
[0027] The current density of the electrolysis is 10A / dm 2 -50A / dm 2 ;
[0028] The electrolysis time is 1 min-5 min.
[0029] If the pickling time is too long and the temperature is too high, it will cause excessive corrosion or excessive dissolution of the material, damage the surface quality of the conductive copper busbar, and reduce the corrosion resistance. If the pickling time is too short and the temperature is too low, the oxides and pollutants on the copper surface cannot be completely removed, affecting the subsequent coating adhesion and surface quality.
[0030] If the current density of electrolysis is too high or the time is too long, the thickness of the electrolytic coating will be uneven, and even defects such as excessive crystallization or pores will appear, which will affect the coating quality and performance of the conductive copper busbar. If the current density of electrolysis is too low or the time is too short, the electrolysis speed will be too slow, the coating thickness will be insufficient or the coating composition will be uneven, which will affect the density and adhesion of the coating.
[0031] As a further technical solution of the present invention, the current density of the anodization is 5A / dm 2 Up to 20A / dm 2 .
[0032] As a further technical solution of the present invention, the anodizing time is 12 min-28 min.
[0033] If the current density of anodizing is too high or the time is too long, the thickness of the anodizing coating will be too thick or the crystallization will be too large, which will affect the appearance and surface quality of the conductive copper busbar. If the current density of anodizing is too low or the time is too short, a uniform and dense oxide film cannot be formed, which will reduce the corrosion resistance and stability of the conductive copper busbar.
[0034] As a further technical solution of the present invention, the thickness of the nickel coating is 30um-50um.
[0035] Too thick a nickel coating will increase the cost and sometimes cause the coating to crack and fall off. Too thin a nickel coating may not effectively protect the surface of the conductive copper busbar, making it susceptible to oxidation and corrosion, reducing its corrosion resistance.
[0036] As a further technical solution of the present invention, the thickness of the silver coating is 5um-20um.
[0037] If the silver coating is too thick, it will increase the difficulty of welding, because welding needs to penetrate the coating and contact the copper substrate. Too thick a coating will increase the welding time and temperature and reduce the welding efficiency. If the silver coating is too thin, it may lead to insufficient conductivity and affect the overall conductivity of the conductive copper busbar.
[0038] As a further technical solution of the present invention, the thickness of the tin coating is 5um-15um.
[0039] Too thick a tin coating may increase the welding temperature and time, affecting production efficiency. Too thin a tin coating may result in a loose and unstable welding joint, affecting the welding performance and reliability of the conductive copper busbar. In addition, too thin a tin coating cannot effectively protect the surface of the conductive copper busbar, making it susceptible to oxidation, corrosion, etc., reducing corrosion resistance.
[0040] A third aspect of the present invention provides use of a conductive copper busbar in preparing a conductive material.
[0041] The conductive copper busbar provided by the invention has high mechanical strength and good conductivity and can be used for preparing conductive materials.
[0042] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects:
[0043] The present invention realizes accurate control of the preparation process of the conductive copper busbar by optimizing the process parameters such as the smelting temperature, the rolling reduction rate, the cooling rate and the final temperature, thereby ensuring the product quality and stability. At the same time, a variety of surface treatment methods such as pickling, electrolysis, grinding, polishing, and anodizing are adopted to comprehensively treat the surface of the conductive copper busbar, thereby ensuring the cleanliness, smoothness and corrosion resistance of the surface. In addition, the thickness of the nickel coating, the silver coating and the tin coating is accurately controlled in the present invention, thereby ensuring the uniformity and stability of the coating and improving the performance and stability of the conductive copper busbar. DETAILED DESCRIPTION
[0044] In order to understand the purpose, features and effects of the present invention; it is obvious that the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments, and other embodiments obtained by technicians in this field based on the embodiments of the present invention without paying creative work all belong to the scope of protection of the present invention.
[0045] In the description of the present invention, the description with reference to terms such as "one embodiment", "some embodiments", "illustrative embodiments", "example", "specific example", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention; in this specification, the schematic expressions of the above terms do not necessarily refer to the same embodiment or example; moreover, the specific features, structures, materials or characteristics described may be combined in an appropriate manner in any one or more embodiments or examples.
[0046] If no specific conditions are specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer; if no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0047] The specific embodiments of the present invention are described in detail below.
[0048] The conductivity test method is to use a conductivity tester to perform resistance test.
[0049] The tensile strength test method is (GB / T228.1 Metal material tensile test part 1: room temperature tensile test method).
[0050] The bending strength test method is (GB / T228.1 Metal material tensile test part 1: room temperature tensile test method).
[0051] The corrosion resistance test method is to expose the sample to a salt spray environment to simulate the corrosion conditions in the ocean or industrial atmosphere to evaluate the corrosion resistance of the coating.
[0052] The welding performance test method is welding tensile test.
[0053] Example 1
[0054] This embodiment is a conductive copper busbar, and the raw materials for preparing the conductive copper busbar are as follows:
[0055] Copper plate with a copper content of 99%, nickel, silver and tin.
[0056] The preparation method of the conductive copper busbar comprises the following steps:
[0057] S1. Put the copper material into a smelting furnace and control the temperature at 1100°C;
[0058] S2, casting the molten copper liquid, using a mold to form a copper plate with a predetermined shape and size;
[0059] S3, the copper plate is immediately cooled after casting, the cooling rate is controlled at 170℃ / min, and cooled to 10℃;
[0060] S4, the cooled copper plate is subjected to rolling treatment, the rolling reduction rate is controlled at 11%, and the final temperature is controlled at 254°C;
[0061] S5, pickling the rolled copper plate, the pickling temperature is controlled at 40°C, and the time is 5 minutes;
[0062] S6. The pickled copper plate is electrolyzed, and the electrolysis current density is controlled at 10A / dm 2 , time is 1min;
[0063] S7. After electrolysis, the copper plate is ground and polished to eliminate the tiny unevenness on the surface;
[0064] S8, anodize the copper plate, and control the current density at 5A / dm 2 , time is 12min;
[0065] S9, firstly plating a nickel coating on the surface of the treated copper plate, and the thickness of the nickel coating is controlled to be 30um;
[0066] S10, after the nickel coating is completed, a silver coating is plated on the surface, and the thickness of the silver coating is controlled to be 5um;
[0067] S11. A tin coating is plated on the surface of the silver coating, and the thickness of the tin coating is controlled to be 5 um.
[0068] Example 2
[0069] This embodiment is a conductive copper busbar, and the raw materials for preparing the conductive copper busbar are as follows:
[0070] Copper plate with a copper content of 99.9%, nickel, silver and tin.
[0071] The difference between the conductive copper busbar preparation method of this embodiment and that of embodiment 1 lies in the different parameters selected, which are as follows:
[0072] Melting temperature: 1150℃;
[0073] Cooling rate: 180℃ / min;
[0074] Final cooling temperature: 12°C;
[0075] Rolling reduction rate: 20%;
[0076] Final rolling temperature: 300℃;
[0077] Pickling temperature: 50℃;
[0078] Pickling time: 10min;
[0079] Electrolysis current density: 30A / dm 2 ;
[0080] Electrolysis time: 3min;
[0081] Anodic oxidation current density: 10A / dm 2 ;
[0082] Anodizing time: 20min;
[0083] Nickel coating thickness: 40μm;
[0084] Silver coating thickness: 10μm;
[0085] Tin coating thickness: 10μm.
[0086] Example 3
[0087] This embodiment is a conductive copper busbar, and the raw materials for preparing the conductive copper busbar are as follows:
[0088] Copper plate with a copper content of 99.95%, nickel, silver and tin.
[0089] The difference between the conductive copper busbar preparation method of this embodiment and that of embodiment 1 lies in the different parameters selected, which are as follows:
[0090] Melting temperature: 1180℃;
[0091] Cooling rate: 200℃ / min;
[0092] Final cooling temperature: 13°C;
[0093] Rolling reduction rate: 25%;
[0094] Final rolling temperature: 320℃;
[0095] Pickling temperature: 55°C;
[0096] Pickling time: 8min;
[0097] Electrolysis current density: 40A / dm 2 ;
[0098] Electrolysis time: 4min;
[0099] Anodic oxidation current density: 15A / dm 2 ;
[0100] Anodizing time: 25min;
[0101] Nickel coating thickness: 35μm;
[0102] Silver coating thickness: 15μm;
[0103] Tin coating thickness: 12μm.
[0104] Example 4
[0105] This embodiment is a conductive copper busbar, and the raw materials for preparing the conductive copper busbar are as follows:
[0106] Copper plate with a copper content of 99.98%, nickel, silver and tin.
[0107] The difference between the conductive copper busbar preparation method of this embodiment and that of embodiment 1 lies in the different parameters selected, which are as follows:
[0108] Melting temperature: 1120℃;
[0109] Cooling rate: 190℃ / min;
[0110] Final cooling temperature: 14°C;
[0111] Rolling reduction rate: 15%;
[0112] Final rolling temperature: 275℃;
[0113] Pickling temperature: 45°C;
[0114] Pickling time: 12min;
[0115] Electrolysis current density: 20A / dm 2 ;
[0116] Electrolysis time: 2min;
[0117] Anodic oxidation current density: 8A / dm 2 ;
[0118] Anodizing time: 18min;
[0119] Nickel coating thickness: 45μm;
[0120] Silver coating thickness: 12μm;
[0121] Tin coating thickness: 8μm.
[0122] Comparative Example 1
[0123] This comparative example is a conductive copper busbar, and the raw materials for preparing the conductive copper busbar are as follows:
[0124] Copper plate with a copper content of 99.5%, nickel, silver and tin.
[0125] The difference between the preparation method of the conductive copper busbar in this comparative example and that in Example 1 lies in the different parameters selected, which are as follows:
[0126] Melting temperature: 1050℃;
[0127] Cooling rate: 100℃ / min;
[0128] Final cooling temperature: 15°C;
[0129] Rolling reduction rate: 5%;
[0130] Final rolling temperature: 200℃;
[0131] Pickling temperature: 35℃;
[0132] Pickling time: 5min;
[0133] Electrolysis current density: 5A / dm2 ;
[0134] Electrolysis time: 1min;
[0135] Anodic oxidation current density: 2A / dm 2 ;
[0136] Anodizing time: 5min;
[0137] Nickel coating thickness: 20μm;
[0138] Silver coating thickness: 2μm;
[0139] Tin coating thickness: 2μm.
[0140] Comparative Example 2
[0141] This comparative example is a conductive copper busbar, and the raw materials for preparing the conductive copper busbar are as follows:
[0142] Copper plate with a copper content of 99.9%, nickel, silver and tin.
[0143] The difference between the preparation method of the conductive copper busbar in this comparative example and that in Example 1 lies in the different parameters selected, which are as follows:
[0144] Melting temperature: 1250℃;
[0145] Cooling rate: 500℃ / min;
[0146] Final cooling temperature: 5°C;
[0147] Rolling reduction rate: 50%;
[0148] Final rolling temperature: 350℃;
[0149] Pickling temperature: 65℃;
[0150] Pickling time: 20min;
[0151] Electrolysis current density: 60A / dm 2 ;
[0152] Electrolysis time: 10min;
[0153] Anodic oxidation current density: 25A / dm 2 ;
[0154] Anodizing time: 35min;
[0155] Nickel coating thickness: 60μm;
[0156] Silver coating thickness: 25μm;
[0157] Tin coating thickness: 20μm.
[0158] The test results of the conductive copper busbars prepared in Examples 1-4 of the present invention and Comparative Examples 1-2 are shown in Table 1.
[0159] illustrate:
[0160] Conductivity reflects the resistivity of a material, the lower the value, the better the conductivity.
[0161] The salt spray test corrosion area indicates the percentage of the area on the sample surface that is corroded during the salt spray test. The lower the value, the better the corrosion resistance.
[0162] Coating adhesion is an assessment of the adhesion between the coating and the copper plate, which is divided into strong, good, poor and poor grades.
[0163] The thickness of nickel coating, silver coating and tin coating is the thickness of the coating, and the unit is micrometer (μm).
[0164] The actual performance of each embodiment and comparative example is recorded in the notes.
[0165] Table 1 Test results of the conductive copper busbars prepared in Examples 1-4 of the present invention and Comparative Examples 1-2
[0166]
[0167] In summary, the present invention optimizes the process parameters such as melting temperature, rolling reduction rate, cooling rate and final temperature, and adopts a variety of surface treatment methods such as pickling, electrolysis, grinding, polishing, anodizing, etc. to comprehensively treat the surface of the conductive copper busbar, thereby ensuring the cleanliness, smoothness and corrosion resistance of the surface. In addition, the thickness of the nickel coating, silver coating and tin coating is precisely controlled in the present invention, thereby ensuring the uniformity and stability of the coating and improving the performance and stability of the conductive copper busbar.
[0168] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A conductive copper busbar, characterized in that: The raw material for preparing the conductive copper busbar includes a copper plate with a copper content of 99%-100%, and the surface of the copper plate has a conductive layer; The structure of the conductive layer includes a dense oxide layer formed on the surface of the copper plate and a metal material layer covering the dense oxide layer.
2. A conductive copper busbar according to claim 1, characterized in that: The metal material layer includes a nickel coating, a silver coating and a tin coating in sequence from the inside to the outside.
3. A method for preparing a conductive copper busbar as claimed in any one of claims 1 to 2, characterized in that: The method comprises the following steps: sequentially melting, casting, cooling, rolling, surface treatment, forming and surface coating the copper material; The smelting temperature is 1100°C-1200°C; The rolling reduction rate is 11%-30%; The final temperature of the rolling is 254°C-330°C; The cooling rate is 170°C / min-210°C / min; The final temperature of the cooling is 10°C-15°C.
4. The preparation method according to claim 3, characterized in that: The surface treatment includes pickling, electrolysis, grinding, polishing and anodizing; The pickling temperature is 40°C-60°C; The pickling time is 5min-15min; The current density of the electrolysis is 10A / dm 2 -50A / dm 2 ; The electrolysis time is 1 min-5 min.
5. The preparation method according to claim 4, characterized in that: The current density of the anodization is 5A / dm 2 Up to 20A / dm 2 .
6. The preparation method according to claim 4, characterized in that: The anodizing time is 12 min-28 min.
7. The preparation method according to claim 3, characterized in that: The thickness of the nickel coating is 30um-50um.
8. The preparation method according to claim 3, characterized in that: The thickness of the silver coating is 5um-20um.
9. The preparation method according to claim 3, characterized in that: The thickness of the tin coating is 5um-15um.
10. Use of the conductive copper busbar according to any one of claims 1 to 9 in preparing conductive materials.