Negative active slurry, negative plate and preparation method of negative plate
By using a particle size matching technique combining styrene-butadiene rubber and graphite to prepare the negative electrode sheet, the side reaction problem of lithium-ion battery negative electrode sheets under high temperature environment was solved, and a negative electrode sheet with high bonding strength and low active sites was achieved, thereby improving the high temperature cycle performance and stability of the battery.
Patent Information
- Application Number
- CN202411058321.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
Existing technologies have failed to effectively address the side reaction problem of lithium-ion battery anode sheets under high-temperature conditions, leading to increased irreversible loss of active lithium and affecting the high-temperature cycle performance and stability of the battery cell.
A negative electrode sheet is prepared using styrene-butadiene rubber (SBR) and graphite as raw materials, combined with particle size matching technology. The graphite particle size Df meets the requirements of 1000nm≤Df≤1600nm, the styrene-butadiene rubber particle size Ds meets the requirements of 50nm≤Ds≤100nm, and Df/Ds≤20, forming a negative electrode sheet with high bonding strength and low rebound.
It improves the adhesion of the negative electrode throughout its entire life cycle, reduces the contact between the active material and the electrolyte, reduces side reactions, and enhances high-temperature cycling performance and storage life.
Smart Images

Figure BDA0004977064660000141 
Figure BDA0004977064660000151
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion battery materials and discloses a negative electrode active slurry, a negative electrode sheet and a preparation method thereof. Background Art
[0002] The electrical conversion efficiency of energy storage equipment is significantly affected by the power consumption of the auxiliary system. Taking lithium iron phosphate energy storage equipment as an example, the power utilization rate of its auxiliary system exceeds 10%, among which the energy consumption of the air conditioning system is particularly significant. Faced with the limitations of the air conditioning cooling system, the traditional solutions are air cooling and liquid cooling, but both face problems such as high cost, insufficient technical stability, and excessive energy consumption. Therefore, it is urgent to develop "high-temperature batteries" that can adapt to "no air conditioning" and still maintain long life and safe and stable operation in high temperature environments. In high temperature environments, the side reactions inside the battery cells are intensified, especially the interface between the negative electrode and the electrolyte will continuously consume active lithium to form an SEI film, thereby increasing the irreversible loss of active lithium. Therefore, how to improve the surface activity of the negative electrode sheet and reduce side reactions is particularly important for the development of high-temperature batteries.
[0003] At present, the research direction for the development of long-cycle negative electrode sheets is mainly focused on negative electrode graphite and binders. For example, CN 116387456 A discloses a long-cycle negative electrode active slurry, a negative electrode sheet and its preparation method, and a cylindrical battery. The negative electrode active slurry adopts low-expansion multilayer artificial graphite, which makes the lithium ion deintercalation resistance less during the charging and discharging process, has good dynamics, and is conducive to reducing the repeated rupture and repair of the SEI film caused by expansion during the cycle. CN 117038867A discloses a long-life multilayer coated thick electrode negative electrode for lithium ion batteries. The negative electrode sheet is coated with negative electrode active slurry at the bottom layer. The emulsion-type liquid retaining agent polyacrylate is added during the preparation. It can absorb a high electrolyte and convert it into electrolyte. It can convert electrolyte with a mass of dozens of times its own into a colloid electrolyte, lock the electrolyte, and in the subsequent cycle of the battery core, due to the consumption of the electrolyte, a concentration difference will be formed, causing the electrolyte in the colloid to precipitate.
[0004] The above studies are limited to the development of long-cycle negative electrode sheets, and there are no relevant reports on the development of high-temperature battery negative electrode sheets. The development of the long-cycle negative electrode sheets in the above patent application uses low-expansion isotropic graphite and adapts the binder to meet the battery BOL and EOL state dynamics. The high-temperature battery does not have high requirements for dynamics, and it is necessary to focus on reducing the active sites of the negative electrode sheet to reduce side reactions. In addition, the above patent application does not consider the impact of the interaction between the binder and the graphite itself on the electrochemical performance of the battery cell. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention provides a negative electrode active slurry, a negative electrode sheet and a preparation method and application thereof. The present invention uses styrene-butadiene rubber (SBR) and graphite as raw materials and cooperates with particle size adaptation technology to prepare the negative electrode sheet. The negative electrode sheet thus prepared has technical advantages such as high bonding strength, low rebound, and low active sites, which effectively improves the bonding strength of the negative electrode sheet throughout its life cycle, and improves high temperature cycle performance and storage life.
[0006] Specifically, the first aspect of the present invention provides a negative electrode active slurry, which includes graphite, styrene-butadiene rubber, a conductive agent, a dispersant and a solvent, wherein the particle size D50 of the graphite is recorded as Df, the particle size D50 of the styrene-butadiene rubber is recorded as Ds, and the Df and Ds satisfy the following conditions:
[0007] 50nm≤Ds≤100nm;
[0008] 1000nm≤Df≤1600nm;
[0009] 15≤Df / Ds≤20.
[0010] In one or more embodiments, the graphite is selected from long-cycle graphite, and the long-cycle graphite is preferably selected from one or more of petroleum coke-derived graphite, asphalt coke-derived graphite, and needle coke-derived graphite.
[0011] In one or more embodiments, the mass ratio of the added amount of the graphite to the solid matter in the negative electrode active slurry is (94.5-97.0):100.
[0012] In one or more embodiments, the mass ratio of the added amount of the styrene-butadiene rubber to the solid matter in the negative electrode active slurry is (1.0-2.5):100.
[0013] In one or more embodiments, the conductive agent is selected from one or more of conductive carbon black, carbon fiber, acetylene black, Ketjen black, graphene and carbon nanotubes.
[0014] In one or more embodiments, the mass ratio of the conductive agent to the solid matter in the negative electrode active slurry is (0.5-2.0):100.
[0015] In one or more embodiments, the dispersant is selected from carboxymethyl cellulose and / or a Byk dispersant.
[0016] In one or more embodiments, the mass ratio of the dispersant to the solid matter in the negative electrode active slurry is (0.5-2.0):100.
[0017] In one or more embodiments, the solvent is water.
[0018] In one or more embodiments, the viscosity of the negative electrode active slurry is 3000-8000 mPa·s.
[0019] The second aspect of the present invention provides a method for preparing a negative electrode active slurry as described in any embodiment of the present invention, the method comprising: mixing graphite, the conductive agent, the dispersant and the solvent, and then adding styrene-butadiene rubber and optionally a solvent, and mixing them evenly.
[0020] The third aspect of the present invention provides a negative electrode sheet, comprising a negative electrode current collector and a negative electrode material layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode material layer comprises graphite, styrene-butadiene rubber, a conductive agent and a dispersant, wherein the particle size D50 of the graphite is recorded as Df, and the particle size D50 of the styrene-butadiene rubber is recorded as Ds, wherein Df and Ds satisfy the following conditions:
[0021] 50nm≤Ds≤100nm;
[0022] 1000nm≤Df≤1600nm;
[0023] 15≤Df / Ds≤20.
[0024] In one or more embodiments, the graphite is selected from long-cycle graphite, and the long-cycle graphite is preferably selected from one or more of petroleum coke-derived graphite, asphalt coke-derived graphite, and needle coke-derived graphite.
[0025] In one or more embodiments, the mass fraction of the graphite in the negative electrode material layer is 94.5%-97%.
[0026] In one or more embodiments, the mass fraction of the styrene-butadiene rubber in the negative electrode material layer is 1.0%-2.5%.
[0027] In one or more embodiments, the conductive agent is selected from one or more of conductive carbon black, carbon fiber, acetylene black, Ketjen black, graphene and carbon nanotubes.
[0028] In one or more embodiments, the conductive agent accounts for 0.5%-2.0% by mass of the negative electrode material layer.
[0029] In one or more embodiments, the dispersant is selected from carboxymethyl cellulose and / or a Byk dispersant.
[0030] In one or more embodiments, the mass fraction of the dispersant in the negative electrode material layer is 0.5%-2.0%.
[0031] A fourth aspect of the present invention provides a method for preparing a negative electrode sheet as described in any embodiment of the present invention, the method comprising coating the negative electrode active slurry described in any embodiment of the present invention onto the negative electrode current collector, and then drying and pressing to obtain the negative electrode sheet.
[0032] A fifth aspect of the present invention provides a lithium ion battery, comprising the negative electrode sheet as described in any embodiment of the present invention.
[0033] A sixth aspect of the present invention provides the use of the negative electrode active slurry or negative electrode sheet as described in any embodiment of the present invention in improving the high temperature cycle performance of a battery.
[0034] A seventh aspect of the present invention provides the use of the negative electrode active slurry or negative electrode sheet as described in any embodiment herein in the preparation of a battery with improved high temperature cycle performance.
[0035] The eighth aspect of the present invention provides the use of graphite and styrene-butadiene rubber in the preparation of negative electrode active materials or negative electrode sheets that can improve the high-temperature cycle performance of batteries, the use of graphite and styrene-butadiene rubber in improving the high-temperature cycle performance of batteries, and the use of graphite and styrene-butadiene rubber in the preparation of batteries with improved high-temperature cycle performance; wherein the particle size D50 of the graphite is denoted as Df, the particle size D50 of the styrene-butadiene rubber is denoted as Ds, and Df and Ds satisfy the following conditions: 50nm≤Ds≤100nm; 1000nm≤Df≤1600nm; 15≤Df / Ds≤20. DETAILED DESCRIPTION
[0036] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in this article. Unless otherwise specified, all technical and scientific terms used in this article are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definitions in this article shall prevail.
[0037] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0038] Herein, “comprising”, “including”, “containing” and similar terms encompass the meanings of “consisting essentially of” and “consisting of”. For example, when “A comprises B and C” is disclosed herein, “A consists essentially of B and C” and “A consists of B and C” should be deemed to be disclosed herein.
[0039] In this article, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are only for brevity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0040] In this document, unless otherwise specified, percentage refers to mass percentage and ratio refers to mass ratio.
[0041] Herein, when describing embodiments or examples, it should be understood that they are not used to limit the present invention to these embodiments or examples. On the contrary, all substitutes, improvements and equivalents of the methods and materials described in the present invention can be included in the scope limited by the claims.
[0042] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0043] The inventors of the present invention have found that, in order to address the problem of aggravated side reactions of lithium-ion batteries in high-temperature environments, the use of styrene-butadiene rubber (SBR) and graphite as raw materials and particle size adaptation technology to prepare negative electrode active slurry to obtain negative electrode sheets can effectively reduce the contact between active materials and electrolytes and reduce side reactions at the interface of negative electrode sheets; it has technical advantages such as high bonding strength, low rebound, and low active sites.
[0044] In the present invention, the particle size D50 of styrene butadiene rubber is recorded as Ds, and Ds satisfies 50nm≤Ds≤100nm, such as 60nm, 70nm, 75nm, 80nm, 90nm or its particle size is within the range formed by any two of the above values. The particle size D50 of the current mainstream styrene butadiene rubber is between 150nm-250nm, while the particle size D50 of the styrene butadiene rubber selected in the present invention is between 50nm-100nm. Styrene butadiene rubber plays the role of a binder. When the amount of styrene butadiene rubber added is the same, the small particle size determines that the contact points between styrene butadiene rubber and graphite particles increase, so it can have a higher bonding force. In addition, after the battery is filled with liquid, styrene butadiene rubber will swell on the graphite surface, and lithium ions need to bypass the styrene butadiene rubber site when embedded in graphite, that is, small-sized styrene butadiene rubber plays a point-like coating role on the graphite particles, which reduces the direct contact between the graphite particles and the electrolyte to a certain extent, thereby reducing side reactions.
[0045] In the present invention, the mass ratio of the added amount of styrene-butadiene rubber to the solid matter in the negative electrode active slurry is (1.0-2.5):100, for example, 1.5:100, 2.0:100, 2.2:100, 2.4:100 or within the range formed by any two of the aforementioned ratios.
[0046] In the present invention, the particle size D50 of graphite is recorded as Df, and Df satisfies 1000nm≤Df≤1600nm, such as 1100nm, 1200nm, 1300nm, 1400nm, 1500nm or within the range formed by any two of the above values. Graphite with a particle size within this particle size range has good processing performance while taking into account dynamics and high temperature performance.
[0047] In the present invention, the particle sizes of graphite and styrene-butadiene rubber satisfy 15≤Df / Ds≤20, for example, 16, 16.25, 17, 18, 19, 20 or within the range formed by any two of the aforementioned values.
[0048] In the present invention, the graphite may be selected from long-cycle graphite. Long-cycle graphite has the advantage of high chemical stability and also has good mechanical strength, and can maintain its structural integrity during high temperature cycles. In some embodiments, the long-cycle graphite is selected from one or more of petroleum coke-derived graphite, asphalt coke-derived graphite, and needle coke-derived graphite.
[0049] In the present invention, the mass ratio of the added amount of graphite to the solid matter in the negative electrode active slurry is (94.5-97.0):100, for example, 95:100, 95:100, 95.8:100, 96:100, 96.8:100 or within the range formed by any two of the foregoing ratios.
[0050] In the present invention, the negative electrode active slurry includes a conductive agent. The conductive agent is used to improve the conductivity of the negative electrode sheet. The type of the conductive agent is not particularly limited, and a conventional conductive agent in the art can be used, for example, one or more selected from conductive carbon black, carbon fiber, acetylene black, Ketjen black, graphene and carbon nanotubes. In some embodiments, the conductive agent is conductive carbon black. The mass ratio of the added amount of the conductive agent to the solid matter in the negative electrode active slurry can be (0.5-2.0):100, for example, 0.8:100, 1.0:100, 1.2:100, 1.5:100, 1.8:100 or within the range composed of any two of the aforementioned ratios.
[0051] In the present invention, the negative electrode active slurry includes a dispersant. The type of the dispersant is not particularly limited, and a conventional dispersant in the art may be used, such as carboxymethyl cellulose and / or a Bick dispersant. The mass ratio of the dispersant to the solid matter in the negative electrode active slurry may be (0.5-2.0):100, such as 0.8:100, 1.0:100, 1.2:100, 1.5:100, 1.8:100, or within the range of any two of the above ratios.
[0052] The negative electrode active slurry of the present invention can be obtained by mixing graphite, a conductive agent, a dispersant and a solvent. In some preferred embodiments, the negative electrode active slurry of the present invention is prepared by the following method: firstly, graphite, a conductive agent, a dispersant and a solvent are mixed, and then styrene-butadiene rubber and optionally a solvent are added. The viscosity of the negative electrode active slurry is preferably 3000-8000mPa·s, for example, 4000mPa·s, 5000mPa·s, 6000mPa·s, 7000mPa·s or within the range formed by any two of the aforementioned values. When the viscosity of the negative electrode active slurry is not within this range, it can be adjusted by adding a solvent. The type of solvent is not particularly limited, and conventional solvent types in the art can be used, such as water, preferably deionized water.
[0053] Negative plate
[0054] The present invention provides a negative electrode sheet, which includes a negative electrode current collector and a negative electrode material layer arranged on at least one surface of the negative electrode current collector, wherein the negative electrode material layer includes graphite, styrene-butadiene rubber, a conductive agent and a dispersant as described in any embodiment of the present invention.
[0055] The negative electrode current collector may be a copper foil, a titanium foil, a nickel foil, an iron foil, a zinc foil, etc. As the shape of the negative electrode current collector, for example, a foil shape, a plate shape, a mesh shape, etc. may be mentioned.
[0056] The mass fraction of graphite in the negative electrode material layer can be 94.5%-97%, such as 95%, 95.7%, 96%, 96.4%, 96.8%. The mass fraction of styrene-butadiene rubber can be 1.0%-2.5%, such as 1.5%, 2%. The mass fraction of the dispersant can be 0.5%-2.0%, such as 1%, 1.2%, 1.5%, 2%, or within the range formed by any two of the aforementioned values. The mass fraction of the conductive agent can be 0.5%-2.0%, such as 1%, 1.2%, 1.5%, 2%, or within the range formed by any two of the aforementioned values.
[0057] The present invention provides a method for preparing a negative electrode sheet, which comprises the following steps: coating the negative electrode active slurry as described in any embodiment of the present invention on one or two surfaces of the negative electrode collector, and then drying, pressing and cutting to obtain a negative electrode sheet.
[0058] The drying, sheeting and slitting are not particularly limited and can be carried out in a conventional manner in the art. The purpose of drying is to remove the solvent. In some embodiments, drying is carried out by drying. In some embodiments, sheeting and slitting are carried out by roller separation.
[0059] Lithium-ion battery
[0060] The present invention provides an electrochemical device, such as a lithium ion battery, comprising the negative electrode sheet of the present invention. The lithium ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the separator is disposed between the positive electrode sheet and the negative electrode sheet. The lithium ion battery of the present invention is characterized in that it comprises the negative electrode sheet of the present invention. The negative electrode sheet of the present invention is applicable to various types of lithium ion batteries.
[0061] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer (also called a positive electrode material layer) disposed on the positive electrode current collector. The positive electrode current collector can be aluminum foil, titanium foil, nickel foil, iron foil, zinc foil, etc. The positive electrode active material layer includes a positive electrode active material (also called a positive electrode material). The positive electrode active material may include a compound that can reversibly embed and deintercalate lithium ions. The positive electrode active material may be selected from a composite oxide containing lithium and at least one selected from cobalt, manganese, nickel and iron, preferably a lithium-containing composite oxide. The lithium-containing composite oxide is preferably LiM x O y and LiM x PO4, wherein M is a combination of one or more transition metals, 0<x≤3, 0<y≤4. Examples of positive electrode active materials include lithium cobalt oxide, lithium manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese aluminum oxide, lithium iron phosphate (LiFePO4), etc.
[0062] The positive electrode active material layer may also include one or more selected from a conductive agent, a dispersant and a binder. The conductive agent is used to improve the conductivity of the electrode. Examples of the conductive agent of the positive electrode include one or more of conductive carbon black, carbon fiber (CF), acetylene black, Ketjen black, graphene and carbon nanotubes. The binder of the positive electrode improves the bonding performance between the positive electrode active material particles and between the positive electrode active material particles and the current collector. Examples of the binder of the positive electrode include at least one of fluorine-containing resin, polypropylene resin, fiber-type binder, rubber-type binder and polyimide-type binder. Examples of the dispersant of the positive electrode include one or more of polyetherimide, polyvinyl pyrrolidone and polyvinyl butyral resin. In some embodiments, the conductive agent in the positive electrode active material layer is conductive carbon black, the binder is polyvinylidene fluoride (PVDF), and the dispersant is polyetherimide.
[0063] The content ratio of each component in the positive electrode active material layer can be conventional. The mass fraction of the positive electrode active material in the positive electrode active material layer can be 90%-97%, for example, 91%, 93%, 93.5%, 94%, 94.7%, 95%, 95.2%, 96%, 96.8%, 97% or within the range composed of any two of the aforementioned values. The mass fraction of the conductive agent can be 0.5%-2%, for example, 1%, 1.1%, 1.5%, 1.8%, 2% or within the range composed of any two of the aforementioned values. The mass fraction of the binder can be 1.0%-2.5%, for example, 1%, 1.5%, 1.6%, 2% or within the range composed of any two of the aforementioned values. The mass fraction of the dispersant can be 0.08%-0.4%, for example, 0.08%, 0.1%, 0.2% or within the range composed of any two of the aforementioned values.
[0064] The positive electrode active material layer is obtained by coating a positive electrode slurry containing various components of the positive electrode active material layer and a solvent onto a positive electrode current collector, followed by drying and pressing. The solvent of the positive electrode slurry may be N-methylpyrrolidone (NMP).
[0065] The material of the separator can be one or more of polyethylene and polypropylene. In some preferred embodiments, the separator material is selected from PP (polypropylene), rubber-coated PP, PE (polyethylene) and rubber-coated PE.
[0066] The electrolyte solution includes a nonaqueous organic solvent and an electrolyte salt.
[0067] The non-aqueous organic solvent suitable for the electrolyte of the present invention can be selected from one or more of carbonate solvents, ether-based solvents, ketone-based solvents and other aprotic solvents. Examples of non-aqueous organic solvents include, but are not limited to, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, triester phosphate, trimethoxymethane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate and ethyl propionate, etc. In some preferred embodiments, the non-aqueous organic solvent includes ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC). Preferably, the mass ratio of propylene carbonate:ethyl methyl carbonate:diethyl carbonate is preferably (0.5-2):(0.5-2):(0.5-2), for example, 1:1:1.
[0068] The electrolyte salt may include or be selected from a lithium salt. A lithium salt is a material that is easily soluble in a non-aqueous organic solvent. The lithium salt may be selected from one or more of an organic lithium salt and an inorganic lithium salt. Examples of lithium salts include, but are not limited to, LiCl, LiBr, LiI, LiClO4, LiBF4, LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, (CF3SO2)2NLi. In some embodiments, the concentration of the electrolyte salt in the electrolyte is 0.5-2 mol / L, for example 0.8 mol / L, 1 mol / L, 1.5 mol / L.
[0069] The electrolyte of the present invention may optionally contain various additives that can be used in the electrolyte, such as desolvating agents, cosolvents, film-forming additives, etc. The mass fraction of each type of additive in the electrolyte may be 0.1%-10%, such as 1%, 2%, 3%, 4%, 5%, or within the range formed by any two of the aforementioned values.
[0070] The electrolyte suitable for the present invention may be a commonly used commercially available electrolyte.
[0071] The positive electrode sheet, the negative electrode sheet and the separator are stacked or wound according to the design requirements, and then packaged in a shell, and then dried, injected (electrolyte is injected), sealed, formed, aged, and divided to obtain an electrochemical device, such as a lithium ion battery. The form of the lithium ion battery of the present invention is not particularly limited, and can be a cylindrical lithium ion battery, a soft-pack lithium ion battery or an aluminum shell lithium ion battery.
[0072] Beneficial effects achieved by the present invention:
[0073] (1) The present invention is simple to prepare, has low cost, and is easy to process and mass produce on a large scale;
[0074] (2) The present invention can effectively improve the bonding strength of the negative electrode sheet over its entire life cycle, reduce the risk of coating shedding, and improve the stability of the electrode sheet;
[0075] (3) The present invention realizes a low rebound negative electrode sheet;
[0076] (4) The present invention can effectively reduce the contact between active materials and electrolytes, and reduce the negative electrode interface side reactions;
[0077] (5) The present invention fully integrates the synergistic effect of the negative electrode particles and the binder, and the negative electrode sheet has an ultra-long high-temperature cycle and storage life.
[0078] The present invention will be described below in the form of specific examples. It should be understood that these examples are merely illustrative and are not intended to limit the scope of the present invention. The methods, reagents and materials used in the examples are, unless otherwise stated, conventional methods, reagents and materials in the art. The raw material compounds in the examples can all be purchased through commercial routes.
[0079] Example 1
[0080] Preparation of negative electrode active slurry
[0081] (1) Long-circulation graphite (petroleum coke-derived graphite) with a particle size D50 of 1000 nm, conductive carbon black (SP), and dispersant carboxymethyl cellulose (CMC) are mixed in deionized water. Then, styrene-butadiene rubber (SBR) with a D50 of 50 nm is added to adjust the slurry viscosity to 7000 mPa·s. The specific adjustment method is to increase the slurry viscosity to 7000 mPa·s by adding deionized water. Among them, the mass ratio of long-circulation graphite: SBR: SP: CMC is 95.8:2.0:1.0:1.2.
[0082] Preparation of negative electrode
[0083] (2) The negative electrode active slurry is coated on the negative electrode current collector copper foil, and then dried, rolled and die-cut to obtain a negative electrode sheet.
[0084] Example 2
[0085] (1) Long-circulation graphite (asphalt coke-derived graphite) with a particle size D50 of 1300 nm, conductive agent SP, and dispersant CMC are mixed in deionized water. SBR with a particle size D50 of 80 nm is then added to adjust the slurry viscosity to 6000 mPa·s. The specific adjustment method is to adjust the slurry viscosity to 6000 mPa·s by adding deionized water. Among them, the mass ratio of graphite: SBR: conductive agent SP: dispersant CMC is 95.0:2.0:1.5:1.5.
[0086] (2) The slurry is uniformly coated on the current collector copper foil, and then dried, rolled and die-cut to obtain a negative electrode sheet.
[0087] Example 3
[0088] (1) Long-circulation graphite (asphalt coke-derived graphite) with a particle size D50 of 1500 nm, conductive agent SP, and dispersant CMC are mixed in deionized water. SBR with a particle size D50 of 100 nm is then added to adjust the slurry viscosity to 4000 mPa·s. The specific adjustment method is to adjust the slurry viscosity to 4000 mPa·s by adding deionized water. Among them, the mass ratio of graphite: SBR: conductive agent SP: dispersant CMC is 96.0:2.0:1.0:1.0.
[0089] (2) The slurry is uniformly coated on the current collector copper foil, and then dried, rolled and die-cut to obtain a negative electrode sheet.
[0090] Example 4
[0091] (1) Long-circulation graphite (petroleum coke-derived graphite) with a particle size D50 of 1400 nm, conductive agent SP, and dispersant CMC are mixed in deionized water. Then SBR with a particle size D50 of 70 nm is added to adjust the slurry viscosity to 4000 mPa·s. The specific adjustment method is to increase the slurry viscosity to 7000 mPa·s by adding deionized water. Among them, according to the mass ratio, graphite: SBR: conductive agent SP: dispersant CMC = 96.0: 2.0: 1.0: 1.0.
[0092] (2) The slurry is uniformly coated on the current collector copper foil, and then dried, rolled and die-cut to obtain a negative electrode sheet.
[0093] Example 5
[0094] (1) Long-circulation graphite (needle coke-derived graphite) with a particle size D50 of 1200 nm, conductive agent SP, and dispersant CMC are mixed in deionized water. SBR with a particle size D50 of 75 nm is then added to adjust the slurry viscosity to 4000 mPa·s. The specific adjustment method is to adjust the slurry viscosity to 4000 mPa·s by adding deionized water. Among them, the mass ratio of graphite: SBR: conductive agent SP: dispersant CMC is 96.0:2.0:1.0:1.0.
[0095] (2) The slurry is uniformly coated on the current collector copper foil, and then dried, rolled and die-cut to obtain a negative electrode sheet.
[0096] Comparative Example 1
[0097] The only difference between this comparative example and Example 1 is that the particle size D50 of the SBR used is 100 nm. Except for the above differences, the materials, formula ratios and preparation operations used in this comparative example are strictly consistent with those in Example 1.
[0098] Comparative Example 2
[0099] The only difference between this comparative example and Example 2 is that the particle size D50 of the long-circulation graphite used is 1700 nm. Except for the above difference, the materials, formula ratios and preparation operations used in this comparative example are strictly consistent with those in Example 2.
[0100] Comparative Example 3
[0101] The only difference between this comparative example and Example 3 is that the particle size D50 of the SBR used is 107 nm. Except for the above differences, the materials, formula ratios and preparation operations used in this comparative example are strictly consistent with those in Example 3.
[0102] Comparative Example 4
[0103] The only difference between this comparative example and Example 4 is that the binder used is styrene acrylic emulsion (PAR). Except for the above differences, the materials, formula ratios and preparation operations used in this comparative example are strictly consistent with those in Example 1.
[0104] Test Example 1
[0105] The negative electrode sheets prepared in Examples 1-5 and Comparative Examples 1-4 were subjected to a peel strength test, and the specific steps of the peel strength test were as follows:
[0106] 1. Cutting the pole piece
[0107] Take the positive / negative electrode sheets after rolling and use a customized die cutter to cut the electrode sheets to a length of 400mm and a width of 40mm.
[0108] 2. Paste and fix the electrode Prepare a flat thin steel plate with a length of about 250mm and a width of about 50mm. Paste a double-sided tape in the center of the steel plate, making sure that the length of the double-sided tape is greater than the test length of the sample and is the same width as the electrode. Smooth the double-sided tape to make it fit tightly in the center of the steel plate. Uncover the covering paper of the double-sided tape and paste the electrode on the tape. Make sure that the electrode and the tape are completely matched and fit together to ensure that the width is consistent when testing the peel force. Otherwise, the test results may be inaccurate, and the peeling curve may have jump points or waves.
[0109] 3. Installation test
[0110] Prepare a tensile testing machine and two clamps. Insert the steel plate with the fixed pole piece glued into the lower clamp and fix it vertically. Insert the pole piece without glue into the upper clamp and fix it at 180° with the pole piece of the lower clamp.
[0111] Calibrate and reset, set the test width, peel length 120mm, peel speed 300mm / min. Start the test, get the peel strength curve and average value. When processing the data, delete the two sections at the beginning and end of the test to get the standard curve.
[0112] The average values of the peel strengths of the negative electrode sheets of Examples 1-5 and Comparative Examples 1-4 are shown in Table 1.
[0113] Test Example 2
[0114] The negative electrode sheets prepared in Examples 1-5 and Comparative Examples 1-4 were used as negative electrode sheets for lithium ion batteries to prepare lithium ion batteries and perform battery performance tests:
[0115] (1) Preparation of positive electrode
[0116] The positive electrode slurry was prepared as follows: lithium iron phosphate active material, conductive agent carbon black, binder PVDF: dispersant were added into a vacuum mixer at a mass ratio of 96.8:1.1:2:0.1 for mixing, and then solvent NMP was added into the mixed slurry, and the mixed slurry was stirred into a uniform state under the action of the vacuum mixer, thereby obtaining the positive electrode slurry of this embodiment.
[0117] The positive electrode slurry is evenly coated on the two surfaces of the positive electrode current collector aluminum foil, and dried in an oven to obtain a positive electrode sheet semi-finished product, which is then hot pressed and cut to obtain the positive electrode sheet to be assembled.
[0118] (2) Preparation of electrolyte
[0119] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of EC:EMC:DEC=1:1:1 to obtain an organic solvent, and then fully dried lithium salt LiPF6 is dissolved in the above organic solvent to prepare an electrolyte with a concentration of 1 mol / L.
[0120] (3) Selection of isolation membrane
[0121] In this embodiment, a 9umPP+2umPCS (polymer composite membrane) membrane is selected as the isolation membrane of the lithium-ion battery.
[0122] (4) Assembly of lithium-ion batteries
[0123] The positive electrode sheet to be assembled, the isolation film, and the negative electrode sheet to be assembled are stacked in sequence, so that the isolation film is located between the positive and negative electrode sheets to play an isolating role, and a bare battery cell is obtained; the bare battery cell is placed in a battery casing, and after drying, an electrolyte is injected, and a lithium-ion battery is obtained through vacuum packaging, standing, forming, shaping and other processes.
[0124] (5) Battery performance test:
[0125] 1) Place the lithium-ion battery under test in a 45°C constant temperature box for 2 hours;
[0126] 2) Charge to 3.65V at 0.5P constant power and let stand for 30 minutes;
[0127] 3) Discharge at a constant power of 0.5P to 2.50V, let stand for 30min, and record the discharge capacity as the initial capacity C1;
[0128] 4) 2-3 step cycle until the capacity and energy fade to 70% or the cycle reaches 13000 cycles;
[0129] 5) Charge to 3.65V at 0.5P constant power and let stand for 30 minutes;
[0130] 3) Discharge at a constant power of 0.5P to 2.50V, let stand for 30min, and record the discharge capacity as the initial capacity C2;
[0131] According to the formula C2 / C1*100%, the 45°C / 0.5P cycle capacity retention rate is obtained.
[0132] Table 1 shows the performance test results of the negative electrode sheets prepared in Examples 1-5 and Comparative Examples 1-4 and the corresponding batteries.
[0133] The particle sizes of graphite and SBR in Examples 1-5 and Comparative Examples 1-4 were all tested using a Mastersizer 3000 particle size analyzer.
[0134] Table 1. Physical and chemical properties of materials and corresponding battery performance
[0135]
[0136]
[0137] Among the test objects, the negative electrode sheets prepared in Examples 1-5 meet the characteristics of 15≤Df / Ds≤20. Combined with the characteristics of the electrode sheets and the high-temperature cycle test results in the table, it can be seen that the peeling strength of the negative electrode sheets that meet the defined characteristics is all>10.0N / m, and the capacity retention rate of the prepared battery cells after 1000 cycles at 45℃@0.5P is ≥95.9%. The negative electrode sheet prepared in Comparative Example 1 belongs to the case of Df / Ds>20. Combined with the data in Table 1, it can be seen that the peeling strength of the negative electrode sheet in Comparative Example 1 is <8.0N / m, and the capacity retention rate is only 93.0%. This is mainly because the graphite particle size in Comparative Example 1 is relatively small, the number of graphite particles and the specific surface area are relatively large, and the SBR with a relatively large particle size of 100nm is selected, which has fewer corresponding coating sites, and the electrode peeling strength is small, which means that the bonding strength is low, resulting in poor stability of the electrode sheet, and a large contact area with the electrolyte during the cycle, and more side reactions in a high-temperature environment. The graphite particle size used in Comparative Example 2 does not meet the 1000nm≤Df≤1600nm, and the corresponding pole piece peeling strength meets the ≥8.0N / m standard, but the high temperature cycle capacity retention rate is poor, mainly due to the poor dynamics of large-particle graphite. As the cycle proceeds, the negative pole piece dynamics decreases, and the later positive and negative pole dynamics do not match, resulting in capacity decay. The SBR particle size used in Comparative Example 3 is 107nm, which does not meet the 50nm≤Ds≤100nm, and the corresponding pole piece peeling strength does not meet the ≥8.0N / m standard, mainly due to the small number of large-particle SBR points, and the later stability of the pole piece is slightly poor, resulting in poor high temperature cycle performance. Comparative Example 4 uses a binder styrene acrylic emulsion (PAR), and the pole piece produces a large swelling after injection, and the side reaction with the electrolyte increases, thereby causing an increase in irreversible active lithium consumption. It can be seen that Examples 1-5 use a specific binder SBR and cooperate with the active material to obtain a particle size adaptation technology to achieve a high bonding strength and low active site negative pole piece, thereby obtaining excellent high temperature performance.
[0138] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A negative electrode active slurry, It is characterized in that It includes graphite, styrene-butadiene rubber, a conductive agent, a dispersant and a solvent, the particle size D50 of the graphite is recorded as Df, the particle size D50 of the styrene-butadiene rubber is recorded as Ds, and the Df and Ds meet the following conditions: 50nm≤Ds≤100nm; 1000nm≤Df≤1600nm; 15≤Df / Ds≤20.
2. The negative electrode active slurry according to claim 1, It is characterized in that The negative electrode active slurry has one or more of the following characteristics: The graphite is selected from long-cycle graphite, and the long-cycle graphite is preferably selected from one or more of petroleum coke-derived graphite, asphalt coke-derived graphite and needle coke-derived graphite; The mass ratio of the added amount of the graphite to the solid matter in the negative electrode active slurry is (94.5-97.0):
100.
3. The negative electrode active slurry according to claim 1, It is characterized in that The mass ratio of the added amount of the styrene-butadiene rubber to the solid matter in the negative electrode active slurry is (1.0-2.5):
100.
4. The negative electrode active slurry according to claim 1, It is characterized in that The negative electrode active slurry has one or more of the following characteristics: The conductive agent is selected from one or more of conductive carbon black, carbon fiber, acetylene black, Ketjen black, graphene and carbon nanotubes; The mass ratio of the conductive agent to the solid matter in the negative electrode active slurry is (0.5-2.0):100; The dispersant is selected from carboxymethyl cellulose and / or Bik dispersant; The mass ratio of the dispersant to the solid matter in the negative electrode active slurry is (0.5-2.0):100; The solvent is water; The viscosity of the negative electrode active slurry is 3000-8000 mPa·s.
5. A method for preparing the negative electrode active slurry according to any one of claims 1 to 4, It is characterized in that The method comprises: mixing graphite, the conductive agent, the dispersant and the solvent, and then adding styrene-butadiene rubber and optionally a solvent, and mixing them uniformly.
6. A negative electrode sheet, It is characterized in that The negative electrode sheet includes a negative electrode current collector and a negative electrode material layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode material layer includes graphite, styrene-butadiene rubber, a conductive agent, and a dispersant. The particle size D50 of the graphite is recorded as Df, and the particle size D50 of the styrene-butadiene rubber is recorded as Ds. The Df and Ds satisfy the following conditions: 50nm≤Ds≤100nm; 1000nm≤Df≤1600nm; 15≤Df / Ds≤20.
7. The negative electrode sheet according to claim 6, It is characterized in that The negative electrode sheet has one or more of the following characteristics: The graphite is selected from long-cycle graphite, and the long-cycle graphite is preferably selected from one or more of petroleum coke-derived graphite, asphalt coke-derived graphite and needle coke-derived graphite; The mass fraction of the graphite in the negative electrode material layer is 94.5%-97%; The mass fraction of the styrene-butadiene rubber in the negative electrode material layer is 1.0%-2.5%; The conductive agent is selected from one or more of conductive carbon black, carbon fiber, acetylene black, Ketjen black, graphene and carbon nanotubes; The mass fraction of the conductive agent in the negative electrode material layer is 0.5%-2.0%; The dispersant is selected from carboxymethyl cellulose and / or Bik dispersant; The mass fraction of the dispersant in the negative electrode material layer is 0.5%-2.0%.
8. A method for preparing the negative electrode sheet according to claim 6 or 7, It is characterized in that The method comprises coating the negative electrode active slurry according to any one of claims 1 to 4 onto the negative electrode current collector, and then drying and pressing the negative electrode sheet to obtain the negative electrode sheet.
9. A lithium ion battery, It is characterized in that The lithium-ion battery comprises the negative electrode sheet according to claim 6 or 7.
10. Use of the negative electrode active slurry according to any one of claims 1 to 4 in improving the high temperature cycle performance of a battery.
Citation Information
Cited By
Method for manufacturing a battery cell, as well as a battery cell
DE102025105517B3