Sodium-sulfur battery electrolyte based on silane-based diluent as well as preparation method and application of sodium-sulfur battery electrolyte
By using low-polar silane solvent as diluent in sodium-sulfur battery electrolyte, the problems of sodium polysulfide dissolution and poor electronic conductivity in sodium-sulfur batteries are solved, and the long life cycle and excellent of sodium-sulfur batteries are achieved. Electrochemical properties.
Patent Information
- Application Number
- CN202411263789.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-10
AI Technical Summary
The sodium-sulfur battery generates sodium polysulfide during charging and discharging, resulting in differences in the concentration of positive and negative electrodes, resulting in loss of active substances and loss of metal sodium, and the electron conductivity of sulfur and polysulfides leads to uneven nucleation and growth on the electrode surface. , may cause safety hazards.
Using sodium-sulfur battery electrolyte based on silane diluents, low polar silane solvents such as dimethyl dimethoxysilane (DMMS) and dimethyl diethoxysilane (DEMS) are introduced into high concentration electrolytes. ) and tetraethyl silicate (TEOS) act as diluents to reduce the viscosity and density of the electrolyte, inhibit the dissolution of polysulfides, and promote the uniform deposition of sodium metal.
It significantly reduces the overall cost and environmental toxicity of the electrolyte, extends the cycle life of sodium metal-sulfur batteries, improves the stability and electrochemical performance of the electrode, reduces the consumption of sodium salt, and avoids the growth of sodium dendrites and the battery. Short circuit.
Smart Images

Figure CN118983528A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of sodium metal batteries, and in particular relates to a sodium-sulfur battery electrolyte based on a silane-based diluent, and a preparation method and application thereof. Background Art
[0002] In recent years, the energy density of lithium-ion batteries has reached a bottleneck. People are pursuing higher battery energy density and have turned their attention to batteries with lower costs and higher theoretical capacity (1675mAh·g -1 ) of sulfur. Metallic lithium has a low redox potential (-3.04Vvs. standard hydrogen electrode) and an ultra-high theoretical capacity (3860mAh·g -1 ), becoming one of the most attractive negative electrode materials. Lithium-sulfur batteries have developed rapidly in the past decade, but lithium resources are in short supply, with an abundance of only 0.01wt.% in the earth's crust. Relatively speaking, sodium resources are much more abundant, with an abundance of 2.3wt.% in the earth's crust, and the price is 25 times lower than that of lithium. Therefore, room temperature sodium-sulfur batteries are a more ideal energy storage solution.
[0003] Among many battery technologies, sodium-sulfur batteries have the advantages of easy availability of raw materials, high energy density, and low price, and are one of the most promising battery systems. However, sodium-sulfur batteries are still in their infancy, and their commercialization faces more severe challenges than lithium-sulfur batteries: 1) Sodium polysulfide is generated during the charge and discharge process of sodium-sulfur batteries, and its dissolution in the electrolyte leads to a concentration difference between the positive and negative electrodes. This difference prompts sodium polysulfide to "shuttle" to the negative electrode with the electrolyte and react with metallic sodium, which in turn leads to the loss of active substances and the loss of metallic sodium. 2) During the charge and discharge process, the electronic conductivity of sulfur and polysulfide is poor, and their volume changes are large. Therefore, in order to maintain rapid electron transfer and good structural integrity, a highly conductive host material is required. 3) As the electrochemical reaction proceeds, metallic sodium undergoes continuous stripping and electroplating on the electrode surface. However, due to the uneven distribution of electrons and ions on the electrode surface, metallic sodium undergoes uneven nucleation and growth, and eventually grows into sodium dendrites. The continued growth of sodium dendrites may penetrate the separator, causing internal short circuit of the battery, which in turn poses a safety hazard.
[0004] In order to solve the above problems, researchers have done a lot of research work in the design of positive electrode structure, modification of sodium metal negative electrode, design of new diaphragm, electrolyte engineering, etc. For example, Zhao et al. used 5% fluoroethylene carbonate as an additive in 1.0M NaClO4-ethylene carbonate / propylene carbonate (EC / PC, V / V=1 / 1) electrolyte, with carbon / sulfur composite as cathode, providing up to 1651mAh·g at 0.1C. -1reversible capacity. And X-ray photoelectron spectroscopy analysis clearly shows that the solid electrolyte interface (SEI) is more effective and the conversion between S and Na2S is more thorough. It is worth noting that carbonate electrolytes will undergo nucleophilic reactions with sodium polysulfide. In the case of lean electrolyte, the cycle life of sodium-sulfur batteries using carbonate electrolytes is significantly attenuated. When using traditional dimethyl ether-based electrolytes, the sulfur positive electrode produces sodium polysulfide that is easily soluble in the electrolyte during the conversion process, resulting in a "shuttle effect", leading to the loss of active substances and passivation of the sodium metal negative electrode. Therefore, electrolyte engineering is considered to be an excellent solution for achieving long-life cycles of sodium-sulfur batteries. Compared with other improvement schemes, the development of new electrolytes can better adapt to existing production lines and accelerate the industrialization of sodium-sulfur batteries. Summary of the invention
[0005] The object of the present invention is to provide a sodium-sulfur battery electrolyte based on a silane-based diluent, and a preparation method and application thereof. The electrolyte uses a sodium salt as a solute, an ether polar solvent as a main solvent, and a low-polarity silane-based solvent as a diluent. The prepared locally high-concentration electrolyte can simultaneously stabilize the metallic sodium negative electrode and the sulfur positive electrode.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] One of the technical solutions of the present invention is to provide a sodium-sulfur battery electrolyte based on a silane-based diluent, wherein the concentration of sodium salt in the electrolyte is 1.0-4.0M, the main solvent is an ether polar solvent, and the diluent is a weakly polar silane-based solvent;
[0008] The weakly polar silane-based solvent is a mixture of one or more of dimethyldimethoxysilane (DMMS), dimethyldiethoxysilane (DEMS), methyltriethoxysilane (MTES) and tetraethyl silicate (TEOS).
[0009] The density of DMMS solvent at 25°C is 0.848 g·cm -3 , the dielectric constant (ε) is 3.70, its solvation ability is poor, which is not conducive to the dissolution of polysulfides and has good compatibility with sodium metal.
[0010] The density of DEMS solvent at 25°C is 0.84 g·cm -3 , the dielectric constant (ε) is 3.22, its solvation ability is poor, which is not conducive to the dissolution of polysulfides and has good compatibility with sodium metal.
[0011] The density of MTES solvent at 25°C is 0.895 g·cm -3 , the dielectric constant (ε) is 3.85, its solvation ability is poor, which is not conducive to the dissolution of polysulfides and has good compatibility with sodium metal.
[0012] The density of TEOS solvent at 25°C is 0.93 g·cm -3 , the dielectric constant (ε) is 4.10, its solvation ability is poor, which is not conducive to the dissolution of polysulfides and has good compatibility with sodium metal.
[0013] The ideal sodium-sulfur battery electrolyte should have high ionic conductivity, relatively low density, excellent electrode stability, and can effectively inhibit the dissolution of polysulfides. The dissolution of polysulfides can be effectively reduced by increasing the salt concentration in the ether-based electrolyte, but the high-concentration electrolyte has the disadvantages of high electrolyte viscosity and high density, which limits its practical application. By introducing a diluent into the high-concentration electrolyte, the unique solvation structure of the high-concentration electrolyte can be maintained and the viscosity of the electrolyte can be significantly reduced, so it has received widespread attention. However, the diluents used in the current local high concentration are mostly fluorine-containing solvents, which have problems such as high density, high price, and corrosion of the metallic sodium negative electrode. The dissolution of polysulfides can be effectively inhibited by increasing the concentration, but the economic benefits are significantly reduced. Therefore, the local high-concentration electrolyte based on a low-cost, low-density and environmentally friendly silane-based diluent provided by the present invention can significantly reduce the overall cost, density and environmental toxicity of the electrolyte, and solve the problem of corrosion of sodium metal by fluorine-containing diluents, thereby achieving a long life cycle of a high-energy sodium metal-sulfur battery.
[0014] Preferably, the sodium salt is a mixture of one or more of sodium bis(trifluoromethylsulfonyl)imide (NaFSI), sodium trifluoromethanesulfonate (NaOTF), sodium perchlorate (NaClO4), sodium tetrafluoroborate (NaBF4), sodium bis(trifluoromethylsulfonyl)imide (NaTFSI) and sodium hexafluorophosphate (NaPF6).
[0015] Preferably, the ether polar solvent is ethylene glycol dimethyl ether (DME).
[0016] Preferably, the volume ratio of the main solvent to the diluent is 2:1 to 1:4.
[0017] The second technical solution of the present invention is to provide a method for preparing the sodium-sulfur battery electrolyte based on a silane-based diluent, the steps comprising:
[0018] The sodium salt, the main solvent and the diluent are mixed to obtain the sodium-sulfur battery electrolyte based on the silane-based diluent.
[0019] The third technical solution of the present invention is to provide an application of the above-mentioned sodium-sulfur battery electrolyte based on silane-based diluent in the preparation of sodium-sulfur batteries.
[0020] Preferably, the positive electrode of the sodium-sulfur battery is a sulfurized polyacrylonitrile positive electrode.
[0021] More preferably, the raw materials of the sulfurized polyacrylonitrile positive electrode include sulfurized polyacrylonitrile, a conductive agent and a binder.
[0022] More preferably, the mass ratio of the sulfided polyacrylonitrile, the conductive agent and the binder is (75-95):(2.5-12.5):(2.5-12.5).
[0023] More preferably, the preparation step of the sulfurized polyacrylonitrile comprises: mixing sulfur powder and polyacrylonitrile in a mass ratio of 1:4, calcining at 300-500° C. for 1-3 hours under a nitrogen atmosphere, and grinding to a particle size of 100-150 nm to obtain the sulfurized polyacrylonitrile.
[0024] More preferably, the conductive agent includes at least one of Super P, acetylene black (AB), conductive carbon black, carbon nanotubes and graphene.
[0025] More preferably, the binder includes at least one of styrene-butadiene rubber (SBR) emulsion, polytetrafluoroethylene, carboxymethyl cellulose (CMC) and polyvinylidene fluoride.
[0026] The beneficial technical effects of the present invention are as follows:
[0027] (1) The present invention uses a lightweight, weakly polar silane-based solvent as an electrolyte diluent, which can effectively reduce the overall concentration of the electrolyte and reduce the consumption of sodium salt.
[0028] (2) The sodium-sulfur battery electrolyte prepared by the present invention using a weakly polar silane-based solvent as a diluent can effectively inhibit the dissolution and shuttle effect of polysulfides.
[0029] (3) The inner layer of the electrode / electrolyte interface of the sodium metal-sulfur battery provided by the present invention is rich in inorganic components, and the outer layer is a polymer layer. This multilayer structure can promote the uniform deposition of metallic sodium and inhibit the growth of sodium dendrites.
[0030] (4) The metal sodium-sulfur battery made of the silane-based diluent sodium-sulfur battery electrolyte and the sulfurized polyacrylonitrile positive electrode provided by the present invention has excellent electrochemical properties and has important application prospects in the field of sodium-sulfur batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is the electrochemical impedance test result of the stainless steel-stainless steel battery in Example 1.
[0032] Figure 2 : is the sodium deposition / stripping polarization curve of the sodium metal symmetric battery in Example 1.
[0033] Figure 3 This is the cycle stability test result of the sodium-sulfur battery in Example 1.
[0034] Figure 4This is a scanning electron microscope image of metallic sodium deposited on the carbon-coated aluminum foil in the sodium / aluminum (Na / Al) battery of Example 1.
[0035] Figure 5 This is the Coulombic efficiency diagram of the sodium / aluminum (Na / Al) battery in Example 1.
[0036] Figure 6 : This is the sodium deposition / stripping polarization curve of the sodium metal symmetric battery in Example 2.
[0037] Figure 7 : This is the sodium deposition / stripping polarization curve of the sodium metal symmetric battery in Example 3.
[0038] Figure 8 : This is the sodium deposition / stripping polarization curve of the sodium metal symmetric battery in Example 4.
[0039] Fig. 9 This is the Coulombic efficiency diagram of the sodium / aluminum (Na / Al) battery in Example 5.
[0040] Fig.10 This is the Coulombic efficiency diagram of the sodium / aluminum (Na / Al) battery in Example 6. DETAILED DESCRIPTION
[0041] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.
[0042] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0043] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention pertains. Although only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention.
[0044] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0045] Unless otherwise specified, the "room temperature" in the embodiments of the present invention refers to a temperature of 25°C.
[0046] Example 1
[0047] (1) In a glove box filled with argon, DME and DMMS solvents were used After dehydration treatment with molecular sieves, NaFSI was kept dry at 80°C overnight.
[0048] (2) Take 203.12 mg of NaFSI obtained in step (1), fully dissolve it in 156 μL of DME solvent obtained in step (1), and then add 283 μL of DMMS obtained in step (1) to obtain an electrolyte with a NaFSI:DME:DMMS molar ratio of 1:1.5:2 (sodium salt concentration is 2.6 M).
[0049] (3) Take 4 g of sulfur powder and 1 g of polyacrylonitrile, mix them evenly, calcine them at 450° C. for 3 h in a nitrogen atmosphere, and grind them to obtain sulfurized polyacrylonitrile powder (100-150 nm).
[0050] (4) The vulcanized polyacrylonitrile powder obtained in step (3) is mixed with Super P, CMC and SBR in a ratio of 8:1:0.5:0.5 to obtain a vulcanized polyacrylonitrile slurry.
[0051] (5) The slurry obtained in step (4) is evenly coated on a carbon-coated aluminum foil and dried in a vacuum drying oven at 80° C. for 10 h to obtain a sulfurized polyacrylonitrile positive electrode material.
[0052] (6) The sulphurized polyacrylonitrile positive electrode material obtained in step (4) is punched into an electrode sheet with a diameter of 6 mm using a punching machine and transferred to a glove box.
[0053] (7) The solution obtained in step (2) was used as the electrolyte of the battery, Glassfiber / A was used as the separator, a stainless steel-stainless steel battery was assembled and an electrochemical impedance spectroscopy test was performed at room temperature.
[0054] (8) The solution obtained in step (2) was used as the electrolyte of the battery, Glassfiber / A was used as the separator, a sodium metal symmetric battery was assembled and the electrochemical performance was tested at room temperature.
[0055] (9) The solution obtained in step (2) was used as the electrolyte of the battery, Glassfiber / A was used as the separator, carbon-coated aluminum foil was used as the working electrode, sodium was used as the counter electrode, a Na / Al battery was assembled and a sodium deposition test was performed at room temperature.
[0056] (10) The solution obtained in step (2) is used as the electrolyte of the battery, Glassfiber / A is used as the separator, sodium metal is used as the negative electrode, the sulfurized polyacrylonitrile positive electrode material obtained in step (6) is used as the positive electrode, a sodium-sulfur battery is assembled, and the electrochemical performance test is performed at room temperature.
[0057] The results of the electrochemical impedance test (25°C, frequency range 100000~0.1Hz) of the stainless steel-stainless steel battery in Example 1 are shown in Figure 1 ,from Figure 1 It can be seen that the electrolyte has a high ionic conductivity.
[0058] Sodium deposition / stripping polarization curves of the sodium metal symmetric battery in Example 1 (25°C, current density 0.5 mA cm -2 , the deposition capacity is 0.5 mAh cm -2 )See Figure 2 ,from Figure 2 It can be seen that the assembled sodium metal symmetric battery has good cycling stability.
[0059] The cycle stability test results of the sodium-sulfur battery in Example 1 are shown in Figure 3 , the positive and negative electrode surface capacity ratio is 4, and the current density is 0.2A·g -1 Under the condition of , the first reversible specific capacity of polyacrylonitrile sulfide cathode is about 421 mAh g -1 After 100 cycles, there is almost no capacity decay.
[0060] In the sodium / aluminum (Na / Al) battery of Example 1, the current density is 0.5 mA·cm -2 , the deposition amount is 2 mAh·cm -2 The metallic sodium was deposited on the carbon-coated aluminum foil under the conditions of Figure 4 .from Figure 4 From the scanning electron microscope photograph, it can be observed that the deposition of sodium metal is relatively smooth and uniform, indicating that the prepared electrolyte can achieve reversible deposition and stripping of metallic sodium.
[0061] The constant current charge and discharge method was used and the test was performed at 1.0 mA cm -2 Current density, 1.0 mAh cm -2 The coulombic efficiency of the sodium / aluminum (Na / Al) battery in Example 1 under the conditions of the deposition amount is shown in Figure 5 .
[0062] Example 2
[0063] Compared with Example 1, the difference is that the content of DMMS added in step (2) is different, and the electrolyte with a molar ratio of NaFSI:DME:DMMS of 1:1.5:3 (sodium salt concentration is 1.7 M) is obtained.
[0064] Figure 6 The sodium deposition / stripping polarization curve of the sodium metal symmetric battery in Example 2 (25°C, current density 1 mA·cm -2, the deposition capacity is 1 mAh cm -2 ). Figure 6 It shows that the symmetrical battery has a large polarization potential and short circuit occurs at around 400h.
[0065] Example 3
[0066] Compared with Example 1, the difference is that no diluent is added in step (2), and a high-concentration electrolyte with a NaFIS:DME molar ratio of 1:1.5 (sodium salt concentration of 6.4 M) is obtained.
[0067] Figure 7 The sodium deposition / stripping polarization curve of the sodium metal symmetric battery in Example 3 (25°C, current density 0.5 mA·cm -2 , the deposition capacity is 0.5 mAh cm -2 ). Figure 7 It shows that the polarization potential of the symmetrical battery is large, the polarization curve is tortuous, and a short circuit occurs around 470h.
[0068] Example 4
[0069] Compared with Example 1, the difference is that in step (2), the diluent is 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, and an electrolyte with the same molar ratio is obtained (sodium salt concentration is 2.2 M).
[0070] Figure 8 The sodium deposition / stripping polarization curve of the sodium metal symmetric battery in Example 4 (25°C, current density 0.5 mA·cm -2 , the deposition capacity is 0.5 mAh cm -2 ). Figure 8 It shows that the symmetrical battery short circuit occurs around 540h.
[0071] Example 5
[0072] Compared with Example 1, the difference is that the diluent in step (2) is 3-fluorotoluene, and an electrolyte with the same molar ratio (sodium salt concentration is 2.7 M) is obtained.
[0073] Fig. 9 The coulombic efficiency diagram (1.0 mA·cm) of the sodium / aluminum (Na / Al) battery in Example 5 is shown in FIG. -2 Current density, 1.0 mAh cm -2 Sedimentation amount). Fig. 9 It shows that the battery coulombic efficiency is extremely low, not exceeding 20% at most.
[0074] Example 6
[0075] Compared with Example 2, the difference is that in step (2), the diluent is 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, and the obtained electrolyte has a molar ratio of NaFIS:DME:diluent of 1:1.5:3 (sodium salt concentration is 1.6M).
[0076] Fig.10 The coulombic efficiency diagram (1.0 mA·cm) of the sodium / aluminum (Na / Al) battery in Example 6 is shown in FIG. -2 Current density, 1.0 mAh cm -2 Sedimentation amount). Fig.10 It shows that the battery has a high coulombic efficiency, but due to the side reaction between the diluent and sodium metal, the coulombic efficiency is significantly reduced.
[0077] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A sodium-sulfur battery electrolyte based on a silane-based diluent, characterized in that: The concentration of sodium salt in the electrolyte is 1.0-4.0M, the main solvent is an ether polar solvent, and the diluent is a weak polar silane-based solvent; The weakly polar silane-based solvent is a mixture of one or more of dimethyldimethoxysilane, dimethyldiethoxysilane, methyltriethoxysilane and tetraethyl silicate.
2. The sodium-sulfur battery electrolyte based on a silane-based diluent according to claim 1, characterized in that: The sodium salt is a mixture of one or more of sodium bis(trifluoromethylsulfonyl)imide, sodium trifluoromethanesulfonate, sodium perchlorate, sodium tetrafluoroborate, sodium bis(trifluoromethylsulfonyl)imide and sodium hexafluorophosphate.
3. The sodium-sulfur battery electrolyte based on a silane-based diluent according to claim 1, characterized in that: The ether polar solvent is ethylene glycol dimethyl ether.
4. The sodium-sulfur battery electrolyte based on a silane-based diluent according to claim 1, characterized in that: The volume ratio of the main solvent to the diluent is 2:1 to 1:
4.
5. A method for preparing a sodium-sulfur battery electrolyte based on a silane-based diluent according to any one of claims 1 to 4, characterized in that the steps include: The sodium salt, the main solvent and the diluent are mixed to obtain the sodium-sulfur battery electrolyte based on the silane-based diluent.
6. Use of the sodium-sulfur battery electrolyte based on a silane-based diluent according to any one of claims 1 to 4 in the preparation of a sodium-sulfur battery.
7. The use according to claim 6, characterized in that: The positive electrode of the sodium-sulfur battery is a sulfurized polyacrylonitrile positive electrode.
8. The use according to claim 7, characterized in that: The raw materials of the sulfided polyacrylonitrile positive electrode include sulfided polyacrylonitrile, a conductive agent and a binder.
9. The use according to claim 8, characterized in that: The mass ratio of the sulfided polyacrylonitrile, the conductive agent and the binder is (75-95):(2.5-12.5):(2.5-12.5).
10. The use according to claim 8, characterized in that: The preparation steps of the sulfurized polyacrylonitrile include: mixing sulfur powder and polyacrylonitrile in a mass ratio of 1:4, calcining at 300-500° C. for 1-3 hours under a nitrogen atmosphere, and grinding to a particle size of 100-150 nm to obtain the sulfurized polyacrylonitrile.
Citation Information
Patent Citations
Alkali metal sulfur battery electrolyte, preparation method thereof and alkali metal sulfur secondary battery containing alkali metal sulfur battery electrolyte
CN117117331A
Low-temperature low-density sodium ion battery electrolyte and sodium ion battery
CN117810542A
Stable room-temperature sodium-sulfur battery
US20190067730A1
Method of Producing Participate Electrode Materials for Alkali Metal Batteries
US20190173079A1
Fire-resistant lithium battery containing an electrode-protecting layer
US20190372148A1