Heat-conducting gasket, manufacturing method and application of heat-conducting gasket
By covering or contacting the grid film on both sides of the thermally conductive silicone gasket, combined with the mixed preparation process of liquid silicone resin and thermally conductive powder, the problem of insufficient thermal conductivity and bonding rate of thermally conductive gaskets in certain application fields is solved. It achieves efficient thermal conductivity and long-life thermal conductivity, and is suitable for semiconductor chips and other fields.
Patent Information
- Application Number
- CN202411088354.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-19
AI Technical Summary
In some application fields, such as semiconductor chips, the thermal conductivity and bonding rate are insufficient, resulting in a short service life and complex process, making it difficult for domestic manufacturers to meet performance needs and rely on imported products.
Using a thermally conductive silicone gasket matrix, covered with or contact composite or single-layer mesh film on both sides, it is prepared by mixing liquid silicone resin, thermally conductive powder, catalyst and additives, and prepared by dispersion vacuum and pressure-release curing processes to form Thermal gasket with high fit rate and thermal conductivity.
It achieves high bonding rate, good thermal conductivity and long service life of thermal gaskets. It is suitable for electronic equipment and cavity etching and other fields, simplifies bonding operations and improves process stability and efficiency.
Smart Images

Figure CN118984566A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of thermal conductive materials, and in particular to a thermal conductive gasket, a preparation method and application thereof. Background Art
[0002] Thermal conductive material is a new type of industrial material, which is widely used in the field of electronic component heat dissipation. It can be filled between electronic components and radiators to expel the air therein, so that the heat generated by the electronic components can be transferred to the radiator more quickly through the thermal interface material, thereby achieving the important role of reducing the operating temperature and extending the service life.
[0003] Thermal conductive materials can be mainly divided into several categories, including thermal grease, thermal gel, thermal gasket, thermal film and thermal phase change material. Among them, thermal gasket has the advantages of easy use, high thermal conductivity, stable thermal performance, good compressibility, self-adhesion and high cleanliness. It is an excellent thermal conductive material with a wide range of applications.
[0004] Thermal conductive gaskets are mainly used in electronic equipment, LED lamps, power machinery, semiconductor chips, automobiles, and military industries. In most fields, thermal conductive gaskets produced by domestic manufacturers can basically meet the performance requirements. However, the thermal conductive gaskets used in some fields (such as semiconductor chips) are still imported. This is mainly due to many factors such as complex formula, multiple physical properties, complicated processes, and special application fields. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides a thermally conductive gasket having the characteristics of high lamination rate, good thermal conductivity and long service life.
[0006] To achieve the above-mentioned purpose, the first aspect of the present invention provides a thermally conductive gasket, including a thermally conductive gasket substrate, wherein both sides of the thermally conductive silicone gasket substrate are fluoroplastic release films. After film transfer, one side is covered with or in contact with a grid film A, and the other side is covered with or in contact with a grid film B; the grid film A is selected from a composite grid film, and the grid film B is selected from a composite grid film or a single-layer grid film.
[0007] The thermally conductive pad substrate is mainly prepared by mixing liquid silicone resin, thermally conductive powder, catalyst, inhibitor and other additives. The liquid silicone resin includes vinyl silicone oil and hydrogen-containing silicone oil.
[0008] The mesh shapes of the mesh membranes A and B are preferably square or diamond.
[0009] The grid side length of the grid membrane A and the grid membrane B is preferably 0.3 to 5 mm;
[0010] And / or, the grid spacing of the grid membrane A and the grid membrane B is preferably 50-1000 um;
[0011] And / or, the grid groove depth of the grid film A and the grid film B is preferably 20-400 um.
[0012] Furthermore, the grid side length of the grid membrane A and the grid membrane B is preferably 0.3 to 3 mm;
[0013] And / or, the grid spacing of the grid membrane A and the grid membrane B is preferably 50-400 um;
[0014] And / or, the grid groove depth of the grid film A and the grid film B is preferably 20-200 um.
[0015] A second aspect of the present invention provides a method for preparing a thermally conductive gasket for an etching chamber, comprising the following steps:
[0016] (1) Dispersed vacuum
[0017] Add liquid silicone resin, thermal conductive powder, catalyst, inhibitor and other additives into a mixing device, disperse and evacuate, and obtain a thermal conductive mixture after uniform dispersion;
[0018] (2) Rolling and curing
[0019] Use the calendering equipment to evenly extrude the thermal conductive mixture into the fluoroplastic release films on both sides, and then pull it into the tunnel furnace for curing;
[0020] (3) Transfer
[0021] The cured thermal conductive layer is transferred to a film, and one side of the fluoroplastic release film is transferred to a grid film A, and the other side of the fluoroplastic release film is transferred to a grid film B, so as to obtain a thermal conductive gasket with one side covered or in contact with the grid film A and the other side covered or in contact with the grid film B, wherein the grid film A is selected from a composite grid film, and the grid film B is selected from a composite grid film or a single-layer grid film.
[0022] The liquid silicone resin described above includes vinyl silicone oil and hydrogen-containing silicone oil. The viscosity of the vinyl silicone oil ranges from 300 to 11000 mPa.s, the viscosity of the hydrogen-containing silicone oil ranges from 50 to 500 mPa.s, and the mass ratio of the vinyl silicone oil to the hydrogen-containing silicone oil is 1:1 to 50:1.
[0023] In the above preparation method, the dispersed vacuuming in step (1) comprises the following steps:
[0024] Step 1-1: First add the non-thermal conductive powder raw material, stir for 5 to 10 minutes at a stirring speed of 10 to 20 rpm / min, and finally add the thermal conductive powder part, with the particle size from large to small, stirring while adding, and the stirring speed is 30 to 50 rpm / min;
[0025] Step 1-2: After adding, stir for 20 to 30 minutes at a stirring speed of 40 to 80 rpm / min;
[0026] Step 1-3: Vacuum and stir for 90 to 120 minutes, with a stirring speed of 60 to 100 rpm / min and an absolute vacuum pressure of 0.1 to 10 Pa.
[0027] The third aspect of the present invention provides an application of a thermally conductive gasket, wherein the thermally conductive gasket is transferred and bonded to an edge ring, the edge ring after bonding the thermally conductive gasket is assembled with a tunable edge sheath ring, and the assembled whole is installed on an Electrostatic chuck and finally applied to cavity etching.
[0028] Furthermore, the transfer, lamination and assembly of the thermally conductive gasket includes the following steps:
[0029] Step 1: Lofting: Peel off the thermal pad from the grid film B, align it with the glue plate through the positioning point, with the grid film A facing down, to form a complete circular ring on the glue plate;
[0030] Step 2: Laminating: Place the edge ring on the laminating plate with the thermal conductive gasket, and apply a certain gravity to make the edge ring and the thermal conductive gasket fit completely;
[0031] Step 3: Remove the edge ring from the glue plate, flip it 180 degrees and place it horizontally, and peel off the grid film A with the thermal pad facing upward, so that the thermal pads are attached to the inner and outer rings of the edge ring.
[0032] Step 4: Assemble: Place the tunable edge sheath ring vertically downward on the outer ring of the edge ring with the thermal pad attached, align them through the positioning holes to form a whole, and assemble them to the Electrostatic chuck. The thermal pad on the inner ring of the edge ring is attached to the Electrostatic chuck, and the thermal pad on the outer ring of the edge ring is attached to the tunable edge sheath ring.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] (1) The thermally conductive gasket of the present invention comprises a thermally conductive silicone gasket substrate, and both sides of the thermally conductive gasket substrate are fluoroplastic release films, which are helpful for demolding after the silicone is cured and have good heat resistance;
[0035] (2) The thermally conductive gasket in the present invention is covered or in contact with the grid film A on one side and the grid film B on the other side. The thermally conductive gasket is in contact with the grid film, so that the grid pattern is printed on the surface of the thermally conductive gasket, which is conducive to the discharge of bubbles when the application end is attached, and a higher attachment ratio can be achieved, thereby achieving a better heat conduction effect and ensuring that the working temperature meets the requirements; in addition, the actual contact area between the grid film and the thermally conductive gasket is low, and the separation force between the thermally conductive gasket and the grid film A is greater than or equal to the separation force between the thermally conductive gasket and the grid film B, which is conducive to the separation of the application end;
[0036] (3) The thermally conductive gasket of the present invention is applied to the plasma chamber etching process, that is, the thermally conductive gasket is transferred and bonded to the edgering, and finally the thermally conductive gasket and different parts are bonded. The thermally conductive gasket of the present invention has the characteristics of simple bonding operation, high bonding rate, good thermal conductivity and long service life. DETAILED DESCRIPTION
[0037] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] <Thermal gasket>
[0039] The first aspect of the present invention provides a thermally conductive gasket, including a thermally conductive silicone gasket substrate, wherein both sides of the thermally conductive silicone gasket substrate are fluoroplastic release films. After film transfer, one side is covered with or in contact with a grid film A, and the other side is covered with or in contact with a grid film B; the grid film A is selected from a composite grid film, and the grid film B is selected from a composite grid film or a single-layer grid film.
[0040] In the embodiment of the present invention, the thermally conductive silicone gasket substrate is mainly prepared by mixing liquid silicone resin, thermally conductive powder, catalyst, inhibitor and other additives, and the liquid silicone resin includes vinyl silicone oil and hydrogen-containing silicone oil.
[0041] Furthermore, in an embodiment of the present invention, the viscosity range of the vinyl silicone oil is 300 to 11000 mPa.s, the viscosity range of the hydrogen-containing silicone oil is 50 to 500 mPa.s, and the mass ratio of the vinyl silicone oil to the hydrogen-containing silicone oil is 1:1 to 50:1.
[0042] In view of the ease of silicone demoulding and the heat resistance of the film, the fluoroplastic release film in the embodiment of the present invention is selected from a fluorine release film with a thickness of 25 to 100 um, and the release force of the fluoroplastic release film is 0.1 to 10 oz / in.
[0043] The composite mesh film of the present invention is a composite of a single-layer mesh film and a PET film. The composite mesh film has good support due to the presence of PET.
[0044] In order to improve the convenience of the subsequent mold transfer process, the peeling force between the thermally conductive gasket substrate and the grid film A is greater than or equal to the peeling force between the thermally conductive gasket substrate and the grid film B. The release force of the grid film A is preferably 10-80oz / in, and the release force of the grid film B is preferably 10-80oz / in. The release force of the grid film A is greater than or equal to the release force of the grid film B, which can indirectly indicate that the peeling force between the thermally conductive gasket substrate and the grid film A is greater than or equal to the peeling force between the thermally conductive gasket substrate and the grid film B.
[0045] From the perspective of the foldability and practical application of the film, the mesh film B in the embodiment of the present invention is preferably a single-layer mesh film.
[0046] In the embodiment of the present invention, the single-layer mesh film is selected from one of PE, PP, PVC and PC materials, and the thickness is preferably 25-100 um.
[0047] Considering the thermal conductivity of the product, the mesh shape of the mesh films A and B in the embodiment of the present invention is preferably a square or a diamond.
[0048] Considering the thermal conductivity of the product, the mesh side length of the mesh film A and the mesh film B in the embodiment of the present invention is preferably 0.3 to 5 mm;
[0049] And / or, the grid spacing of the grid membrane A and the grid membrane B is preferably 50-1000 um;
[0050] And / or, the grid groove depth of the grid film A and the grid film B is preferably 20-400 um.
[0051] Furthermore, the grid side length of the grid membrane A and the grid membrane B in the embodiment of the present invention is preferably 0.3 to 3 mm;
[0052] And / or, the grid spacing of the grid membrane A and the grid membrane B is preferably 50-400 um;
[0053] And / or, the grid groove depth of the grid film A and the grid film B is preferably 20-200 um.
[0054] <Method for preparing thermally conductive pad>
[0055] A second aspect of the present invention provides a method for preparing a thermally conductive pad, comprising the following steps:
[0056] (1) Dispersed vacuum
[0057] Add liquid silicone resin, thermal conductive powder, catalyst, inhibitor and other additives into a mixing device, disperse and evacuate, and obtain a thermal conductive mixture after uniform dispersion;
[0058] (2) Rolling and curing
[0059] Use the calendering equipment to evenly extrude the thermal conductive mixture into the fluoroplastic release films on both sides, and then pull it into the tunnel furnace for curing;
[0060] (3) Transfer
[0061] The cured thermal conductive layer (i.e., thermal conductive gasket substrate) is transferred to form a fluoroplastic release film on one side into a mesh film A, and the other side into a mesh film B, so as to obtain a thermal conductive gasket with one side covered or in contact with the mesh film A and the other side covered or in contact with the mesh film B, wherein the mesh film A is selected from a composite mesh film, and the mesh film B is selected from a composite mesh film or a single-layer mesh film.
[0062] In an embodiment of the present invention, the thermally conductive silicone gasket matrix is mainly prepared by mixing liquid silicone resin, thermally conductive powder, catalyst, inhibitor and other additives, wherein the liquid silicone resin includes vinyl silicone oil and hydrogen-containing silicone oil, the viscosity range of the vinyl silicone oil is 300 to 11000 mPa.s, and the vinyl content is 0.20% to 0.40%; the viscosity range of the hydrogen-containing silicone oil is 50 to 500 mPa.s, and the silicon-hydrogen bond content is 0.01% to 0.10%, and the mass ratio of the vinyl silicone oil to the hydrogen-containing silicone oil is 1:1 to 50:1.
[0063] In an embodiment of the present invention, the thermally conductive powder is selected from one or more of aluminum oxide, aluminum hydroxide, aluminum powder, zinc oxide, aluminum nitride, and boron nitride, preferably aluminum oxide; the median particle size of the thermally conductive powder is 0.5 to 120 μm. The use of two (or more) thermally conductive powders of specific particle sizes for matching and filling can better fill the gaps between the thermally conductive powders and form a better thermal conductive channel. The mass fraction of the thermally conductive powder accounts for 70% to 96% of all materials, preferably 80% to 92%.
[0064] In an embodiment of the present invention, the catalyst includes chloroplatinic acid and Custer platinum catalyst, preferably Custer platinum catalyst, and its content is 0.01-0.40% of the total weight of the liquid silicone resin, preferably 0.05-0.20%.
[0065] In an embodiment of the present invention, the inhibitor includes one or more of maleates, fumarates, alkynes, and organic phosphines, and the content thereof is 0.01 to 0.20%, preferably 0.02 to 0.1%, of the total weight of the liquid silicone resin.
[0066] The other additives include organic additives and inorganic additives: the organic additives include silane coupling agents and viscosity reducers; the inorganic additives include one or more of nano carbon black, conductive nano carbon black, graphite, graphene, nano silicon dioxide, and nano titanium dioxide. The amount of other additives is 0.01% to 1% of the total weight of all materials, preferably 0.02% to 0.5%.
[0067] In view of the ease of silicone demoulding and the heat resistance of the film, the fluoroplastic release film in the embodiment of the present invention is selected from a fluorine release film with a thickness of 25 to 100 um, and the release force of the fluoroplastic release film is 0.1 to 10 oz / in.
[0068] In the embodiment of the present invention, the single-layer mesh film is selected from one of PE, PP, PVC and PC materials, and the thickness is preferably 25-100 um.
[0069] Considering the thermal conductivity of the product, the mesh shape of the mesh films A and B in the embodiment of the present invention is preferably a square or a diamond.
[0070] Considering the thermal conductivity of the product, the mesh side length of the mesh film A and the mesh film B in the embodiment of the present invention is preferably 0.3 to 5 mm;
[0071] And / or, the grid spacing of the grid membrane A and the grid membrane B is preferably 50-1000 um;
[0072] And / or, the grid groove depth of the grid film A and the grid film B is preferably 20-400 um.
[0073] Furthermore, the grid side length of the grid membrane A and the grid membrane B in the embodiment of the present invention is preferably 0.3 to 3 mm;
[0074] And / or, the grid spacing of the grid membrane A and the grid membrane B is preferably 50-400 um;
[0075] And / or, the grid groove depth of the grid film A and the grid film B is preferably 20-200 um.
[0076] In the embodiment of the present invention, the dispersed vacuuming in step (1) comprises the following steps:
[0077] Step 1-1: First add the non-thermal conductive powder raw material, stir for 5 to 10 minutes at a stirring speed of 10 to 20 rpm / min, and finally add the thermal conductive powder part, with the particle size from large to small, stirring while adding, and the stirring speed is 30 to 50 rpm / min;
[0078] Step 1-2: After adding, stir for 20 to 30 minutes at a stirring speed of 40 to 80 rpm / min;
[0079] Step 1-3: Vacuum and stir for 90 to 120 minutes, with a stirring speed of 60 to 100 rpm / min and an absolute vacuum pressure of 0.1 to 10 Pa.
[0080] In step (2) of the embodiment of the present invention, the tunnel furnace has a total of 8 ovens, which are arranged in sequence, each oven is 1 m long, and the sample enters the oven for curing at a pulling speed of 0.1 m / min. The temperature of each oven is 60-100°C, 100-130°C, 130-140°C, 130-140°C, 130-140°C, 130-140°C, 100-130°C, and 60-100°C, respectively.
[0081] From the perspective of ease of film transfer operation, the release force between the thermally conductive gasket substrate and the grid film A in step (3) of the present invention is greater than or equal to the release force between the thermally conductive gasket substrate and the grid film B. The release force of the grid film A is preferably 10 to 80 oz / in, and the release force of the grid film B is preferably 10 to 80 oz / in. It is preferred to transfer one side of the fluoroplastic release film to the grid film A, and then transfer the other side of the fluoroplastic release film to the grid film B. In other possible methods, the order of mold transfer can also be adjusted according to actual usage. In addition, according to actual usage, the cured thermal conductive layer can be die-cut into small sizes before film transfer in step (3), for example, 10 to 100 cm in length and 10 to 50 cm in width; the thickness can be controlled by adjusting the parameters of the calender roller of the die-cutting machine, for example, the thickness is 0.10 to 1.00 mm; after one side of the release film is transferred to the grid film A or the grid film B, it can be die-cut into small sizes, for example, 2 to 90 cm in length and 1 to 40 cm in width; the thermal conductive layer after die-cutting can be in a variety of shapes, such as rectangular, square, circular, arc-shaped, etc.
[0082] <Application of thermal pads>
[0083] A third aspect of the present invention provides an application of a thermally conductive gasket, which is mainly used in a 3D NAND channel hole etching process.
[0084] The main steps are: transferring and bonding the thermal pad to the edge ring, assembling the edge ring with the tunable edge sheath ring after bonding the thermal pad, and installing the assembled whole on the Electrostatic chuck, finally realizing the bonding of the thermal pad and different components, and exerting its application performance during the operation of the etching chamber, so as to achieve the characteristics of low application temperature and long service life.
[0085] The thermal pad installation process includes four steps: "layout - glue pressing - film tearing - assembly":
[0086] Step 1: Lofting: Peel off the thermal pad from the grid film B, align it with the glue plate through the positioning point, with the grid film A facing down, to form a complete circular ring on the glue plate;
[0087] Step 2: Laminating: Place the edge ring on the laminating plate with the thermal conductive gasket, and apply a certain gravity to make the edge ring and the thermal conductive gasket fit completely;
[0088] Step 3: Remove the edge ring from the glue plate, flip it 180 degrees and place it horizontally, peel off the grid film A with the thermal pad facing up, and finally make sure that the thermal pads are attached to the inner and outer rings of the edge ring;
[0089] Step 4: Assemble: Place the tunable edge sheath ring vertically downward on the outer ring of the edge ring with the thermal pad attached, align them through the positioning holes to form a whole, and assemble them to the Electrostatic chuck. The thermal pad on the inner ring of the edge ring is attached to the Electrostatic chuck, and the thermal pad on the outer ring of the edge ring is attached to the tunable edge sheath ring. BRIEF DESCRIPTION OF THE DRAWINGS
[0090] Figure 1 This is a flow chart of the preparation of the thermally conductive gasket in Example 1 of the present invention.
[0091] Figure 2 This is a diagram of an application scenario of a thermally conductive gasket in an embodiment of the present invention.
[0092] Figure 3 This is a diagram for evaluating the lamination performance of the thermally conductive gasket in an embodiment of the present invention.
[0093] Example
[0094] The present invention is described below with reference to the following examples, but the present invention is not limited to the following examples.
[0095] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0096] Example 1
[0097] This embodiment provides a method for preparing a thermally conductive pad, comprising the following steps:
[0098] (1) Dispersed vacuum
[0099] Add vinyl silicone oil (viscosity 1150mPa.s), hydrogenated silicone oil (viscosity 230mPa.s), thermally conductive powder, catalyst, inhibitor and other additives into a mixing device, disperse and evacuate, and obtain a thermally conductive mixture after uniform dispersion. Among them, the mass fractions of each component are: 9.4 parts of vinyl silicone oil, 0.6 parts of hydrogenated silicone oil; 40.5 parts of 50um median particle size Al2O3 powder, 10.0 parts of 10um median particle size Al2O3 powder, 22.5 parts of 5um median particle size Al2O3 powder, 17.0 parts of 2um median particle size Al2O3 powder; 0.008 parts of platinum catalyst, 0.002 parts of inhibitor, 0.08 parts of nano carbon black, and 0.02 parts of KH570 silane coupling agent.
[0100] The dispersed vacuuming comprises the following steps:
[0101] Step 1-1: First add the non-thermal conductive powder raw material, and stir for 10 minutes at a stirring speed of 20rpm / min. Finally, add the thermal conductive powder, with the particle size from large to small, and stir while adding, at a stirring speed of 40rpm / min;
[0102] Step 1-2: After adding, stir for 20 minutes at a stirring speed of 40 rpm / min;
[0103] Step 1-3: Evacuate and stir for 120 min, with a stirring speed of 80 rpm / min and an absolute vacuum pressure of 5 Pa.
[0104] (2) Rolling and curing
[0105] The heat-conducting mixture in step (1) is uniformly extruded into a fluoroplastic release film (PET) with a thickness of 50 μm on both sides by using a calendering device, and is pulled into a tunnel oven at a pulling speed of 0.1 m / min for curing, wherein the temperatures of the eight ovens are 60° C., 100° C., 140° C., 140° C., 140° C., 100° C., and 60° C., respectively;
[0106] (3) Transfer
[0107] The thermal conductive layer cured in step (2) is transferred to a mold, and the 50um fluoroplastic release film (PET) on one side is first torn off, and a composite mesh film (PP+PET) with a thickness of 100um is covered, and then the 50um fluoroplastic release film (PET) on the other side is torn off and replaced with a 50um single-layer mesh film (PP), and finally a thermal conductive gasket product is obtained with one side contacting the composite mesh film and the other side contacting the single-layer mesh film, wherein the mesh shape of the composite mesh film and the single-layer mesh film is square, the mesh side length is 0.3mm, the mesh spacing is 50um, and the mesh groove depth is 20um.
[0108] Example 2
[0109] The experimental steps of this embodiment are the same as those of Embodiment 1, except that in this embodiment, the grid shape of the composite grid membrane and the single-layer grid membrane in step (3) is square, the grid side length is 1.0 mm, the grid spacing is 150 um, and the grid groove depth is 70 um.
[0110] Example 3
[0111] The experimental steps of this embodiment are the same as those of Embodiment 1, except that in this embodiment, the grid shape of the composite grid membrane and the single-layer grid membrane in step (3) is square, the grid side length is 3.0 mm, the grid spacing is 360 um, and the grid groove depth is 180 um.
[0112] Example 4
[0113] The experimental steps of this embodiment are the same as those of Embodiment 1, except that in this embodiment, the grid shape of the composite grid membrane and the single-layer grid membrane in step (3) is square, the grid side length is 5.0 mm, the grid spacing is 800 um, and the grid groove depth is 360 um.
[0114] Example 5
[0115] The experimental steps of this embodiment are the same as those of Embodiment 1, except that in this embodiment, the grid shape of the composite grid membrane and the single-layer grid membrane in step (3) is diamond, the grid side length is 5.0 mm, the grid spacing is 1000 um, and the grid groove depth is 400 um.
[0116] Example 6
[0117] The experimental steps of this embodiment are the same as those of Embodiment 1, except that in this embodiment, the grid shape of the composite grid membrane and the single-layer grid membrane in step (3) is diamond, the grid side length is 3.0 mm, the grid spacing is 400 um, and the grid groove depth is 200 um.
[0118] Example 7
[0119] The experimental steps of this embodiment are the same as those of Embodiment 1, except that in this embodiment, the grid shape of the composite grid membrane and the single-layer grid membrane in step (3) is diamond, the grid side length is 1.0 mm, the grid spacing is 180 um, and the grid groove depth is 80 um.
[0120] Example 8
[0121] The experimental steps of this embodiment are the same as those of Embodiment 1, except that in this embodiment, the grid shape of the composite grid membrane and the single-layer grid membrane in step (3) is diamond, the grid side length is 0.3 mm, the grid spacing is 50 um, and the grid groove depth is 20 um.
[0122] Example 9
[0123] This embodiment provides a method for preparing a thermally conductive pad, comprising the following steps:
[0124] (1) Dispersed vacuum
[0125] Add vinyl silicone oil (viscosity 10480mPa.s), hydrogenated silicone oil (viscosity 230mPa.s), thermally conductive powder, catalyst, inhibitor and other additives to a mixing device for dispersion and vacuuming, and obtain a thermally conductive mixture after uniform dispersion. Among them, the mass fractions of each component are: 9.70 parts of vinyl silicone oil, 0.21 parts of hydrogenated silicone oil; 40.5 parts of 50um median particle size Al2O3 powder, 10.0 parts of 10um median particle size Al2O3 powder, 22.5 parts of 5um median particle size Al2O3 powder, 17.0 parts of 2um median particle size Al2O3 powder; 0.008 parts of platinum catalyst, 0.002 parts of inhibitor, 0.08 parts of nano carbon black, and 0.02 parts of KH570 silane coupling agent.
[0126] The dispersed vacuuming comprises the following steps:
[0127] Step 1-1: First add the non-thermal conductive powder raw material, and stir for 10 minutes at a stirring speed of 20rpm / min. Finally, add the thermal conductive powder, with the particle size from large to small, and stir while adding, at a stirring speed of 40rpm / min;
[0128] Step 1-2: After adding, stir for 20 minutes at a stirring speed of 40 rpm / min;
[0129] Step 1-3: Evacuate and stir for 120 min, with a stirring speed of 80 rpm / min and an absolute vacuum pressure of 5 Pa.
[0130] (2) Rolling and curing
[0131] The heat-conducting mixture in step (1) is uniformly extruded into a fluoroplastic release film (PET) with a thickness of 50 μm on both sides by using a calendering device, and is pulled into a tunnel oven at a pulling speed of 0.1 m / min for curing, wherein the temperatures of the eight ovens are 60° C., 100° C., 140° C., 140° C., 140° C., 100° C., and 60° C., respectively;
[0132] (3) Transfer
[0133] The thermal conductive layer cured in step (2) is transferred to a mold, and the 50um fluoroplastic release film (PET) on one side is first torn off, and a composite mesh film (PP+PET) with a thickness of 150um is covered, and then the 50um fluoroplastic release film (PET) on the other side is torn off and replaced with a 75um single-layer mesh film (PP), and finally a thermal conductive gasket product is obtained with one side contacting the composite mesh film and the other side contacting the single-layer mesh film, wherein the mesh shape of the composite mesh film and the single-layer mesh film is square, the mesh side length is 0.3mm, the mesh spacing is 50um, and the mesh groove depth is 20um.
[0134] Example 10
[0135] The experimental steps of this example are the same as those of Example 1, except that in this comparative example, in step (3), the single-sided 50 μm fluoroplastic release film (PET) is first torn off and covered with a 150 μm thick composite mesh film A. , (PP+PET), then tear off the 50um fluoroplastic release film (PET) on the other side and replace it with 100um composite mesh film B , (PP+PET), finally obtaining a composite mesh film A with one side in contact , , one side contact composite grid membrane B , Thermally conductive gasket products, including composite mesh film A , And composite mesh membrane B , The grid shape is square, the grid side length is 0.3mm, the grid spacing is 50um, and the grid groove depth is 20um.
[0136] Comparative Example 1
[0137] The experimental steps of this comparative example are the same as those of Example 1, except that in this comparative example, the fluoroplastic release films on both sides in step (3) are retained and no film transfer operation is performed.
[0138] Comparative Example 2
[0139] The experimental steps of this comparative example are the same as those of Example 1, except that in this comparative example, one side of the fluoroplastic release film in step (3) is retained, and only one side of the fluoroplastic release film is converted into a composite mesh film.
[0140] <Test Method>
[0141] Film release force: using ASTM D3330 test standard;
[0142] Evaluation method for thermal pad bonding performance: According to the above thermal pad installation process, the parts bonded to the thermal pad are replaced with two mirror glasses, which are bonded to the two sides of the thermal pad respectively, and other steps remain the same; the thermal pad and mirror glass are placed horizontally after bonding, and photographed vertically downward. The photograph is processed with CAD software, and the effective bonding area ratio of the thermal pad and the mirror glass is calculated (the product of the bonding area ratios of the two sides of the thermal pad and the mirror glass), so as to quantify the difference in bonding effect;
[0143] The temperature test method of the machine when evaluating the application of thermal pads in the 3D NAND channel hole etching process: the system is evacuated to an absolute pressure of 0.4Pa. On the Lam FLEX HXE machine, the 60M output power is adjusted to 8000-9000 watts, the 400K output power is adjusted to 19000-21000 watts, and the tunable edge sheath output power is adjusted to 1000-3000 watts. The temperature of the internal circulating coolant in the electrostatic chuck is set to 60-80℃, and the initial temperature, real-time temperature (the 10th, 20th, and 30th day of continuous operation of the machine) and stable duration on the tunable edge sheath ring are monitored by a temperature probe to reflect the application performance of the thermal pad.
[0144] Table 1 is a comparison of various data of the thermal conductive gaskets of Examples 1-10 and Comparative Examples 1-2.
[0145] Table 1
[0146]
[0147] As can be seen from Table 1, the thermally conductive gasket of Comparative Example 1-2 has a poor lamination effect, the initial operating temperature of the machine is high, and it cannot maintain normal operation for a long time. Compared with Comparative Example 1-2, the thermally conductive gasket with mesh films on both sides in Example 1-10 has a better lamination effect, the machine operating temperature is low, and it can maintain normal operation for a long time, which shows that the thermally conductive gasket with mesh films on both sides in Example 1-10 has good thermal conductivity.
[0148] Although the present invention has been described in detail above by means of general description, specific implementation methods and tests, it is obvious to those skilled in the art that some modifications or improvements may be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.
Claims
1. A thermally conductive pad, characterized in that: It includes a thermally conductive silicone gasket substrate, both sides of which are fluoroplastic release films. After film transfer, one side is covered with or in contact with a grid film A, and the other side is covered with or in contact with a grid film B; the grid film A is selected from a composite grid film, and the grid film B is selected from a composite grid film or a single-layer grid film.
2. A thermally conductive pad as claimed in claim 1, characterized in that: The thermally conductive silicone gasket matrix is mainly prepared by mixing liquid silicone resin, thermally conductive powder, catalyst, inhibitor and other additives. The liquid silicone resin preferably includes vinyl silicone oil and hydrogen-containing silicone oil.
3. A thermally conductive pad as claimed in claim 1 or 2, characterized in that: The mesh shapes of the mesh membranes A and B are preferably square or diamond.
4. A thermally conductive pad as claimed in claim 1 or 2, characterized in that: The grid side length of the grid membrane A and the grid membrane B is preferably 0.3 to 5 mm; And / or, the grid spacing of the grid membrane A and the grid membrane B is preferably 50 to 1000 um; And / or, the grid groove depth of the grid film A and the grid film B is preferably 20-400 um.
5. A thermally conductive pad as claimed in claim 1 or 2, characterized in that: The grid side length of the grid membrane A and the grid membrane B is preferably 0.3 to 3 mm; And / or, the grid spacing of the grid membrane A and the grid membrane B is preferably 50-400 um; And / or, the grid groove depth of the grid film A and the grid film B is preferably 20-200 um.
6. A method for preparing a thermally conductive gasket, characterized in that: The following steps are involved: (1) Dispersed vacuum Add liquid silicone resin, thermal conductive powder, catalyst, inhibitor and other additives into a mixing device, disperse and evacuate, and obtain a thermal conductive mixture after uniform dispersion; (2) Rolling and curing Use the calendering equipment to evenly extrude the thermal conductive mixture into the fluoroplastic release films on both sides, and then pull it into the tunnel furnace for curing; (3) Transfer The cured thermal conductive layer is transferred to a film, and one side of the fluoroplastic release film is transferred to a grid film A, and the other side of the fluoroplastic release film is transferred to a grid film B, so as to obtain a thermal conductive gasket with one side covered or in contact with the grid film A and the other side covered or in contact with the grid film B, wherein the grid film A is selected from a composite grid film, and the grid film B is selected from a composite grid film or a single-layer grid film.
7. A method for preparing a thermally conductive pad as claimed in claim 6, characterized in that: The liquid silicone resin comprises vinyl silicone oil and hydrogen-containing silicone oil, the viscosity of the vinyl silicone oil ranges from 300 to 11000 mPa.s, the viscosity of the hydrogen-containing silicone oil ranges from 50 to 500 mPa.s, and the mass ratio of the vinyl silicone oil to the hydrogen-containing silicone oil is 1:1 to 50:
1.
8. A method for preparing a thermally conductive gasket as claimed in claim 6 or 7, characterized in that: The dispersed vacuuming in step (1) comprises the following steps: Step 1-1: First add the non-thermal conductive powder raw material, stir for 5 to 10 minutes at a stirring speed of 10 to 20 rpm / min, and finally add the thermal conductive powder part, with the particle size from large to small, stirring while adding, and the stirring speed is 30 to 50 rpm / min; Step 1-2: After adding, stir for 20 to 30 minutes at a stirring speed of 40 to 80 rpm / min; Step 1-3: Vacuum and stir for 90 to 120 minutes, with a stirring speed of 60 to 100 rpm / min and an absolute vacuum pressure of 0.1 to 10 Pa.
9. An application of the thermally conductive gasket according to any one of claims 1 to 6 or the thermally conductive gasket prepared by the preparation method according to claims 7 to 8, characterized in that: The thermal conductive gasket is transferred and bonded to the edge ring, and the edge ring after bonding the thermal conductive gasket is assembled with the tunable edge sheath ring. The assembled whole is then installed on the Electrostaticchuck and finally applied to the cavity etching.
10. An application of the thermally conductive pad as claimed in claim 9, characterized in that: The transfer, lamination and assembly of the thermally conductive pad comprises the following steps: Step 1: Lofting: Peel off the thermal pad from the grid film B, align it with the glue plate through the positioning point, with the grid film A facing down, to form a complete circular ring on the glue plate; Step 2: Laminating: Place the edge ring on the laminating plate with the thermal conductive pad, and apply a certain gravity to make the edge ring and the thermal conductive pad fit together completely; Step 3: Remove the edge ring from the glue plate, flip it 180 degrees and place it horizontally, and peel off the grid film A with the thermal pad facing upward, so that the thermal pads are attached to the inner and outer rings of the edge ring. Step 4: Assemble: Place the tunable edge sheath ring vertically downward on the outer ring of the edgering with the thermal pad attached, align them through the positioning holes to form a whole, and assemble them to the Electrostatic chuck. The thermal pad on the inner ring of the edgering is attached to the Electrostatic chuck, and the thermal pad on the outer ring of the edge ring is attached to the tunable edge sheath ring.