Composite graphene fiber antibacterial surgical suture based on silver / copper double-nanometer metal particles and preparation method of composite graphene fiber antibacterial surgical suture

Through the composite material of silver/copper double nanometal particles and graphene oxide fibers, combined with chemical reduction and wet spinning technology, surgical sutures with antibacterial and wound healing functions were prepared, solving the lack of anti-infection of traditional surgical sutures. and the problem of promoting tissue repair has achieved efficient wound healing effect.

CN118987319APending Publication Date: 2024-11-22ZHEJIANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410956794.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Traditional surgical sutures lack anti-infection and pro-tissue repair functions, resulting in prolonged wound healing cycle and increased risk of infection, especially in body surface wounds that are more susceptible to external impurities and bacteria.

Method used

Using a composite material of silver/copper double nanometal particles and graphene oxide fibers, surgical sutures with antibacterial and wound healing functions were prepared through chemical reduction and wet spinning processes, combining the release mechanism of epidermal growth-promoting factors.

Benefits of technology

It has achieved high tensile strength, effective antibacterial and promotes wound healing functions, becoming an ideal alternative to traditional surgical sutures and can be used in a variety of wound scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118987319A_ABST
    Figure CN118987319A_ABST
Patent Text Reader

Abstract

The invention discloses a composite graphene fiber antibacterial surgical suture based on silver / copper double nano-metal particles and a preparation method thereof, and the specific process comprises the following steps: 1) preparing a graphene oxide (GO) / silver nitrate solution, and preparing nano-silver loaded GO by using a mild combined chemical reducing agent through reduction; 2) preparing a GO / Cu < 2 + > solution, and reducing to obtain GO loaded with nano-copper; (3) preparing a mixed spinning solution from the two materials with the single nano-composite structure, and performing wet spinning and drafting orientation to prepare a composite GO fiber with a double nano-sheet oriented arrangement structure; (4) reducing by combining programmed heating and high-temperature thermal reduction to obtain composite graphene fibers; and 5) dipping the sample in a PBS solution containing epidermal growth promoting factors to form a triple nano space adsorption structure, drying at low temperature, packaging, and sterilizing to obtain the surgical suture. The surgical suture has the functions of high strength, infection resistance, wound healing promotion and the like, and can be used for replacing a traditional suture.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation technology of surgical sutures, and in particular to a composite graphene fiber antibacterial surgical suture based on silver / copper double nanometal particles and a preparation method thereof. Background Art

[0002] Surgical sutures refer to special threads used for ligation and hemostasis, suture and tissue suture during surgical operations or trauma treatment. When used for tissue suture, it can ensure wound closure, support its healing and reduce the chance of infection. The most commonly used surgical sutures in clinical practice can be divided into catgut, chemical synthetic thread, pure natural collagen suture, etc. according to the material, which can meet the most basic suture function. However, even after suturing, the wound will still cause redness, swelling and infection, resulting in prolonged wound healing cycle and even wound ulceration; especially the wound on the surface of the body is in direct contact with the outside world, impurities or bacteria in the air are more likely to enter the wound site, which further increases the incidence of infection and worsens the wound healing condition. And other related problems will arise, such as the degradable surgical sutures degrade within the original degradation cycle, but the actual wound has not healed due to the occurrence of infection. Therefore, if a new functional surgical suture with antibacterial function and wound healing function can be developed, it will have a huge boost to the solution of such problems.

[0003] As a new type of carbon nanomaterial, graphene has unique and excellent properties in optics, electricity, mechanics, chemistry, etc., and shows broad application prospects in energy science, materials science, environmental protection, biomedicine and other fields. Graphene fiber is a new type of carbon fiber macroscopically assembled from graphene sheets along a one-dimensional direction. It has good biocompatibility and mechanical properties and can be used as an ideal matrix for surgical sutures. Silver, copper and other materials have shown certain antibacterial effects, but how to introduce metals such as silver and copper into graphene fibers to achieve organic-inorganic fusion is a major technical problem. At the same time, how to further add the function of promoting wound healing to the fiber is also a huge challenge.

[0004] Therefore, in order to solve the above technical problems, the present invention simultaneously designs two nanofillers, AgNPs / GO and CuNPs / GO, and uses them as raw materials to prepare graphene oxide composite fibers, and further reduces GO to obtain composite graphene fiber antibacterial surgical suture materials based on silver / copper dual nanometal particles. The material has high tensile strength, and the combination of silver / copper shows outstanding antibacterial effect. In addition, the release of epidermal growth-promoting factors further promotes wound healing, making it an ideal substitute for traditional surgical sutures. Summary of the invention

[0005] The purpose of the present invention is to provide a composite graphene fiber antibacterial surgical suture based on silver / copper dual nanometal particles and a preparation method thereof to address the problems that traditional surgical sutures do not have the functions of anti-infection and promoting tissue repair. The present invention is implemented by the following technical solutions:

[0006] A method for preparing a composite graphene fiber antibacterial surgical suture based on silver / copper dual nanometal particles comprises the following steps:

[0007] 1) Prepare graphene oxide (GO) / silver nitrate mixed solution and GO / Cu under light-proof conditions. 2+ The solutions are mixed, and the two mixed solutions are fully stirred and reduced for a long time using a mild chemical reducing agent to prepare GO loaded with nano-silver, namely AgNPs / GO, and GO loaded with nano-copper, namely CuNPs / GO, respectively. The two products are centrifugally cleaned and precipitated to be reconfigured into AgNPs / GO dispersion and CuNPs / GO dispersion respectively;

[0008] 2) The two dispersions having a single nanocomposite structure are mixed into a mixed spinning solution in proportion, and GO fibers based on silver / copper double nanometal particles having a double nanosheet oriented arrangement structure are prepared by wet spinning and drawing orientation process;

[0009] 3) reducing it into composite graphene fiber by combining programmed heating and high temperature thermal reduction process;

[0010] 4) The sample is immersed in a PBS solution containing epidermal growth promoting factors, and a triple nano-space adsorption structure of the epidermal growth promoting factors is formed through the immersion process. After low-temperature drying, packaging, and sterilization, a composite graphene fiber antibacterial surgical suture based on silver / copper dual nano-metal particles is obtained.

[0011] Furthermore, in step 1), during the preparation of the graphene oxide (GO) / silver nitrate mixed solution, the GO size is 10-15 microns, the concentration is 0.2-0.5wt%, and the silver nitrate concentration is 5-10wt%; the GO / Cu 2+ During the preparation of the mixed solution, the GO size was 10-15 μm, the concentration was 0.2-0.5 wt%, and the Cu 2+ Provided by one of copper chloride and copper sulfate, with a concentration of 5-10wt%;

[0012] The stirring rate is 200-400 r / min and the stirring time is 30-60 min, so as to electrostatically chelate the silver ions and GO and electrostatically chelate the copper ions and GO respectively.

[0013] Further, in step 1), during the reduction preparation process, the mild chemical reducing agent includes a medium-strength reducing agent and a low-strength reducing agent, wherein the medium-strength reducing agent is one of tartaric acid, tannin, sodium ascorbate, ammonium formate, and sodium citrate, and the low-strength reducing agent is one of glucose, maltose, and lactose, the concentration of the medium-strength reducing agent is 2-5wt%, the concentration of the low-strength reducing agent is 5-12wt%, the reduction time is 5-10h, and the stirring rate is 500-1000r / min;

[0014] During the centrifugal cleaning process, the centrifugal speed is 13000-15000 rpm, the centrifugation is performed 3-5 times, each time for 10-20 minutes, and the cleaning medium is deionized water;

[0015] The concentrations of the two dispersions after redispersion were both 0.6-1.0 wt%.

[0016] Furthermore, in step 2), the volume ratio of the AgNPs / GO to CuNPs / GO dispersions is 1:3-3:1.

[0017] Furthermore, the volume ratio of the AgNPs / GO to CuNPs / GO dispersions is 1:1.

[0018] Furthermore, the wet spinning process in step 2) is: using a micro-injection pump for injection spinning, the injection hole diameter is 70-100 microns, and the injection rate is 5-10 ml / h; the coagulation bath used is a methanol / water mixed solution of sodium hydroxide, sodium chloride, and potassium chloride;

[0019] The stretching orientation process is: using a cylindrical roller stretching device, the roller diameter is 10-20cm, and the rotation speed is 15-25r / min.

[0020] Furthermore, in step 3), the programmed temperature rise process is: a heating rate of 1-2.5°C / min, and an end point temperature of 850-900°C;

[0021] The high temperature thermal reduction is as follows: the cooling rate is 5°C / min, and the cooling end point is 30-40°C.

[0022] Furthermore, in step 4), the immersion in a PBS solution containing epidermal growth promoting factors is specifically: the epidermal growth promoting factors are one or more of epidermal growth factor, transforming growth factor α, heparin binding epidermal growth factor, growth factor-like, amphotericin and beta cell regulatory factor, the concentration is 0.25-0.50g / ml, and the immersion time is 30-60min;

[0023] The low temperature drying is: 20-25°C, nitrogen air drying;

[0024] The packaging is vacuum packaging using light-proof aluminum foil packaging material;

[0025] The sterilization is irradiation sterilization.

[0026] A composite graphene fiber antibacterial surgical suture based on silver / copper dual nanometal particles is obtained by any of the above-mentioned preparation methods.

[0027] Compared with the prior art, the present invention has the following advantages:

[0028] 1) The present invention uses GO, silver nitrate, soluble Cu 2+ Salt, medium / low strength chemical reducing agents, epidermal growth promoting factors, etc. are used as raw materials, and a composite graphene fiber antibacterial surgical suture material based on silver / copper double nanometal particles is prepared by combining chemical reduction, wet spinning, stretching orientation, programmed heating reduction, impregnation loading and other combined processes. The above raw material selection and process combination are original to the present invention.

[0029] 2) In the present invention, the negatively charged oxygen-containing functional groups on GO are respectively bonded to Cu 2+ and Ag + The electrostatic adsorption between the two is used to chelate the metal ions on the surface of the GO sheet, and then the two nanofillers AgNPs / GO and CuNPs / GO are obtained by in-situ mild chemical reduction by selecting low and medium strength reducing agents instead of high strength reducing agents, without reducing GO, to ensure the high dispersibility of the nanofillers in the aqueous solvent system and not affect the subsequent wet spinning (to prevent defects inside the fiber due to uneven dispersion, affecting the tensile strength). After the fiber is obtained by wet spinning and stretching orientation process (to ensure the regular arrangement of graphene sheets), the composite graphene fiber antibacterial surgical suture material based on silver / copper dual nanometal particles is obtained by using programmed heating and thermal reduction technology. The programmed heating makes the reduction process slow and continuous, preventing the heating rate from being too fast. After the oxygen-containing functional groups on the surface of GO become gas, tiny pores are formed inside the fiber, causing the fiber strength to decrease; and after GO is reduced to form graphene fiber surgical sutures, the dispersion ability of graphene in aqueous solvents is greatly reduced, ensuring that the subsequent sutures will not dissolve and break during use. The above series of composite processes are designed for the present invention according to the actual preparation scenario requirements, realizing the innovative application of old technologies. The above combined processes synergistically enhance efficiency and realize the efficient preparation of the required materials.

[0030] 3) The composite graphene fiber antibacterial surgical suture material based on silver / copper dual nanometal particles in the present invention has multiple composite structures: a single nanocomposite structure, a double nanosheet directional arrangement structure, and a triple nanospace adsorption structure. The single nanocomposite structure is nanosilver and nanocopper composited on the surface of GO, and because it is prepared by in-situ chemical reduction, the nanoparticles are evenly dispersed / compounded; the double nanosheet directional arrangement structure is that after the AgNPs / GO and CuNPs / GO nanofiller sheets are wet-spinned and stretched, the sheets are arranged in parallel along the fiber axis, providing the main structural source for the high strength of the fiber; the triple nanospace adsorption structure is that the epidermal growth promoting factors are adsorbed in the nanospace between the graphene sheets by the immersion adsorption method, and the subsequent sutures are released through the tissue fluid medium when in use to promote tissue repair.

[0031] 4) The composite graphene fiber antibacterial surgical suture material based on silver / copper dual nanometal particles of the present invention has high biocompatibility, high tensile strength, high-efficiency antibacterial ability and tissue repair ability, and the above functions work together to promote wound recovery and healing. Among them, the coagulation bath, stretching orientation process, programmed temperature rise thermal reduction process and other operations in the specially designed wet spinning process jointly ensure the high tensile strength of the surgical suture; the combination of AgNPs / GO and CuNPs / GO ensures efficient killing of bacteria; when the bactericide kills bacteria to control infection, it creates a suitable basic condition for tissue repair, and the epidermal growth factor further exerts its ability to promote wound healing. The above functions each perform their duties, from wound suturing to anti-infection, and further to tissue repair, and jointly complete this complex process.

[0032] 5) The composite graphene fiber antibacterial surgical suture material based on silver / copper dual nanometal particles prepared in the present invention has high strength, controllable fiber size, can be used as a single fiber or after twisting multiple fibers, and will not degrade / dissolve in the wound for a long time. Therefore, it can be used in various wound suturing scenarios and has obvious universality and versatility. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 Schematic diagram of the preparation process of composite graphene fiber antibacterial surgical sutures based on silver / copper dual nanometal particles;

[0034] Figure 2 This is a photo of composite graphene fibers based on silver / copper dual nanometal particles (Example 1);

[0035] Figure 3 The release curve of copper ions and silver ions in the composite graphene fiber antibacterial surgical suture based on silver / copper dual nanometal particles (Example 1);

[0036] Figure 4 The tensile strength results of composite graphene fiber antibacterial surgical sutures based on silver / copper dual nanometal particles (Example 1). DETAILED DESCRIPTION

[0037] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0038] Comparative Example 1:

[0039] 1) Using 0.3wt% GO solution as spinning solution, wet spinning was performed using a micro-injection pump (injection hole diameter of 70 microns, injection rate of 8 ml / h; coagulation bath was a methanol / water mixed solution of sodium hydroxide, sodium chloride, and potassium chloride), and GO fibers with a nanosheet oriented arrangement structure were obtained under the action of a stretching orientation process (stretching orientation used a cylindrical roller stretching device with a roller diameter of 15 cm and a rotation speed of 15 r / min);

[0040] 2) performing programmed heating at a heating rate of 2.5°C / min, with an end point temperature of 900°C, maintaining the temperature for 2 hours for high temperature thermal reduction, and then reducing the temperature at a cooling rate of 5°C / min, with an end point of 40°C, to reduce the temperature to graphene fibers;

[0041] 3) The sample is vacuum packed and irradiated to obtain graphene fiber surgical sutures, and the storage conditions are -20-0°C.

[0042] The tensile strength of graphene fiber is 264.2MPa; it does not dissolve after being immersed in PBS solution for 10 days; the results of 7-day CCK-8 experimental detection show that the cell survival rate is 94.5%; the wound infection model was used for experimental verification, and after 3 days, the wound had redness, swelling and exudation, and the healing effect was poor. The exudate was taken for in vitro bacterial culture, which showed that internal infection occurred.

[0043] Comparative Example 2:

[0044] 1) Using 0.3wt% GO solution as spinning solution, wet spinning was performed using a micro-injection pump (injection hole diameter of 70 microns, injection rate of 8 ml / h; coagulation bath was a methanol / water mixed solution of sodium hydroxide, sodium chloride, and potassium chloride), and GO fibers with a nanosheet oriented arrangement structure were obtained under the action of a stretching orientation process (stretching orientation used a cylindrical roller stretching device with a roller diameter of 15 cm and a rotation speed of 15 r / min);

[0045] 2) performing programmed heating at a heating rate of 2.5°C / min, with an end point temperature of 900°C, maintaining the temperature for 2 hours for high temperature thermal reduction, and then reducing the temperature at a cooling rate of 5°C / min, with an end point of 40°C, to reduce the temperature to graphene fibers;

[0046] 3) The sample was immersed in a PBS solution containing 0.25 g / ml epidermal growth factor, and an epidermal growth factor-promoting factor nano-space adsorption structure was formed through an immersion process (immersion for 30 min). After low-temperature drying (20-25° C., nitrogen air drying), vacuum packaging, and irradiation sterilization, epidermal growth factor composite graphene fiber surgical sutures were obtained, and the storage conditions were -20-0° C.

[0047] Compared with comparative example 1, epidermal growth promoting factors were introduced on the basis of GO fiber. The tensile strength of the composite fiber was 258.1MPa; it did not dissolve after being immersed in PBS solution for 10 days; the results of CCK-8 test for 7 days showed that the cell survival rate was 96.8%; the wound infection model was used for experimental verification, and after 3 days, the wound surface had redness, swelling and exudation, and the healing effect was poor. The exudate was taken for in vitro bacterial culture, indicating that there was an infection inside (which means that the infection was not suppressed, and the addition of epidermal growth promoting factors had no obvious effect on the healing of infected wounds).

[0048] Embodiment 1:

[0049] 1) Under light-proof conditions, GO with a size of 10-15 microns and silver nitrate were used to prepare a mixed solution (0.2wt% GO / 8wt% silver nitrate), and the mixture was stirred at a low speed of 200 r / min for 60 min to allow the silver ions to be completely chelated on the surface of the GO sheet by electrostatic action. A mild chemical reducing agent (2wt% sodium ascorbate / 5wt% glucose) was used for reduction for 5 h to prepare an AgNPs / GO stock solution, which was washed five times by ultrahigh-speed centrifugation at 15000 rpm, using deionized water for the washing, and the precipitate was reconfigured into a 0.6wt% AgNPs / GO dispersion;

[0050] 2) GO with a size of 10-15 microns and copper chloride were used to prepare a mixed solution (0.2wt% GO / 5wt% copper chloride), and a mild chemical reducing agent (2wt% sodium ascorbate / 5wt% glucose) was used to reduce for 5 hours to prepare a CuNPs / GO stock solution, which was then washed five times by ultracentrifugation at 15000 rpm using deionized water, and the precipitate was reconfigured into a 0.6wt% CuNPs / GO dispersion;

[0051] 3) The above two materials with a single nanocomposite structure are prepared into a mixed spinning solution in a volume ratio of 1:1, and wet spinning is performed using a micro-injection pump (the injection hole diameter is 70 microns, the injection rate is 8 ml / h; the coagulation bath is a methanol / water mixed solution of sodium hydroxide, sodium chloride, and potassium chloride), and GO fibers based on silver / copper double nanometal particles with a double nanosheet oriented arrangement structure are obtained under the action of a stretching orientation process (the stretching orientation adopts a cylindrical roller stretching device with a roller diameter of 15 cm and a rotation speed of 15 r / min);

[0052] 4) performing programmed heating at a heating rate of 2.5°C / min, with an end point temperature of 900°C, maintaining the temperature for 2h for high temperature thermal reduction, and then reducing the temperature at a cooling rate of 5°C / min, with an end point of 40°C, to reduce the composite graphene fiber;

[0053] 5) The sample was immersed in a PBS solution containing 0.25 g / ml epidermal growth factor, and a triple nano-space adsorption structure of epidermal growth factor was formed through an immersion process (immersion for 30 min). After low-temperature drying (20-25° C., nitrogen air drying), vacuum packaging using light-proof aluminum foil packaging materials, and irradiation sterilization, a composite graphene fiber antibacterial surgical suture based on silver / copper dual nanometal particles was obtained ( Figure 2 ), storage conditions are -20-0℃.

[0054] Compared with comparative example 2, AgNPs and CuNPs were introduced on the basis of GO. The tensile strength of the composite fiber was 260.6MPa. Figure 4 ; No dissolution occurred after immersion in PBS solution for 10 days; The results of CCK-8 experimental detection after 7 days showed that the cell survival rate was 88.4%; The wound infection model was used for experimental verification, and the wound began to heal after 3 days without redness, swelling or exudation.

[0055] Embodiment 2:

[0056] 1) In the dark, GO with a size of 10-15 microns and silver nitrate were used to prepare a mixed solution (0.2wt% GO / 8wt% silver nitrate), and the mixture was stirred at a low speed of 200 r / min for 60 min to allow the silver ions to be completely chelated on the surface of the GO sheet by electrostatic action. A mild chemical reducing agent (2wt% sodium ascorbate / 5wt% glucose) was used for reduction for 5 h to prepare an AgNPs / GO stock solution, which was washed 5 times by ultra-high speed centrifugation at 15000 rpm, using deionized water for the washing, and the precipitate was reconfigured into a 1.0wt% AgNPs / GO dispersion;

[0057] 2) GO with a size of 10-15 μm and copper chloride were used to prepare a mixed solution (0.2 wt% GO / 5 wt% copper chloride), and a mild chemical reducing agent (2 wt% sodium ascorbate / 5 wt% glucose) was used to reduce for 5 h to prepare a CuNPs / GO stock solution, which was then washed five times by ultracentrifugation at 15,000 rpm using deionized water, and the precipitate was reconfigured into a 1.0 wt% CuNPs / GO dispersion;

[0058] 3) The above two materials with a single nanocomposite structure are prepared into a mixed spinning solution in a volume ratio of 1:1, and wet spinning is performed using a micro-injection pump (the injection hole diameter is 70 microns, the injection rate is 8 ml / h; the coagulation bath is a methanol / water mixed solution of sodium hydroxide, sodium chloride, and potassium chloride), and GO fibers based on silver / copper double nanometal particles with a double nanosheet oriented arrangement structure are obtained under the action of a stretching orientation process (the stretching orientation adopts a cylindrical roller stretching device with a roller diameter of 15 cm and a rotation speed of 15 r / min);

[0059] 4) performing programmed heating at a heating rate of 2.5°C / min, with an end point temperature of 900°C, maintaining the temperature for 2h for high temperature thermal reduction, and then reducing the temperature at a cooling rate of 5°C / min, with an end point of 40°C, to reduce the composite graphene fiber;

[0060] 5) The sample was immersed in a PBS solution containing 0.25 g / ml epidermal growth factor, and a triple nano-space adsorption structure of epidermal growth factor was formed through an immersion process (immersion for 30 min). The sample was then dried at low temperature (20-25°C, air-dried with nitrogen), vacuum-packed using light-proof aluminum foil packaging materials, and sterilized by irradiation to obtain a composite graphene fiber antibacterial surgical suture based on silver / copper dual-nanometallic particles.

[0061] Compared with Example 1, the concentrations of AgNPs / GO and CuNPs / GO dispersions were increased. The tensile strength of the composite fiber was 286.3MPa. Due to the increase in concentration, the orderly stacking and arrangement of the internal graphene sheets became more dense, which was significantly improved compared with Example 1. No dissolution occurred after immersion in PBS solution for 10 days. The results of the 7-day CCK-8 test showed that the cell survival rate was 85.6%. At the same time, the 7-day in vitro release test showed that the release of silver ions and copper ions was compared with Example 1 ( Figure 3 ) increased by 16% and 23% respectively; the wound infection model was used for experimental verification, and the wound began to heal after 3 days without redness, swelling or exudation.

[0062] The composite graphene fiber antibacterial surgical suture based on silver / copper dual nanometal particles has high tensile strength. The combination of silver / copper shows outstanding antibacterial effect. In addition, the release of epidermal growth factors further promotes wound healing, making it an ideal substitute for traditional surgical sutures.

Claims

1. A method for preparing composite graphene fiber antibacterial surgical suture based on silver / copper dual nanometal particles, characterized in that: The following steps are involved: 1) Prepare graphene oxide (GO) / silver nitrate mixed solution and GO / Cu under light-proof conditions. 2+ The solutions are mixed, and the two mixed solutions are fully stirred and reduced for a long time using a mild chemical reducing agent to prepare GO loaded with nano-silver, namely AgNPs / GO, and GO loaded with nano-copper, namely CuNPs / GO, respectively. The two products are centrifugally cleaned and precipitated to be reconfigured into AgNPs / GO dispersion and CuNPs / GO dispersion respectively; 2) The two dispersions having a single nanocomposite structure are mixed into a mixed spinning solution in proportion, and GO fibers based on silver / copper double nanometal particles having a double nanosheet oriented arrangement structure are prepared by wet spinning and drawing orientation process; 3) reducing it into composite graphene fiber by combining programmed heating and high temperature thermal reduction process; 4) The sample is immersed in a PBS solution containing epidermal growth promoting factors, and a triple nano-space adsorption structure of the epidermal growth promoting factors is formed through the immersion process. After low-temperature drying, packaging, and sterilization, a composite graphene fiber antibacterial surgical suture based on silver / copper dual nano-metal particles is obtained.

2. The method for preparing the composite graphene fiber antibacterial surgical suture based on silver / copper dual nanometal particles according to claim 1, characterized in that: In step 1), during the preparation of the graphene oxide (GO) / silver nitrate mixed solution, the GO size is 10-15 microns, the concentration is 0.2-0.5wt%, and the silver nitrate concentration is 5-10wt%; the GO / Cu 2+ During the preparation of the mixed solution, the GO size was 10-15 μm, the concentration was 0.2-0.5 wt%, and the Cu 2+ Provided by one of copper chloride and copper sulfate, with a concentration of 5-10wt%; The stirring rate is 200-400 r / min and the stirring time is 30-60 min, so as to electrostatically chelate the silver ions and GO and electrostatically chelate the copper ions and GO respectively.

3. The method for preparing the composite graphene fiber antibacterial surgical suture based on silver / copper dual nanometal particles according to claim 1, characterized in that: In step 1), during the reduction preparation process, the mild chemical reducing agent includes a medium-strength reducing agent and a low-strength reducing agent, wherein the medium-strength reducing agent is one of tartaric acid, tannin, sodium ascorbate, ammonium formate, and sodium citrate, and the low-strength reducing agent is one of glucose, maltose, and lactose. The concentration of the medium-strength reducing agent is 2-5wt%, the concentration of the low-strength reducing agent is 5-12wt%, the reduction time is 5-10h, and the stirring rate is 500-1000r / min; During the centrifugal cleaning process, the centrifugal speed is 13000-15000 rpm, the centrifugation is performed 3-5 times, each time for 10-20 minutes, and the cleaning medium is deionized water; The concentrations of the two dispersions after redispersion were both 0.6-1.0 wt%.

4. The method for preparing the composite graphene fiber antibacterial surgical suture based on silver / copper dual nanometal particles according to claim 1, characterized in that: In step 2), the volume ratio of AgNPs / GO to CuNPs / GO dispersion is 1:3-3:

1.

5. The method for preparing the composite graphene fiber antibacterial surgical suture based on silver / copper dual nanometal particles according to claim 4, characterized in that: The volume ratio of the AgNPs / GO to CuNPs / GO dispersions is 1:

1.

6. The method for preparing the composite graphene fiber antibacterial surgical suture based on silver / copper dual nanometal particles according to claim 1, characterized in that: The wet spinning process in step 2) is: using a micro-injection pump for injection spinning, the injection hole diameter is 70-100 microns, and the injection rate is 5-10 ml / h; the coagulation bath used is a methanol / water mixed solution of sodium hydroxide, sodium chloride, and potassium chloride; The stretching orientation process is: using a cylindrical roller stretching device, the roller diameter is 10-20cm, and the rotation speed is 15-25r / min.

7. The method for preparing the composite graphene fiber antibacterial surgical suture based on silver / copper dual nanometal particles according to claim 1, characterized in that: In step 3), the programmed temperature rise process is: a heating rate of 1-2.5°C / min, and an end point temperature of 850-900°C; The high temperature thermal reduction is as follows: the cooling rate is 5°C / min, and the cooling end point is 30-40°C.

8. The method for preparing the composite graphene fiber antibacterial surgical suture based on silver / copper dual nanometal particles according to claim 1, characterized in that: In step 4), the immersion in a PBS solution containing epidermal growth promoting factors is specifically: the epidermal growth promoting factors are one or more of epidermal growth factor, transforming growth factor α, heparin binding epidermal growth factor, growth factor-like, amphotericin and beta cell regulatory factor, the concentration is 0.25-0.50g / ml, and the immersion time is 30-60min; The low temperature drying is: 20-25°C, nitrogen air drying; The packaging is vacuum packaging using light-proof aluminum foil packaging material; The sterilization is irradiation sterilization.

9. A composite graphene fiber antibacterial surgical suture based on silver / copper dual nanometal particles, characterized in that: The method is adopted as described in any one of claims 1 to 8.