Preparation method and application of graphene oxide film with pH response and non-response conversion characteristic
Through sodium alginate modification and Ca2+ replacement technology, the responsiveness and water flux of graphene oxide films under different pH environments are improved, and the problem of insufficient pH response of existing graphene oxide films is solved, thus realizing the dye molecules Efficient interception and separation.
Patent Information
- Application Number
- CN202411132895.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-22
AI Technical Summary
The existing graphene oxide films have limited pH response and the introduction of pH-sensitive materials will affect the flux of water molecules, making it difficult to achieve high sensitivity response and selective interception.
By adding sodium alginate solution to graphene oxide suspension, modified graphene oxide nanosheets were formed, and the nanosheets were assembled into a film by vacuum filtration, and combined with Ca2+ to replace Na+, the membrane was achieved with sensitive response under different pH environments and High water flux.
It realizes the high sensitivity response and high water flux of graphene oxide films under different pH environments, and can achieve precise control and separation of dye molecules in the fields of water purification and intelligent screening.
Smart Images

Figure CN118988007A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of nanofiltration membranes, and specifically relates to a preparation method and application of a graphene oxide membrane having pH response and non-response conversion characteristics. Background Art
[0002] Adaptive responsive nanochannels with intelligent management characteristics play a key role in energy conversion, drug delivery, chemical separation, water purification, etc. Drawing inspiration from the nanochannels of biological membranes, it is of great value to construct biomimetic nanochannels with adaptive responsive characteristics based on new nanomaterials.
[0003] Many membrane materials have been developed and utilized. Among these membrane materials, two-dimensional graphene oxide has become a popular candidate material for assembling thin films due to its unique physicochemical properties, high specific surface area and high mechanical strength, rich oxygen-containing functional groups, and flexible and adjustable interlayer spacing of stacked membranes. It is reported that the carboxyl groups of graphene oxide nanosheets have slight pH responsiveness. However, most of these carboxyl groups are distributed at the edges of the sheets, resulting in very limited pH response. Relevant technicians have made many attempts to optimize the pH response of graphene oxide membranes. Introducing pH-sensitive materials between graphene oxide laminates is an optimization idea. However, the introduced macromolecules also occupy the transmission space of water molecules, causing the membrane to fall into a trade-off between selectivity and flux.
[0004] Therefore, it is necessary to develop a simple and efficient method to precisely regulate the physical and chemical properties of graphene oxide two-dimensional nanochannels to achieve sensitive response of the channels and selective retention of molecules or ions. Summary of the invention
[0005] In view of the above problems existing in the prior art, the purpose of the present invention is to design and provide a preparation method and application technical solution of graphene oxide membrane with high sensitive pH intelligent responsiveness. The membrane has sensitive channel response under different pH environments while maintaining high water flux. Furthermore, using divalent Ca 2+ Replacement of Na + , which can "lock" the response. In dye separation, the channel can be turned "on" or "off" for certain specific dye molecules by adjusting the external pH, which can be used in water purification, intelligent screening and transmission and other related fields.
[0006] The method for preparing a graphene oxide film having pH response and non-response conversion characteristics is characterized by comprising the following steps:
[0007] 1) adding sodium alginate solution to graphene oxide suspension, wherein the molecular weight of sodium alginate is 4000-100000, and sodium alginate with a higher molecular weight has a higher density of carboxyl groups, but when the molecular weight is too high, it will affect the passage of water molecules; the concentration of graphene oxide suspension is 2-5 mg / mL, and when the concentration of graphene oxide is low, it will affect the film preparation efficiency, while when the concentration is high, it is not conducive to the formation of a single sheet; the mass ratio of sodium alginate: graphene oxide: water is 1-4:2:25-100, and a higher amount of sodium alginate added is beneficial to improving the pH responsiveness of the two-dimensional channel, but when the sodium alginate content is too high, it will also hinder the passage of water molecules and reduce the membrane flux; diluting with water and fully stirring to obtain a sodium alginate modified graphene oxide nanosheet mixed solution; the graphene oxide suspension in the present invention is prepared by a modified Hummers method, and its thickness is a single atomic layer and its average lateral size is 500 nm.
[0008] 2) The mixed solution is deposited onto a porous substrate membrane by vacuum filtration, and the membrane is dried at a temperature of 45-80°C for 6-36 hours. Appropriate drying time is conducive to fully removing free water in the membrane and making the nanosheets more tightly assembled, but too high drying temperature and time will reduce the nanosheets; thus, a graphene oxide membrane with pH responsive characteristics is obtained.
[0009] The method for preparing a graphene oxide film having pH response and non-response conversion characteristics is characterized in that: the film prepared in step 2) is soaked in a CaCl2 solution for 0.4-0.6h before drying to make Ca 2+ Ions fully replace Na + , the concentration of CaCl2 solution is 0.1-1.0 mol / L, and further drying is performed to obtain a graphene oxide film with pH non-responsive conversion characteristics. 2+ Can make the membrane Na + Rapid replacement, but when the concentration is too high, it affects the internal structure of the two-dimensional nanochannel.
[0010] The method for preparing a graphene oxide film having pH-responsive and non-responsive conversion characteristics is characterized in that in step 1), the molecular weight of sodium alginate is 8000-15000, preferably 10000.
[0011] The method for preparing a graphene oxide film having pH-responsive and non-responsive conversion characteristics is characterized in that in step 1), the concentration of the graphene oxide suspension is 3-4 mg / mL.
[0012] The method for preparing a graphene oxide film with pH responsive and non-responsive conversion characteristics is characterized in that in step 1), the mass ratio of sodium alginate: graphene oxide: water is 2-3:2:40-60, preferably 2:2:50.
[0013] The method for preparing a graphene oxide film with pH responsive and non-responsive conversion characteristics is characterized in that in step 1): magnetic stirring is adopted, the stirring speed is 300-1200r / min, and the stirring time is 0.5-4h; preferably the stirring speed is 600-800r / min; the stirring time is 2-3h; and appropriate stirring speed and stirring time are conducive to full contact and uniform mixing of sodium alginate and graphene oxide nanosheets.
[0014] The method for preparing a graphene oxide membrane with pH responsive and non-responsive conversion characteristics is characterized in that in step 2): the porous substrate membrane is a mixed cellulose ester, nylon, polyacrylonitrile, polycarbonate, aluminum oxide, zirconium oxide, silicon oxide or titanium oxide, and the average pore size of the porous substrate membrane is 0.05-0.45 μm, and the driving pressure is 0.1-0.5 MPa; preferably, the average pore size is 0.1-0.22 μm, and the driving pressure is 0.1-0.2 MPa. A moderate supporting substrate pore size can ensure that the water flux is not affected, while providing strong mechanical support for the separation layer. A moderate driving pressure can not only ensure high efficiency of membrane production, but also enable the nanosheets to be stacked evenly.
[0015] The method for preparing a graphene oxide film with pH responsive and non-responsive conversion characteristics is characterized in that in step 2): the drying temperature is 50-60° C.; the drying time is 10-30 hours, preferably 15-20 hours.
[0016] The method for preparing a graphene oxide film with pH response and non-response conversion characteristics is characterized in that the concentration of the CaCl2 solution is 0.25-0.8 mol / L.
[0017] The graphene oxide membrane prepared by the present invention is applied in the fields of water purification, intelligent screening and transmission.
[0018] In the technical solution of the present invention, a sodium alginate gel molecule with a carboxyl group is used to modify a graphene oxide nanosheet, and then the nanosheet is assembled into a film by vacuum filtration, and alginate molecules are introduced into a two-dimensional nanochannel. The modified two-dimensional nanochannel carries a large number of carboxyl groups, so that the sodium alginate molecular chain shows a change in configuration under different pH environments, thereby affecting the change in the structure of the two-dimensional nanochannel. In the intelligent response of different external pH values, the two-dimensional channel membrane can achieve a "switch" effect on the transfer of dye molecules while maintaining a high water flux. The present invention uses a microscopic modification of graphene oxide nanochannels to prepare a two-dimensional channel stack membrane that has the characteristic of sensitive changes in channel structure under different pH environments, and has good application prospects in the fields of water purification and intelligent screening.
[0019] The technical solution provided by the present invention has the following beneficial effects:
[0020] (1) The present invention uses green and non-toxic sodium alginate molecular chains to modify graphene oxide nanosheets, and the process flow is simple and does not produce secondary pollution.
[0021] (2) The present invention uniformly introduces carboxyl groups between the stacked two-dimensional nanochannel layers, thereby achieving the purpose of precisely regulating the physical and chemical structure of the nanochannel, and further achieving high-precision response of the two-dimensional channel under different pH conditions;
[0022] (3) The present invention further introduces Ca in situ 2+ , which can achieve the "locking" of the channel pH, thereby realizing the flexible conversion of the nanochannel between pH response and non-response. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A flow chart of the preparation scheme of the present invention;
[0024] Figure 2 This is an atomic force microscope image of the sodium alginate-modified graphene oxide nanosheets prepared in Example 1;
[0025] Figure 3 The surface and cross-sectional electron microscope scanning images of the graphene oxide film prepared in Example 1;
[0026] Figure 4 The XRD diagram of the graphene oxide film prepared in Example 1 at different pH values;
[0027] Figure 5 The water flux and rejection rate of the graphene oxide membrane prepared in Example 1 for Orange IV at different pH values;
[0028] Figure 6 (a) and (b) are the test results of interlayer spacing XRD, dye retention rate and water flux of the graphene oxide membrane prepared in Example 2 at different pH values;
[0029] Figure 7 The test results of water flux and ratio at different pH values of Comparative Example 1 and Examples 1, 3, 4, 5 and 6 are shown. DETAILED DESCRIPTION
[0030] The present invention is described clearly and completely below in conjunction with the accompanying drawings and specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Example 1
[0032] 1) 2 mL of 0.1 mg / mL sodium alginate solution was added to 2 mL of 0.1 mg / mL graphene oxide suspension, the molecular weight of sodium alginate was 10000, and the suspension was diluted to 50 mL with deionized water. The suspension was stirred for 2 h under magnetic stirring at 600 r / min to obtain sodium alginate-modified graphene oxide nanosheets, which were observed by atomic force microscopy. Figure 2 As shown;
[0033] 2) depositing the mixed solution obtained in step 1) onto a mixed cellulose ester substrate having an average pore size of 0.22 μm using a vacuum filtration method at a pressure of 0.1 MPa;
[0034] 3) The two-dimensional channel separation layer with substrate support obtained in step 2) was placed in an oven at 60°C for 12 hours to further improve the degree of cross-linking between sodium alginate and graphene oxide nanosheets, thereby obtaining a graphene oxide membrane with pH responsive properties, the surface and tomographic scanning electron microscopy of which are as follows: Figure 3 shown.
[0035] The interlayer spacing of the graphene oxide film at different pH values was tested. The interlayer spacing at pH 2 was The interlayer spacing at pH 12 is like Figure 4 The retention rate and water flux of dye molecules at pH = 2 and pH = 12 were further tested. The retention rates of methylene blue and orange IV dye molecules at pH = 2 were 98.55% and 99.67%, respectively, and the water flux was 122.67 L m -2 h -1 bar -1 At pH 12, the retention rate of methylene blue dye molecules was 99.86%, the retention rate of orange IV dye molecules was 27.55%, and the water flux was 76.76 L m -2 h -1 bar -1 , the ratio of water flux at different pH is 1.60, such as Figure 5 As shown. It can be seen that at different pH values, the retention rate and water flux of the membrane for dye molecules vary greatly. At pH 2, the two dyes can be removed simultaneously, while at pH 12, the two dyes can be separated.
[0036] Example 2
[0037] 1) adding 2 ml of 0.1 mg / ml sodium alginate solution to 2 ml of 0.1 mg / mL graphene oxide suspension, i.e., the mass ratio of sodium alginate to graphene oxide is 1:1, and diluting to 50 ml with deionized water, and stirring for 2 h under magnetic stirring at 600 r / min, to obtain sodium alginate-modified graphene oxide nanosheets;
[0038] 2) depositing the mixed solution obtained in step 1) onto a mixed cellulose ester substrate having an average pore size of 0.22 μm using a vacuum filtration method at a pressure of 0.1 MPa;
[0039] 3) The two-dimensional channel membrane with substrate support obtained in step 2) is placed in a 0.5 mol / L CaCl2 solution and fully soaked for 0.5 h. The membrane is then placed in an oven at 60°C and dried for 12 h to further enhance the binding force between calcium alginate and graphene oxide nanosheets, thereby obtaining a graphene oxide membrane with pH non-responsive conversion characteristics.
[0040] The XRD interlayer spacing of the graphene oxide film at different pH values was tested. Figure 6 As shown in (a), the interlayer spacing changes at pH = 2 and pH = 12 are almost negligible, respectively. and The dye retention rate and water flux were further tested at pH 2 and pH 12. The dye retention rate was 99.69% and the water flux was 12.21 L m at pH 2. -2 h -1 bar -1 ; At pH 12, the retention rate of dye molecules was 99.56% and the water flux was 13.22 L m -2 h -1 bar -1 It can be seen that under different pH changes, the dye retention rate and water flux of the membrane have almost no change, indicating that after adding Ca 2+ Finally, the membrane completes the transformation from pH smart response to response "locked" state.
[0041] Example 3
[0042] The preparation method provided in this embodiment is the same as that in Example 1, except that the amount of sodium alginate added is 1 mL, that is, the mass ratio of sodium alginate to graphene oxide is 0.5:1, and further diluted to 25 mL with deionized water. The water flux at pH 2 and pH 12 and the ratio of water flux at different pH values were further tested. The water flux at pH 2 was 69.24 Lm -2 h -1 bar -1 ; At pH 12, the water flux was 90.22 L m-2 h -1 bar -1 , the ratio of water flux at different pH is 1.30, such as Figure 7 shown.
[0043] Example 4
[0044] The preparation method provided in this embodiment is the same as that in Example 1, except that the amount of sodium alginate added is 1.6 mL, that is, the mass ratio of sodium alginate to graphene oxide is 0.8:1. The water flux at pH 2 and pH 12 and the ratio of water flux at different pH values were further tested. The water flux at pH 2 was 70.19 L m -2 h -1 bar -1 ; At pH 12, the water flux was 100.73 L m -2 h -1 bar -1 , the ratio of water flux at different pH is 1.44, such as Figure 7 shown.
[0045] Example 5
[0046] The preparation method provided in this embodiment is the same as that in Example 1, except that the amount of sodium alginate added is 3 mL, that is, the mass ratio of sodium alginate to graphene oxide is 1.5:1. The water flux at pH 2 and pH 12 and the ratio of water flux at different pH values were further tested. The water flux at pH 2 was 67.87 L m -2 h -1 bar -1 ; At pH 12, the water flux was 107.58 L m -2 h -1 bar -1 , the ratio of water flux at different pH is 1.58, such as Figure 7 shown.
[0047] Example 6
[0048] The preparation method provided in this embodiment is the same as that in Example 1, except that the amount of sodium alginate added is 4 mL, that is, the mass ratio of sodium alginate to graphene oxide is 2:1. The water flux at pH 2 and pH 12 and the ratio of water flux at different pH values were further tested. The water flux at pH 2 was 62.50 L m -2 h -1 bar -1 ; At pH = 12, the water flux is 79.18Lm -2 h -1 bar -1 , the ratio of water flux at different pH is 1.27, such as Figure 7 shown.
[0049] Comparative Example 1
[0050] This comparative example compares the nanofiltration performance of the original graphene oxide membrane. The preparation method is as follows:
[0051] 2mL of 0.1mg / mL graphene oxide suspension was diluted to 50mL with deionized water and ultrasonicated for 15min. The nanosheets were deposited onto a mixed cellulose ester substrate with an average pore size of 0.22μm using a vacuum filtration method. The pressure used was 0.1MPa. The two-dimensional channel separation layer with substrate support was placed in an oven at 60℃ and dried for 12h to obtain the original graphene oxide membrane.
[0052] The retention rate and water flux of dye molecules were tested at pH = 2 and pH = 12. At pH 2, the water flux was 108.72 L m -2 h -1 bar -1 ; At pH 12, the water flux was 115.44 L m -2 h -1 bar -1 , the ratio of the two is 1.06, such as Figure 7 As shown, it can be seen that the original graphene oxide film has almost no response characteristics to pH.
[0053] In the technical scheme of the present invention, the molecular weight of sodium alginate is 4000, 8000, 15000, 50000 or 100000, the concentration of graphene oxide suspension is 0.05 mg / mL, 0.15 mg / mL or 2 mg / mL, the mass ratio of sodium alginate: graphene oxide: water is 2:2:25, 2:2:75 or 2:2:100, the drying temperature of the film is 45°C, 70°C or 80°C, the drying time is 36h, 20h or 6h, the concentration of CaCl2 solution is 0.1mol / L, 0.8mol / L or 1.0mol / L, and the technical effect described in the present invention can also be achieved.
[0054] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a graphene oxide film having pH-responsive and non-responsive conversion characteristics, characterized in that The following steps are involved: 1) adding a sodium alginate solution to a graphene oxide suspension, wherein the molecular weight of the sodium alginate is 4000-100000, the concentration of the graphene oxide suspension is 0.05-0.2 mg / mL, diluting with water and fully stirring, wherein the mass ratio of sodium alginate: graphene oxide: water is 1-4:2:25-100, and obtaining a sodium alginate-modified graphene oxide nanosheet mixed solution; 2) The mixed solution is deposited onto a porous substrate membrane by vacuum filtration, and the membrane is dried at a temperature of 45-80° C. for a time of 6-36 h, thereby obtaining a graphene oxide membrane having pH responsive characteristics.
2. The method for preparing a graphene oxide film having pH responsive and non-responsive conversion characteristics according to claim 1, characterized in that: The membrane prepared in step 2) was soaked in a CaCl2 solution for 0.4-0.6h before drying to make the Ca 2+ Ions fully replace Na + , the concentration of the CaCl2 solution is 0.1-1.0 mol / L, and further drying is performed to obtain a graphene oxide film having pH non-responsive conversion characteristics.
3. The method for preparing a graphene oxide film having pH responsive and non-responsive conversion characteristics as claimed in claim 1, characterized in that In step 1), the molecular weight of sodium alginate is 8000-15000, preferably 10000.
4. The method for preparing a graphene oxide film having pH responsive and non-responsive conversion characteristics according to claim 1, characterized in that In step 1), the concentration of the graphene oxide suspension is 0.05-0.2 mg / ml.
5. The method for preparing a graphene oxide film having pH responsive and non-responsive conversion characteristics according to claim 1, characterized in that In step 1), the mass ratio of sodium alginate: graphene oxide: water is 2-3:2:40-60, preferably 2:2:
50.
6. The method for preparing a graphene oxide film having pH responsive and non-responsive conversion characteristics according to claim 1, characterized in that In step 1), magnetic stirring is used, the stirring speed is 300-1200 r / min, and the stirring time is 0.5-4 h; preferably, the stirring speed is 600-800 r / min; and the stirring time is 2-3 h.
7. The method for preparing a graphene oxide film having pH responsive and non-responsive conversion characteristics according to claim 1, characterized in that In step 2): the porous substrate membrane is a mixed cellulose ester, nylon, polyacrylonitrile, polycarbonate, aluminum oxide, zirconium oxide, silicon oxide or titanium oxide, the average pore size of the porous substrate membrane is 0.05-0.45 μm, and the driving pressure is 0.1-0.5 MPa; preferably, the average pore size is 0.1-0.22 μm, and the driving pressure is 0.1-0.2 MPa.
8. The method for preparing a graphene oxide film having pH responsive and non-responsive conversion characteristics according to claim 1, characterized in that In step 2), the drying temperature is 50-60° C. and the drying time is 10-30 h, preferably 15-20 h.
9. The method for preparing a graphene oxide film having pH responsive and non-responsive conversion characteristics according to claim 2, characterized in that: The concentration of CaCl2 solution is 0.25-0.8 mol / L.
10. Application of the graphene oxide membrane prepared as claimed in claim 1 or 2 in the fields of water purification, intelligent screening and transmission.
Citation Information
Cited By
Graphene oxide and sodium alginate composite membrane for extracting ocean osmotic energy and preparation method of graphene oxide and sodium alginate composite membrane
CN119524638A
Graphene oxide-sodium alginate composite membrane for extracting marine osmotic energy and preparation method thereof
CN119524638B
Graphene oxide composite membrane capable of stimulating response as well as preparation method and application of graphene oxide composite membrane
CN121401899A
A stimuli-responsive graphene oxide composite film, and a preparation method and application thereof
CN121401899B