Cu2-xS / carbon / MnO2 / attapulgite composite catalyst with plasmon effect and application thereof
By loading MnO2 on the concave and convex rock support and forming Cu2-xS plasmon effect on its surface, the problems of high thermal catalytic temperature and agglomeration of MnO2 catalysts are solved, and low-temperature photothermal synergistic catalytic oxidation is achieved, which improves catalytic activity and surface area .
Patent Information
- Application Number
- CN202411021264.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-29
AI Technical Summary
The existing MnO2 catalysts have high thermal catalytic temperature when catalyzing benzene, and there are agglomeration problems that lead to a reduction in catalytic activity. How to reduce the reaction temperature and increase the specific surface area and active site of the catalyst.
Concave and convex rock stones are used as the support to uniformly load sheet MnO2 and Cu2-xS with plasmon effect is loaded on its surface, which reduces the catalytic temperature through photothermal coupling.
The catalytic oxidation VOCs reaction temperature is effectively reduced, the specific surface area and active site of the catalyst are increased, photothermal synergistic catalytic oxidation under low temperature conditions is achieved, and catalytic activity is improved.
Smart Images

Figure HDA0004967333860000011 
Figure HDA0004967333860000012 
Figure HDA0004967333860000021
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of catalyst preparation, and specifically relates to a Cu catalyst having plasmon effect. 2-x Preparation method and application of S / carbon / MnO2 / attapulgite composite catalyst. Background Art
[0002] Volatile organic compounds (VOCs), as one of the main air pollutants, are the main cause of secondary organic aerosols, atmospheric photochemical smog and ozone destruction. Aromatic VOCs include benzene, toluene, o-xylene and chlorobenzene, which are highly toxic and "carcinogenic-mutagenic-teratogenic" to human health. Catalytic oxidation is widely used due to its high treatment efficiency, no secondary pollution and relatively low ignition temperature. Catalysts are the core of catalytic oxidation technology, among which non-precious metals have the advantages of abundant resources and low prices, which have attracted widespread attention. MnO2, as a typical non-precious metal catalyst, has the advantages of relatively low-temperature catalytic activity, wide raw material sources and simple preparation process, and is used in the field of catalytic treatment of VOCs. Flake MnO2 has the advantages of large specific surface area and a large number of active sites, and has become a research hotspot. Chinese patent (CN115744995A) discloses a continuous flow microwave method for preparing flake manganese dioxide, wherein a divalent manganese salt, a heptavalent manganese salt, an alkali and water are mixed to obtain a mixed solution; the mixed solution is then injected into a microwave chemical reactor for continuous flow microwave reaction, and the mixture is filtered and dried after exiting the microwave chemical reactor to obtain the flake manganese dioxide. The flake manganese dioxide prepared by this method has serious stacking and agglomeration problems, which leads to a significant reduction in the catalytic oxidation performance of the manganese-based catalyst. How to solve the agglomeration of manganese dioxide is a key technical problem to be solved.
[0003] At present, the thermal catalytic temperature required for Mn-based catalysts to catalyze benzene derivatives (such as benzene, toluene, xylene, etc.) is still greater than 300°C. In order to further reduce the catalytic reaction temperature, the use of light-driven catalysts coupled with thermal catalysts for photothermal synergistic catalytic oxidation of VOCs is a catalytic oxidation technology with the advantages of mild reaction conditions, low energy consumption and environmental friendliness. Nanomaterials with localized surface plasmon resonance effect will produce hot electrons with higher energy (much higher than the electron energy in thermodynamic equilibrium) under light conditions. In recent years, compared with precious metal catalysts such as platinum and gold, non-precious metal nanocatalysts have become a research hotspot due to their low prices. In particular, non-stoichiometric Cu 2-x S is widely used in the field of photothermal catalysis due to its simple preparation process, strong localized surface plasmon resonance (LSPR) effect and excellent visible-near-infrared light absorption ability. Summary of the invention
[0004] In view of the two problems raised in the background technology, the present invention provides a Cu 2-x The invention discloses a method for preparing a S / carbon / MnO2 / attapulgite composite catalyst. The purpose is: on the one hand, using attapulgite as a carrier, uniformly loading flaky manganese dioxide on the attapulgite carrier to prepare a MnO2 / attapulgite catalyst, so as to overcome the problems of easy agglomeration and stacking of the flaky MnO2 catalyst, thereby increasing the specific surface area and active sites of the MnO2 catalyst; on the other hand, loading Cu with plasmon effect on the surface of the flaky MnO2 2-x S can form a strong photothermal effect to further reduce the reaction temperature of the thermal catalyst MnO2 during the catalytic oxidation of VOCs, solving the problem of the excessively high active temperature of the Mn-based thermal catalyst.
[0005] The Cu 2-x The preparation method of S / carbon / MnO2 / attapulgite catalyst comprises the following specific steps:
[0006] 1. While stirring, disperse thiophene and attapulgite in acetone solvent, stir evenly, continue to add potassium permanganate to the solution, and at the same time, continuously introduce ozone (O3) gas at a flow rate of 3 to 6 mL / min into the system through a flow meter (MCR-500SLPMM, Alicat, USA). After ultrasonic reaction for 1 h to 3 h, stop ventilation, filter, and wash with deionized water to obtain a polythiophene / MnO2 / attapulgite composite filter cake;
[0007] In step 1, the mass ratio of thiophene to acetone is 0.02-0.05:1, and the molar ratio of thiophene to potassium permanganate is 0.8-1.2:1; wherein the mass ratio of manganese dioxide (theoretical value) to attapulgite is 0.5-1.2:1;
[0008] 2. The polythiophene / MnO2 / attapulgite composite filter cake obtained in step 1 is redispersed in deionized water to prepare a dispersion slurry with a mass percentage concentration of 10% to 13%, and a soluble copper salt is added; the obtained dispersion is subjected to an adsorption reaction at room temperature for 2 to 4 hours, filtered, washed, dried, and crushed; and the obtained powder is pyrolyzed at a temperature of 300°C to 450°C for 1 to 3 hours under a nitrogen atmosphere to obtain Cu 2-x S / carbon / MnO2 / attapulgite composite catalyst.
[0009] The soluble copper salt in step 2 is one of copper sulfate pentahydrate (CuSO4·5H2O), copper chloride dihydrate (CuCl2·2H2O) or copper nitrate trihydrate (Cu(NO3)2·3H2O). The molar ratio of the soluble copper salt to the thiophene in step 1 is 1.1-1.3:1.
[0010] The prepared Cu 2-xUnder light conditions, the S / carbon / MnO2 / attapulgite composite catalyst promotes the plasmon effect on the catalyst surface and catalytically oxidizes VOCs under the synergistic effect of photothermal coupling.
[0011] Beneficial effects of the present invention:
[0012] 1. The present invention uses thiophene to react with potassium permanganate, which has the following advantages: ① thiophene is reductive, and the reaction with potassium permanganate, which has strong oxidative properties, promotes the formation of MnO2, and thiophene is oxidized into a polymer; ② the sulfur atoms (S) contained in the polythiophene molecular chain can react with copper ions (Cu 2+ ) undergoes complexation and coordination, adsorbing copper ions in situ onto the surface of the polythiophene / MnO2 / attapulgite composite. Then, under high temperature and inert atmosphere conditions, the polythiophene adsorbing copper ions undergoes pyrolysis to generate activated carbon materials with high adsorption capacity, which can quickly enrich VOCs gas onto the catalyst surface and also generate H2S gas, which quickly reacts with Cu 2+ The reaction generates Cu with plasmon effect 2-x S, under illumination conditions, the generated hot electrons are converted into local heat, improving the photothermal efficiency.
[0013] 2. The present invention makes full use of the "skeleton" effect of the one-dimensional nanostructure of fibrous or rod-shaped attapulgite clay, so that the lamellar MnO2 can be stably and orderly loaded in situ on its surface, effectively preventing the stacking and agglomeration of lamellar MnO2, and increasing the specific surface area and the number of active sites of the MnO2 thermal catalyst.
[0014] 3. The present invention will have plasmon effect Cu 2-x S was further loaded on the surface of flake MnO2 to prepare the bifunctional Cu 2-x S / MnO2 / attapulgite composite catalyst, which has the dual functions of thermal catalysis and plasmon photothermal effect, greatly reduces the reaction temperature when the catalyst catalyzes the oxidation of VOCs, and achieves the purpose of photothermal coupling synergistic catalytic oxidation of VOCs under low temperature conditions.
[0015] 4. The introduced ozone gas and potassium permanganate play a synergistic oxidation function, which can oxidize thiophene monomers into polythiophenes. In addition, the introduced ozone gas has a bubbling effect, which can more effectively disperse the solid particles in the system and prevent them from settling, which is conducive to more uniform loading of the active components on the surface of the attapulgite carrier. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 The XRD patterns of Example 4 and Comparative Examples 1-2 are shown;
[0017] Figure 2 TEM photo of Example 4;
[0018] Figure 3 It is the ultraviolet-visible absorption spectrum (UV-Vis) of Example 4 and Comparative Examples 1-2. DETAILED DESCRIPTION
[0019] The present invention will be further described in detail below in conjunction with specific embodiments, but the embodiments of the present invention are not limited thereto. For process parameters not particularly noted, conventional techniques may be used.
[0020] Example 1
[0021] 1. While stirring, disperse 1.24 g of thiophene and 2.0 g of attapulgite in 41.0 g of acetone solvent. After stirring evenly, continue to add 2.9 g of potassium permanganate to the solution, and at the same time, continuously introduce ozone (O3) gas at a flow rate of 3 mL / min into the system through a flow meter (MCR-500SLPMM, Alicat, USA). After ultrasonic reaction for 1 hour, stop ventilation, filter, and wash with deionized water to obtain a polythiophene / MnO2 / attapulgite composite filter cake;
[0022] 2. The polythiophene / MnO2 / attapulgite composite filter cake obtained in step 1 was re-deionized in water to prepare a dispersion slurry with a mass percentage concentration of 10%, and 4.72 g of copper sulfate pentahydrate was added. The obtained dispersion was immersed in adsorption reaction at room temperature for 2 hours, filtered, washed, dried, and crushed. Under a nitrogen atmosphere, the obtained powder was pyrolyzed at 450°C for 3 hours to obtain Cu 2-x S / carbon / MnO2 / attapulgite composite catalyst.
[0023] Example 2
[0024] 1. While stirring, disperse 2.78 g of thiophene and 2.0 g of attapulgite in 55.0 g of acetone solvent. After stirring evenly, continue to add 4.3 g of potassium permanganate to the solution, and at the same time, continuously introduce ozone (O3) gas at a flow rate of 4 mL / min into the system through a flow meter (MCR-500SLPMM, Alicat, USA). After ultrasonic reaction for 2 hours, stop ventilation, filter, and wash with deionized water to obtain a polythiophene / MnO2 / attapulgite composite filter cake;
[0025] 2. The polythiophene / MnO2 / attapulgite composite filter cake obtained in step 1 was re-deionized in water to prepare a dispersion slurry with a mass percentage concentration of 13%, and 5.78 g of cupric chloride dihydrate was added. The obtained dispersion was immersed in adsorption reaction at room temperature for 4 hours, filtered, washed, dried, and crushed. Under a nitrogen atmosphere, the obtained powder was pyrolyzed at 300°C for 1 hour to obtain a Cu 2-x S / carbon / MnO2 / attapulgite composite catalyst.
[0026] Example 3
[0027] 1. While stirring, disperse 1.96 g of thiophene and 2.0 g of attapulgite in 48.0 g of acetone solvent. After stirring evenly, continue to add 3.62 g of potassium permanganate to the solution, and at the same time, continuously introduce ozone (O3) gas at a flow rate of 6 mL / min into the system through a flow meter (MCR-500SLPMM, Alicat, USA). After ultrasonic reaction for 3 hours, stop ventilation, filter, and wash with deionized water to obtain a polythiophene / MnO2 / attapulgite composite filter cake;
[0028] 2. The polythiophene / MnO2 / attapulgite composite filter cake obtained in step 1 was re-deionized in water to prepare a dispersion slurry with a mass percentage concentration of 11%, and 6.4 g of copper nitrate trihydrate was added. The obtained dispersion was immersed in adsorption reaction at room temperature for 3 hours, filtered, washed, dried, and crushed. Under a nitrogen atmosphere, the obtained powder was pyrolyzed at 400°C for 2 hours to obtain a Cu 2-x S / carbon / MnO2 / attapulgite composite catalyst.
[0029] Example 4
[0030] 1. While stirring, disperse 1.7 g of thiophene and 2.0 g of attapulgite in 42.3 g of acetone solvent. After stirring evenly, continue to add 3.2 g of potassium permanganate to the solution, and at the same time, continuously introduce ozone (O3) gas at a flow rate of 5 mL / min into the system through a flow meter (MCR-500SLPMM, Alicat, USA). After ultrasonic reaction for 2 hours, stop ventilation, filter, and wash with deionized water to obtain a polythiophene / MnO2 / attapulgite composite filter cake;
[0031] 2. The polythiophene / MnO2 / attapulgite composite filter cake obtained in step 1 was re-deionized in water to prepare a dispersion slurry with a mass percentage concentration of 11%, and 6.1 g of copper sulfate pentahydrate was added. The obtained dispersion was immersed in adsorption reaction at room temperature for 3 hours, filtered, washed, dried, and crushed. Under a nitrogen atmosphere, the obtained powder was pyrolyzed at 400°C for 3 hours to obtain a Cu 2-x S / carbon / MnO2 / attapulgite composite catalyst.
[0032] Figure 1 The XRD diagram of Example 4; Example 4 is obtained by comparing MnO2 and Cu 2-x The PDF card of S shows that the diffraction peaks unique to MnO2 appear at 2θ of 28.3° and 37.3° (JCPDS PDF#24-0735). The peaks of Cu appear at 2θ of 27.7°, 31.9°, 45.2°, and 54.8°. 1.8The XRD results show that the carbon is in an amorphous state. ...
[0033] Figure 2 This is the TEM photo of Example 4. It can be seen that in the catalyst prepared in Example 4, the generated Cu 2-x S nanoparticles are uniformly loaded on the surface of flaky MnO2, and carbon is free on the catalyst surface.
[0034] Comparative Example 1
[0035] In Comparative Example 1, the Cu in the sample prepared in Example 4 2-x The S component is deleted, and other processes remain unchanged. The specific steps are as follows:
[0036] 1. While stirring, disperse 1.7 g of thiophene and 2.0 g of attapulgite in 42.3 g of acetone solvent. After stirring evenly, continue to add 3.2 g of potassium permanganate to the solution, and at the same time, continuously introduce ozone (O3) gas at a flow rate of 5 mL / min into the system through a flow meter (MCR-500SLPMM, Alicat, USA). After ultrasonic reaction for 2 hours, stop ventilation, filter, wash with deionized water, dry and crush to obtain a polythiophene / MnO2 / attapulgite composite catalyst;
[0037] 2. The polythiophene / MnO2 / attapulgite composite catalyst obtained in step 1 is introduced into a nitrogen atmosphere, and the obtained powder is pyrolyzed at 400°C for 3 hours to obtain a carbon / MnO2 / attapulgite composite catalyst.
[0038] Comparative Example 2
[0039] In Comparative Example 2, the MnO2 component in the sample prepared in Example 4 was deleted, and other processes remained unchanged. The specific steps are as follows:
[0040] 1. While stirring, disperse 1.7 g of thiophene and 2.0 g of attapulgite in 42.3 g of acetone solvent, stir evenly, then add 9.8 g of anhydrous ferric chloride to the solution, and after ultrasonic reaction for 2 hours, stop ventilation, filter, and wash with deionized water to obtain a polythiophene / attapulgite composite filter cake;
[0041] 2. The polythiophene / attapulgite composite filter cake obtained in step 1 was re-dissolved in deionized water to prepare a dispersion slurry with a mass percentage concentration of 11%, and 6.1 g of copper sulfate pentahydrate was added. The obtained dispersion was immersed in adsorption reaction at room temperature for 3 hours, filtered, washed, dried, and crushed. Under a nitrogen atmosphere, the obtained powder was pyrolyzed at 400° C. for 3 hours to obtain a Cu 2-x S / carbon / attapulgite composite catalyst.
[0042] Comparative Example 3
[0043] In Comparative Example 3, the carbon component in the sample prepared in Example 4 was deleted, and other processes remained unchanged. The specific steps are as follows:
[0044] 1. While stirring, disperse 2.0 g of attapulgite in 42.3 g of acetone solvent. After stirring evenly, continue to add 3.2 g of potassium permanganate to the solution. At the same time, continuously introduce ozone (O3) gas at a flow rate of 5 mL / min into the system through a flow meter (MCR-500SLPMM, Alicat, USA). After ultrasonic reaction for 2 hours, stop ventilation, filter, and wash with deionized water to obtain a MnO2 / attapulgite composite filter cake;
[0045] 2. The MnO2 / attapulgite composite filter cake obtained in step 1 is re-dissolved in deionized water to prepare a dispersion slurry with a mass percentage concentration of 11%. 6.1 g of copper sulfate pentahydrate and 3.1 g of sodium thiosulfate are added to the dispersion. After ultrasonic reaction for 30 minutes, the obtained dispersion is hydrothermally reacted at a temperature of 180°C for 3 hours, cooled to room temperature, stirred evenly, filtered, washed, dried, and crushed. Under a nitrogen atmosphere, the obtained powder is pyrolyzed at a temperature of 400°C for 3 hours to obtain a Cu 2-x S / MnO2 / attapulgite composite catalyst.
[0046] Comparative Example 4
[0047] In Comparative Example 4, the Cu 2-x The S component is replaced by the Cu component, and the other processes remain unchanged. The specific steps are as follows:
[0048] 1. While stirring, disperse 2.0 g of attapulgite in 42.3 g of acetone solvent. After stirring evenly, continue to add 3.2 g of potassium permanganate to the solution. At the same time, continuously introduce ozone (O3) gas at a flow rate of 5 mL / min into the system through a flow meter (MCR-500SLPMM, Alicat, USA). After ultrasonic reaction for 2 hours, stop ventilation, filter, and wash with deionized water to obtain a MnO2 / attapulgite composite filter cake;
[0049] 2. The MnO2 / attapulgite composite filter cake obtained in step 1 is re-additized with deionized water to prepare a dispersion slurry with a mass percentage concentration of 11%. 6.1 g of copper sulfate pentahydrate and 2.0 g of glucose (converted to the same amount of carbon in thiophene) are added to the dispersion. After ultrasonic reaction for 30 minutes, the obtained dispersion is hydrothermally reacted at 180°C for 3 hours, cooled to room temperature, stirred evenly, filtered, washed, dried and crushed. Under a nitrogen atmosphere, the obtained powder is pyrolyzed at 400°C for 3 hours to obtain a Cu / carbon / MnO2 / attapulgite composite catalyst.
[0050] Performance Evaluation
[0051] Catalytic oxidation activity evaluation: The catalyst in the present invention was subjected to catalytic oxidation experiments using toluene as a simulated gas. The activity evaluation of the catalyst was carried out on a photo-thermal synergistic catalytic reaction VOC adsorption and desorption device (VDRT-3000, Quzhou Ward Instrument Co., Ltd.), and the light source used in the reaction was a PLS SXE300 full-spectrum xenon lamp light source from Beijing Perfect Light Technology Co., Ltd., and the reaction light rate density was 300mW / m 2 . 0.1g of catalyst was placed in a quartz tube (inner diameter 28mm), toluene was produced by bubbling nitrogen at room temperature, high-purity air was used as carrier gas, and the toluene concentration was controlled by adjusting the flow rates of bubbling gas and carrier gas, i.e., toluene concentration was 400ppm, catalyst dosage was 200mg, reaction gas flow rate was 167mL / min, mass space velocity was 50000mL / g·h, and nitrogen was used as balance gas; the toluene concentration was analyzed online by GC-2014 gas chromatograph (Shimadzu Instrument, Japan). As can be seen from the test results in Table 1, the Cu prepared by the present invention 2-x The S / carbon / MnO2 / attapulgite composite catalyst exhibits good photothermal catalytic activity, and the conversion rate of toluene can reach 93%.
[0052] Table 2 Specific surface area of the prepared sample catalyst and the maximum limit temperature reached by the sample catalyst under xenon lamp irradiation. Under xenon lamp irradiation, the pressed catalyst was placed in the center of the aperture, and the surface temperature of the catalyst was measured by a handheld infrared camera. The highest temperature it could reach was recorded (DS-2TPH10-3AUF, Hangzhou Hikvision Digital Technology Co., Ltd.). As can be seen from the table, Cu 2-x The S / carbon / MnO2 / attapulgite catalyst has a higher specific surface area and temperature rise, indicating that the Cu prepared by the present invention 2-x The S / carbon / MnO2 / attapulgite composite catalyst has excellent photothermal conversion efficiency.
[0053] Figure 3 The UV-Vis absorption spectra (UV-Vis) of Example 4 and Comparative Examples 1-2 are shown in Table 1. Compared with MnO2 / attapulgite, the Cu prepared in Example 42-x The S / carbon / MnO2 / attapulgite composite catalyst has an additional significant absorption peak at 870nm, indicating that the catalyst has a plasmon resonance effect, which can form a photothermal effect and reduce the catalytic oxidation reaction temperature of the catalyst; on the other hand, Cu 2-x The visible light absorption band of the S / carbon / MnO2 / attapulgite composite catalyst is significantly improved in the near-infrared light absorption range, broadening the absorption range of the catalyst.
[0054] Table 1
[0055] sample Conversion time / min Toluene conversion Example 1 40 88% Example 2 40 83% Example 3 40 90% Example 4 40 93% Comparative Example 1 40 50% Comparative Example 2 40 32% Comparative Example 3 40 52% Comparative Example 4 40 60%
[0056] Table 2
[0057] sample <![CDATA[Specific surface area (m 2 / g)]]> Maximum temperature(℃) Example 4 198 228 Comparative Example 1 163 198 Comparative Example 2 97 178
Claims
1. A Cu with plasmon effect 2-x The preparation method of S / carbon / MnO2 / attapulgite composite catalyst is characterized by: (1) dispersing thiophene and attapulgite in a solvent, stirring the solution, adding potassium permanganate, introducing ozone, stopping the aeration after ultrasonic treatment, filtering, washing, and obtaining a polythiophene / MnO2 / attapulgite composite filter cake; (2) dispersing the polythiophene / MnO2 / attapulgite composite filter cake obtained in step (1) in water to prepare a dispersion slurry, adding a soluble copper salt, adsorbing, filtering, washing, drying, and crushing, and pyrolyzing at 300 to 450° C. in a nitrogen atmosphere to obtain Cu 2-x S / carbon / MnO2 / attapulgite composite catalyst.
2. The Cu with plasmon effect according to claim 1 2-x The preparation method of S / carbon / MnO2 / attapulgite composite catalyst is characterized by: The mass ratio of thiophene to the solvent is 0.02-0.05:1, and the molar ratio of thiophene to potassium permanganate is 0.8-1.2:
1.
3. The Cu with plasmon effect according to claim 1 2-x The preparation method of S / carbon / MnO2 / attapulgite composite catalyst is characterized by: The ratio of the theoretical value of manganese dioxide to the mass of attapulgite is 0.5 to 1.2:
1.
4. The Cu with plasmon effect according to claim 1 2-x The preparation method of S / carbon / MnO2 / attapulgite composite catalyst is characterized by: The molar ratio of the soluble copper salt to thiophene is 1.1-1.3:
1.
5. The Cu with plasmon effect according to claim 1 2-x The preparation method of S / carbon / MnO2 / attapulgite composite catalyst is characterized by: The soluble copper salt is one of copper sulfate, copper chloride and copper nitrate.
6. The Cu with plasmon effect according to claim 1 2-x The preparation method of S / carbon / MnO2 / attapulgite composite catalyst is characterized by: The pyrolysis reaction time is 1 to 3 hours.
7. A Cu with plasmon effect prepared by the method according to any one of claims 1 to 6 2-x S / Carbon / MnO2 / attapulgite composite catalyst.
8. A Cu with plasmon effect prepared by the method according to any one of claims 1 to 6 2-x S / Carbon The application of / MnO2 / attapulgite composite catalyst is characterized by: Cu 2-x The S / carbon / MnO2 / attapulgite composite catalyst was used for catalytic oxidation of VOCs.
9. The use according to claim 8, characterized in that: Catalytic oxidation of VOCs under light.
Citation Information
Patent Citations
Carbon-based non-metallic oxygen reduction catalyst as well as preparation method and application thereof
CN104014367A
Catalyst for removing VOCs through photocatalysis in cooperation with thermal catalytic oxidation and preparation method and application of catalyst
CN105413705A
Preparation method and application of attapulgite composite material with plasmon resonance effect
CN109999791A